Production method of iron-nickel-based alloy bar

Through the continuous casting and rolling process of square billets, the problems of low yield and high cost in iron-nickel-based alloy rod production are solved, and the production of low sulfur, low oxygen and high purity is achieved, which significantly improves the yield rate. and product quality.

CN119020673APending Publication Date: 2024-11-26SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146578.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing iron-nickel-based alloy rod production process is long, the material yield is low, the cost is high, and the sulfur content, oxygen content and inclusions in the steel are high, resulting in large fluctuations in performance.

Method used

Using billet continuous casting and rolling technology, the sulfur, oxygen content and inclusion levels are controlled through medium-frequency furnace or electric furnace smelting, AOD refining, LF bottom blown argon gas supply and high-temperature rolling, so as to achieve low sulfur, low oxygen and high Production of iron-nickel-based alloy rods with pureness.

Benefits of technology

It significantly shortens the production cycle, improves the yield rate, reduces production costs, and improves product quality and purity, and increases the yield rate by more than 15% compared with traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a method for producing an iron-nickel-based alloy bar, in particular to a technology for producing the bar through square billet continuous casting and rolling, which is used for reducing the production cost, improving the yield of the whole process and shortening the production period. The bar is produced in a mode of '30-ton intermediate frequency furnace (or 90-ton electric furnace) + 45-ton AOD + 45-ton LF + square billet continuous casting + rolling '. In order to ensure the high quality of the bar, a smelting method of an iron-nickel-based alloy with low sulfur (S is less than or equal to 0.0010%), low oxygen ([O] is less than or equal to 0.0010%) and high purity (four types of inclusions A, B, C and D are all less than 0.5 grade) is needed, and the specification of a continuous casting square billet is 180-220 mm. A high-rolling-force rolling mill is adopted for bar rolling, the blank heating temperature, the heating deformation rate and the finish rolling temperature are controlled, the high-quality phi 50-110 mm iron-nickel-based alloy bar is produced, and compared with a traditional technology of vacuum induction, electroslag and forging, the yield is increased by 15% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing an iron-nickel based alloy bar, and specifically refers to a technology for producing the bar by continuous casting and rolling square billets, thereby reducing production costs, improving the yield rate of the entire process, and shortening the production cycle. Background Art

[0002] Iron-nickel-based alloys are widely used in petrochemicals, key equipment and other fields due to their excellent mechanical properties and corrosion resistance. For bar production, the current common production process is: vacuum induction furnace + electroslag remelting + forging bars. Its production process is long, the yield rate is low, and the manufacturing cost is high; and there is no refining and slag making outside the furnace, and the sulfur content, oxygen content and inclusions in the steel are high, resulting in large fluctuations in its performance. The yield rate of the whole process is only 70%.

[0003] In response to the above situation, this patent proposes the "continuous casting square billet + rolling" process to produce rods, and produces iron-nickel based alloy rods with low sulfur (S≤0.001%), low oxygen ([O]≤0.001%), and high purity (four types of inclusions A, B, C, and D are all less than level 0.5). The overall quality is not lower than the traditional manufacturing process of "vacuum induction + electroslag + forging", which can greatly shorten the production cycle and increase the yield rate by more than 15% compared with the traditional process, significantly improving competitiveness.

[0004] The present invention specifically refers to the production of bar technology through "bill continuous casting + rolling" to replace the traditional process of "vacuum induction furnace + electroslag remelting + forging bar", so as to reduce production costs, improve the yield rate of the whole process, shorten the production cycle and improve product quality. Summary of the invention

[0005] The purpose of the present invention is to provide a method for producing an iron-nickel based alloy rod in view of the above problems.

[0006] The object of the present invention is achieved in this way: a method for producing an iron-nickel based alloy rod, comprising the following steps: step 1: smelting: using a medium frequency furnace or an electric furnace for smelting, the chemical composition mass percentage after smelting is: C: 1.5-2.5%, Si: 0-0.2%, Mn: 0-0.2%, P: 0-0.025%, S: 0-0.15%, Cr: 19.0-25%, Ni: 28.0%-36%, and the rest is iron and unavoidable impurities; step 2: refining: AOD is reduced by pure aluminum, and the reduction time is 13-18m in, LF bottom blowing argon gas supply intensity is controlled at 2-5L / min / t, stirring time is controlled at 10-15min, to ensure that the sulfur content in the steel is ≤0.0010%, the oxygen content in the steel is ≤0.0010%, and the four types of inclusions A, B, C, and D are all less than 0.5 level; Step three: billet continuous casting: continuous casting adopts protective slag with a melting point of 1020-1080℃ and a basicity CaO / SiO2 of 0.80-0.90, and the superheat of the molten steel in the tundish is controlled to be 40-70℃ higher than the liquidus temperature; Step four: Rolling: The rolling mill is used for bar rolling.

[0007] The specific requirements for bar rolling in step 4 are: the billet heating temperature is controlled at 1240-1280℃, the holding time is 2-3h, the deformation amount in the first three passes is controlled at ≤8%, the strain rate is ≤10s-1, and the billet surface temperature after the first three passes is ensured to be 1120-1200℃, and the final rolling temperature is 950-1000℃.

[0008] The beneficial effects of the present invention are: the production efficiency of the bars produced by "bill continuous casting + rolling" is high, and the yield rate is 15% higher than that of the traditional process. The surface of the bars has no defects such as folding, cracks, etc., the composition is uniform and consistent, and the overall quality of the bars is not lower than that of the traditional process. DETAILED DESCRIPTION

[0009] The technical solution of the present invention is as follows: The test alloy used in the present invention is N08810, and the standard composition control range is as shown in the following table.

[0010]

[0011] The rod production technology of the present invention is specifically as follows: 1. Process flow: The present invention adopts "medium frequency furnace (or electric furnace) + AOD + LF + billet continuous casting + rolling" to produce rods.

[0012] That is, the raw alloy is melted in a 30-ton medium frequency furnace (or a 90-ton electric furnace), smelted in a 45-ton AOD furnace, refined in a 45-ton LF furnace, continuously cast in billets, and rolled in a rolling mill to produce low-sulfur, low-oxygen, high-purity iron-nickel-based alloy N08810 bars. The smelting time is 90-150 minutes.

[0013] 2. Refining technology: AOD uses pure aluminum reduction, the reduction time is 13-18 minutes, the LF bottom blowing argon gas supply intensity is controlled at 2-5L / min / t, and the stirring time is controlled at 10-15 minutes. To ensure that the sulfur content in the steel is ≤0.0010%, the oxygen content in the steel is ≤0.0010%, and the four types of inclusions A, B, C, and D are all less than 0.5 level.

[0014] 3. Billet continuous casting technology: The continuous casting uses protective slag with a melting point of 1050℃ and a basicity (CaO / SiO2) of 0.85. The superheat of the molten steel in the tundish is 40-70℃ higher than the liquidus temperature. The specifications of the continuous casting billet are 180-220mm square.

[0015] Since the surface of the continuous casting billet has no defects, no surface grinding is required.

[0016] 4. Rolling technology: Use high-speed rolling mill with high rolling force for bar rolling. The billet heating temperature is controlled at 1240-1280℃, and the holding time is 2-3h. Since the continuous casting square billet is a cast structure, the billet mill follows the principle of low speed and small deformation during rolling. The deformation of the first three passes is controlled at ≤8%, the strain rate is ≤10s-1, and the billet surface temperature after the first three passes is guaranteed to be ≥1120℃, and the final rolling temperature is ≥950℃. Then, normal rolling is carried out according to the hole matching, and the bar specifications after billet opening are controlled between φ50-110mm.

[0017] The bars produced by this process have high steel purity, including: S≤0.0010%, ([O]≤0.0010%), high purity (A, B, C, D four types of inclusions are all less than 0.5 level), and the yield rate is 15% higher than that of traditional processes.

[0018] The specific embodiments are as follows.

[0019]

[0020] Embodiment 1 AOD uses pure aluminum reduction, and the reduction time is 14 minutes. The LF bottom blowing argon gas supply intensity is controlled at 3.5L / min / t, and the stirring time is controlled at 12 minutes. The sulfur content in the steel is 0.0009%, the oxygen content in the steel is 0.0008%, and the four types of inclusions A, B, C, and D are 0, 0, 0.5, and 0.5, respectively.

[0021] The continuous casting uses protective slag X-1 with a melting point of 1050℃ and a basicity (CaO / SiO2) of 0.85. The superheat of the molten steel in the tundish is 55℃ higher than the liquidus temperature. The specification of the continuous casting billet is 220mm square. The surface of the continuous casting billet is free of defects and no surface grinding treatment is required.

[0022] High rolling force and high speed rolling mill are used for bar rolling. The billet heating temperature is controlled at 1255℃ and the holding time is 2.4h. The deformation of the first three passes of rolling is controlled to be ≤8%, the strain rate is ≤10s-1, the billet surface temperature after the first three passes of billet opening is 1130℃, and the final rolling temperature is 960℃. The finished product specification of the bar after billet opening is φ110mm.

[0023] The yield rate of the entire line from ingot to bar is 89%. Embodiment 2

[0024] AOD uses pure aluminum reduction, and the reduction time is 15 minutes. The LF bottom blowing argon gas supply intensity is controlled at 4L / min / t, and the stirring time is controlled at 14 minutes. The sulfur content in the steel is 0.0008%, the oxygen content in the steel is 0.0007%, and the four types of inclusions A, B, C, and D are level 0, level 0, level 0.5, and level 0 respectively.

[0025] The continuous casting adopts protective slag X-1 with a melting point of 1050℃ and a basicity (CaO / SiO2) of 0.85. The superheat of the molten steel in the tundish is 50℃ higher than the liquidus temperature. The specification of the continuous casting billet is 220mm square. The surface of the continuous casting billet is free of defects and no surface grinding treatment is required.

[0026] High rolling force and high speed rolling mill are used for bar rolling. The heating temperature of the billet is controlled at 1260℃ and the holding time is 2.6h. The deformation of the first three passes of rolling is controlled to be ≤8%, the strain rate is ≤10s-1, the surface temperature of the billet after the first three passes is 1150℃, and the final rolling temperature is 955℃. The finished product specification of the bar after the billet is opened is φ90mm.

[0027] The yield rate of the entire line from ingot to bar is 90%.

[0028] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A method for producing an iron-nickel based alloy bar, characterized in that: The following steps are involved: Step 1: Smelting: Use medium frequency furnace or electric furnace for smelting. The chemical composition by mass percentage after smelting is: C: 1.5-2.5%, Si: 0-0.2%, Mn: 0-0.2%, P: 0-0.025%, S: 0-0.15%, Cr: 19.0-25%, Ni: 28.0%-36%, and the rest is iron and unavoidable impurities; Step 2: Refining: AOD uses pure aluminum reduction, the reduction time is 13-18 minutes, the LF bottom blowing argon gas supply intensity is controlled at 2-5L / min / t, the stirring time is controlled at 10-15 minutes, and the sulfur content in the steel is guaranteed to be ≤0.0010%, the oxygen content in the steel is ≤0.0010%, and the four types of inclusions A, B, C, and D are all less than 0.5 level; Step 3: Billet continuous casting: The continuous casting adopts protective slag with a melting point of 1020-1080℃ and a basicity of CaO / SiO2 of 0.80-0.90, and the superheat of the molten steel in the tundish is controlled to be 40-70℃ higher than the liquidus temperature; Step 4: Rolling: The bars are rolled using a rolling mill.

2. The method for producing an iron-nickel based alloy bar according to claim 1, characterized in that: The specific requirements for bar rolling in step 4 are: the billet heating temperature is controlled at 1240-1280℃, the holding time is 2-3h, the deformation amount in the first three passes is controlled at ≤8%, the strain rate is ≤10s-1, and the billet surface temperature after the first three passes is ensured to be 1120-1200℃, and the final rolling temperature is 950-1000℃.