Steel with excellent performance for oil gas and preparation method thereof
The oil and gas steel prepared through specific chemical composition and process flow solves the shortcomings of existing oil and gas steel in terms of corrosion resistance and high extrusion resistance, and achieves the goals of excellent performance and low cost, which is suitable for deep well oil casing need.
Patent Information
- Application Number
- CN202411090940.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing oil and gas steels have shortcomings in corrosion resistance and high extrusion resistance, and the production costs are high, making it difficult to meet the demand for deep well oil casing.
Chemical components are C: 0.25-0.5%, Si: 0.2-0.4%, Mn: 0.8-1.2%, Cr: 0.3-0.6%, Mo: 0.3-0.5%, Nb: 0.05-0.1%, V: 0.05-0.05- 0.1%, Al: 0.01-0.03%, Ce: 0.002-0.004%, N: 0.01-0.015%, P < 0.015%, O+S < 0.003%, oil and gas steel, through vacuum smelting, casting, rolling and heat treatment Process preparation, the main structure is tempered martensite, room temperature yield strength ≥950MPa, tensile strength ≥1000MPa, room temperature full-size V-shaped notch impact work ≥170J.
It has achieved excellent performance of oil and gas steel, with controllable costs, improved material performance, reduced inclusions, improved rare earth yield during smelting, simple process, low production cost, and surpassed ordinary 125Ksi-grade oil and gas casing steel.
Smart Images

Figure CN119020690A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of steel materials, and in particular relates to oil and gas steel with excellent performance and a preparation method thereof. Background Art
[0002] As a strategic reserve resource, oil and natural gas have always attracted much attention. Most of the proven oil and natural gas deposits are concentrated in areas with harsh natural environments such as deep surface layers and polar oceans; oil and gas wells with completion depths of 4500 to 6000 meters are usually called deep wells. According to statistics, more than 6.2 billion tons of exploitable oil in my country are stored below 5000 meters below the surface; and with the increase in energy demand, the oil resources in the shallow surface layers are over-exploited. Countries around the world are gradually shifting their development focus to areas with rich reserves but extremely harsh mining environments such as deep surface layers and oceans, which has increased the demand for deep well oil casing.
[0003] Conventional oil and gas steel can no longer meet the corrosion resistance requirements of exploration and development and long-term service, and excessive oxygen content in the steel will seriously affect the performance of the material. When the strength of ordinary 13Cr material rises to 110Ksi, the toughness has seriously decreased, and the impact energy value is less than 10J, which cannot meet the requirements of high collapse resistance and high strength and toughness in the service conditions of shale gas wells.
[0004] The patent application with application number CN202210520840.5 provides a 125ksi grade low-alloy oil well pipe steel resistant to sulfide stress cracking, but its process requires two quenchings, and its composition contains nickel and copper. Given the current market conditions of the two, its production cost remains high and is not suitable for large-scale production.
[0005] The patent application with application number CN202310447336.1 provides a 125Ksi high-strength and tough SUP13Cr oil well pipe for shale gas and a hot rolling process manufacturing method, but it contains higher chromium (13%) and nickel (6%), and its alloy cost is more expensive than patent CN202210520840.5; in addition, the control of oxygen in its composition is relatively loose, which is not conducive to the long-term service of the oil well pipe.
[0006] Therefore, developing a high-strength and tough oil and gas steel with excellent performance that meets or even exceeds 125Ksi, low cost, and suitable for large-scale production is a technical problem that needs to be urgently solved by domestic and foreign steel companies. Summary of the invention
[0007] The object of the present invention is to provide an oil and gas steel with excellent performance and a preparation method thereof.
[0008] To achieve the above object, the present invention adopts the following technical solution:
[0009] A steel for oil and gas with excellent performance, whose chemical composition is C: 0.25-0.5%, Si: 0.2-0.4%, Mn: 0.8-1.2%, Cr: 0.3-0.6%, Mo: 0.3-0.5%, Nb: 0.05-0.1%, V: 0.05-0.1%, Al: 0.01-0.03%, Ce: 0.002-0.004%, N: 0.01-0.015%, P < 0.015%, O + S < 0.003%, and the balance is iron and unavoidable impurities.
[0010] Furthermore, the oil and gas steel of the present invention has a main structure of tempered martensite, a room temperature yield strength of ≥950MPa, a tensile strength of ≥1000MPa, and a room temperature full-size V-notch impact energy of ≥170J.
[0011] Furthermore, the method for preparing oil and gas steel of the present invention includes vacuum smelting and casting, rolling and heat treatment steps.
[0012] Furthermore, the vacuum smelting and casting process of the present invention is as follows: smelting is performed according to the target composition, and casting is performed into a square ingot with a bottom of 150*150~160*160; nitrogen is filled into the smelting process before steel is tapped for gas phase nitriding, and the nitriding time is controlled at 10~15min.
[0013] Furthermore, the rolling process of the present invention includes rough rolling and finish rolling; in the rough rolling process, the reduction rate of each pass is controlled below 17%, the start rolling temperature is controlled at 1200±10°C, and the final rolling temperature is controlled at 1130±10°C; in the finish rolling process, the reduction rate of each pass is controlled above 20%, the start rolling temperature is controlled at 1140±15°C, and the final rolling temperature is controlled at 900±10°C. After rolling, the steel plate is slowly cooled to room temperature, and the final thickness of the finished steel plate is controlled at 10-15mm.
[0014] Furthermore, the heat treatment process of the present invention is: quenching and tempering in sequence; the quenching temperature is 870±20°C, kept warm for 50-70 minutes, and then oil-cooled to room temperature; the tempering temperature is 550±10°C, kept warm for 70-90 minutes, and then slowly cooled to room temperature.
[0015] The beneficial effects of adopting the above technical solution are:
[0016] (1) Nb, V, N and Ce in steel can refine grains, thereby improving material properties. In addition, the components of the present invention are all conventional components, containing only trace amounts of rare earths, so the cost of the present invention is controllable.
[0017] (2) Using nitrogen for vapor phase nitriding can not only ensure the uniformity of nitrogen, but also avoid the increase in the content of inclusions, phosphorus, sulfur and gas caused by the addition of nitriding alloys.
[0018] (3) In the present invention, O+S is controlled within 30 ppm, which can not only reduce inclusions in steel from the source, but also improve the recovery rate of rare earths in the smelting process.
[0019] (4) Through the combination of rough rolling and finishing rolling processes, not only can a plate with suitable thickness be quickly obtained, but also a steel plate with high plate shape accuracy and excellent surface quality can be obtained.
[0020] (5) Through a simple two-batch heat treatment process, oil and gas steel with excellent performance (better than general 125Ksi) can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the metallographic structure of the oil and gas steel in Example 1. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described in detail below through specific embodiments.
[0023] Example 1
[0024] A steel for oil and gas, the preparation method of which includes vacuum smelting and casting, rolling, and heat treatment, as follows:
[0025] 1) Vacuum smelting and casting
[0026] According to the relevant target components, 0.1 kg of carbon powder, 0.12 kg of metal silicon, 0.4 kg of electrolytic manganese, 0.12 kg of metal chromium, 0.046 kg of ferroniobium, 0.0382 kg of ferrovanadium, 0.16 kg of molybdenum bars, 0.01 kg of aluminum particles, 0.008 kg of ferrocerium, and 39.01 kg of pure iron were calculated and weighed. The alloy material was baked at 150 ° C for 2.5 hours, and then the pure iron was loaded into the induction furnace. After melting, alloying began gradually. After alloying was completed, sampling was carried out. Before steel was tapped, 15000 Pa of nitrogen was filled for nitriding. The nitriding time was 10 minutes. After the composition was qualified, the temperature was raised and cast into a 150*150*220 mm ingot. The composition of the steel was tested, and the results are shown in Table 1.
[0027] Table 1 Measured values of steel composition in Example 1 (%)
[0028] element C Si Mn Al Cr Ce Nb V Mo P S O N Measured value 0.251 0.301 0.99 0.02 0.308 0.0020 0.075 0.052 0.4 0.003 0.002 0.0008 0.011
[0029] 2) Rolling
[0030] The surface of the ingot was polished and then heated to 1200°C. After keeping the temperature for 2 hours, rough rolling began. The reduction rate of each pass is shown in Table 2. The final rolling temperature of rough rolling was 1140°C. After 8 rolling passes, the ingot was rolled into a 46 mm thick slab.
[0031] Table 2 Data of each pass of rough rolling in Example 1
[0032] path 1 2 3 4 5 6 7 8 Thickness(mm) 137 119 101 84 71 59 49 46 Pressure rate (%) 8.67% 13.13% 15.13% 16.83% 15.48% 16.9% 16.95% 6.12%
[0033] The slab obtained by rough rolling was heated to 1155°C, and after keeping warm for 1.5h, finish rolling began. The reduction ratio of each pass is shown in Table 3. The final rolling temperature of finish rolling was 910°C. After 5 rolling passes, a slab with a thickness of 12mm was obtained, which was then slowly cooled to room temperature.
[0034] Table 3 Data of each pass of finishing rolling in Example 1
[0035]
[0036]
[0037] 3) Heat treatment
[0038] The slab was heated to 890°C, kept at this temperature for 70 minutes, and oil-cooled to room temperature; then the slab was heated to 560°C, kept at this temperature for 1.5 hours, and then slowly cooled to room temperature.
[0039] Example 2
[0040] 1) Vacuum smelting and casting
[0041] According to the relevant target components, the following materials were calculated and weighed: 0.196 kg of carbon powder, 0.08 kg of metal silicon, 0.48 kg of electrolytic manganese, 0.24 kg of metal chromium, 0.0522 kg of ferroniobium, 0.0612 kg of ferrovanadium, 0.2 kg of molybdenum bars, 0.006 kg of aluminum particles, 0.009 kg of ferrocerium, and 38.12 kg of pure iron. The alloy material was baked at 150 ° C for 2.5 hours. The pure iron was then loaded into the induction furnace, and alloying was gradually started after melting. After alloying was completed, samples were taken for testing. Before steel was tapped, 15000 Pa of nitrogen was filled for nitriding. The nitriding time was 15 minutes. After the components were qualified, the temperature was raised and cast into a 160*160*200 mm ingot. The steel grade composition was tested, and the results are shown in Table 4.
[0042] Table 4 Measured values of steel composition in Example 2 (%)
[0043] element C Si Mn Al Cr Ce Nb V Mo P S O N Measured value 0.49 0.205 1.2 0.011 0.6 0.0035 0.085 0.082 0.5 0.004 0.0018 0.0009 0.0147
[0044] 2) Rough rolling and finishing rolling
[0045] The surface of the ingot was polished and then heated to 1210°C. After keeping the temperature for 2.5 h, rough rolling began. The reduction rate of each pass is shown in Table 5. The final rolling temperature of the rough rolling was 1120°C. After 8 rolling passes, the ingot was rolled into a 50 mm thick slab.
[0046] Table 5 Data of each pass of rough rolling in Example 2
[0047] path 1 2 3 4 5 6 7 8 Thickness(mm) 140 118 106 90 77 67 58 50 Pressure rate (%) 12.5% 15.7% 10.16% 15.1% 14.4% 12.98% 13.4% 16%
[0048] The slab obtained by rough rolling was heated to 1125°C, and after keeping warm for 1.5 hours, the finish rolling began. The reduction ratio of each pass is shown in Table 6. The final rolling temperature of the finish rolling was 890°C. After 5 rolling passes, a slab with a thickness of 15 mm was obtained, which was then slowly cooled to room temperature.
[0049] Table 6 Data of each pass of finishing rolling in Example 2
[0050]
[0051]
[0052] 3) Heat treatment
[0053] The slab was heated to 850°C, kept at this temperature for 60 minutes, and oil-cooled to room temperature; the slab was then heated to 540°C, kept at this temperature for 1.2 hours, and then slowly cooled to room temperature.
[0054] Example 3
[0055] 1) Vacuum smelting and casting
[0056] According to the relevant target components, the carbon powder is calculated and weighed, 0.14Kg, metal silicon is 0.152Kg, electrolytic manganese is 0.32Kg, metal chromium is 0.2Kg, ferroniobium is 0.0615Kg, ferrovanadium is 0.0398Kg, molybdenum bar is 0.12Kg, aluminum particles are 0.012Kg, ferrocerium is 0.008Kg, and pure iron is 38.1Kg. The alloy material is baked at 160℃ for 2h. Then the pure iron is loaded into the induction furnace, and alloying is gradually started after melting. After the alloying is completed, sampling and testing are carried out. Before steel is tapped, 15000Pa nitrogen is filled for nitriding. The nitriding time is 13min. After the composition is qualified, the temperature is raised and cast into a 150*150*220mm ingot. The composition of the steel grade is tested, and the results are shown in Table 7.
[0057] Table 7 Measured values of steel composition in Example 3 (%)
[0058] element C Si Mn Al Cr Ce Nb V Mo P S O N Measured value 0.35 0.38 0.8 0.03 0.51 0.0025 0.1 0.052 0.3 0.0035 0.0016 0.0007 0.0127
[0059] 2) Rough rolling and finishing rolling
[0060] The surface of the ingot was polished and then heated to 1190°C. After keeping warm for 2.2 hours, rough rolling began. The reduction rate of each pass is shown in Table 8. The final rolling temperature of rough rolling was 1128°C. After 7 rolling passes, the ingot was rolled into a 50 mm thick slab.
[0061] Table 8 Data of each pass of rough rolling in Example 3
[0062] path 1 2 3 4 5 6 7 Thickness(mm) 135 115 98 83 69 58 50 Pressure rate (%) 10% 14.8% 14.7% 15.3% 16.86% 16.9% 13.8%
[0063] The slab obtained by rough rolling was heated to 1135°C and kept warm for 2 hours before finishing rolling. The reduction ratio of each pass is shown in Table 9. The final rolling temperature of finishing rolling was 905°C. After 6 rolling passes, a slab with a thickness of 10 mm was obtained, which was then slowly cooled to room temperature.
[0064] Table 9 Data of each pass of finishing rolling in Example 3
[0065] path 1 2 3 4 5 6 Thickness(mm) 39 31 24 18 14 10 Pressure rate (%) 22% 20.5% 22.5% 25% 22.2% 28.5%
[0066] 3) Heat treatment
[0067] The slab was heated to 870°C, kept at this temperature for 50 minutes, and oil-cooled to room temperature. The slab was then heated to 548°C, kept at this temperature for 1.4 hours, and then slowly cooled to room temperature.
[0068] Example 4
[0069] 1) Vacuum smelting and casting
[0070] According to the relevant target components, the following materials were calculated and weighed: 0.16Kg of carbon powder, 0.144Kg of metal silicon, 0.42Kg of electrolytic manganese, 0.18Kg of metal chromium, 0.0338Kg of ferroniobium, 0.0765Kg of ferrovanadium, 0.18Kg of molybdenum bars, 0.01Kg of aluminum particles, 0.007Kg of ferrocerium, and 38.79Kg of pure iron. The alloy material was baked at 150°C for 2h. The pure iron was then loaded into an induction furnace, and alloying was gradually started after melting. After alloying was completed, samples were taken for testing. Before steel was tapped, 15000Pa of nitrogen was filled for nitriding. The nitriding time was 12min. After the components were qualified, the temperature was raised and cast into a 160*160*200mm ingot. The steel grade composition was tested, and the results are shown in Table 10.
[0071] Table 10 Measured values of steel composition in Example 4 (%)
[0072] element C Si Mn Al Cr Ce Nb V Mo P S O N Measured value 0.4 0.36 1.05 0.025 0.448 0.0040 0.055 0.1 0.45 0.003 0.002 0.0009 0.012
[0073] 2) Rough rolling and finishing rolling
[0074] The surface of the ingot was polished and then heated to 1205°C. After keeping warm for 2 hours, rough rolling began. The reduction rate of each pass is shown in Table 11. The final rolling temperature of rough rolling was 1135°C. After 9 rolling passes, the ingot was rolled into a 40 mm thick slab.
[0075] Table 11 Data of each pass of rough rolling in Example 4
[0076] path 1 2 3 4 5 6 7 8 9 Thickness(mm) 142 122 105 90 75 63 53 45 40 Pressure rate (%) 11.2% 14.1% 13.9% 14.3% 16.6% 16% 15.8% 15.1% 11.1%
[0077] The slab obtained by rough rolling was heated to 1145°C and kept warm for 1.5h before finishing rolling. The reduction ratio of each pass is shown in Table 12. The final rolling temperature of finishing rolling was 900°C. After 4 rolling passes, a slab with a thickness of 13 mm was obtained, which was then slowly cooled to room temperature.
[0078] Table 12 Data of each pass of finishing rolling in Example 4
[0079] path 1 2 3 4 Thickness(mm) 32 24 18 13 Pressure rate (%) 20% 25% 25% 27.7%
[0080] 3) Heat treatment
[0081] The slab was heated to 875°C, kept at this temperature for 75 minutes, and oil-cooled to room temperature; the slab was then heated to 548°C, kept at this temperature for 1.5 hours, and then slowly cooled to room temperature.
[0082] Example 1 Microstructure of oil and gas steel Figure 1 shown by Figure 1 It can be seen that the main structure is tempered martensite. The metallographic structures of the oil and gas steels in the other embodiments are the same as those in embodiment 1 and are not listed one by one.
[0083] The mechanical properties of the oil and gas steels of each embodiment were tested, and the results are shown in Table 13.
[0084] Table 13 Mechanical properties of oil and gas steel in various embodiments
[0085] Example Yield strength (MPa) Tensile strength(MPa) Full-size V-notch impact energy at room temperature (J) 1 1178 1323 175 2 1223 1305 181 3 1258 1385 179 4 1198 1361 177 Normal 125KSi 870~1000 980~1100 140~150
[0086] It can be seen from Table 13 that the oil and gas steel provided by the present invention has excellent mechanical properties, far exceeding ordinary 125KSi grade oil and gas casing steel.
Claims
1. A steel for oil and gas with excellent performance, characterized in that: The chemical composition of the oil and gas steel is: C: 0.25-0.5%, Si: 0.2-0.4%, Mn: 0.8-1.2%, Cr: 0.3-0.6%, Mo: 0.3-0.5%, Nb: 0.05-0.1%, V: 0.05-0.1%, Al: 0.01-0.03%, Ce: 0.002-0.004%, N: 0.01-0.015%, P < 0.015%, O + S < 0.003%, and the balance is iron and unavoidable impurities.
2. The oil and gas steel with excellent performance according to claim 1, characterized in that: The oil and gas steel has a main structure of tempered martensite, a room temperature yield strength of ≥950MPa, a tensile strength of ≥1000MPa, and a room temperature full-size V-notch impact energy of ≥170J.
3. A method for preparing oil and gas steel according to claim 1 or 2, characterized in that: Including vacuum smelting and casting, rolling and heat treatment processes.
4. The method for preparing oil and gas steel according to claim 3, characterized in that: The vacuum smelting and casting process is to perform smelting and casting according to the target composition; in the smelting process, nitrogen is filled into the steel before tapping for gas phase nitriding, and the nitriding time is controlled within 10 to 15 minutes.
5. The method for preparing oil and gas steel according to claim 3, characterized in that: The rolling process includes rough rolling and finish rolling; in the rough rolling process, the reduction rate of each pass is controlled below 17%, the start rolling temperature is controlled at 1200±10°C, and the final rolling temperature is controlled at 1130±10°C; in the finish rolling process, the reduction rate of each pass is controlled above 20%, the start rolling temperature is controlled at 1140±15°C, and the final rolling temperature is controlled at 900±10°C; after rolling, the steel is slowly cooled to room temperature.
6. The method for preparing oil and gas steel according to claim 3, characterized in that: In the rolling process, the thickness of the final steel plate product is controlled to be 10 to 15 mm.
7. The method for preparing oil and gas steel according to claim 3, characterized in that: The heat treatment process includes quenching and tempering; the quenching temperature is 870±20°C, kept warm for 50-70 minutes, and then oil-cooled to room temperature; the tempering temperature is 550±10°C, kept warm for 70-90 minutes, and then slowly cooled to room temperature.
Citation Information
Patent Citations
Preparation method of superfine grain martensitic steel reinforced and controlled by nano precipitated phase
CN101713046A
Rare earth-containing low-cost high collapse-resisting petroleum casing pipe and production method thereof
CN104630643A
Abrasion-resistant steel with excellent ductility and toughness and manufacturing method thereof
CN109023119A
Preparation method of high-strength, high-toughness and high-collapse-resistance petroleum casing pipe containing rare earth Ce
CN112853215A
Sleeve with high extrusion resistance and sulfur resistance and manufacturing method thereof
CN115637377A