Titanium-containing H-grade anti-corrosion steel for sucker rod and preparation method of titanium-containing H-grade anti-corrosion steel

Through the design and heat treatment process of low nickel, low chromium, vanadium-de-vacancies and titanium, the high cost and anti-hydrogen embrittlement sensitivity of suction rod steel are solved, and high-strength and low-cost H-grade anti-corrosion suction rod steel is achieved. Improve its efficiency under harsh conditions.

CN119020691AInactive Publication Date: 2024-11-26HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411090942.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing suction rod steels have shortcomings in terms of high strength, corrosion resistance and low cost, especially the high cost of nickel and chromium and the anti-hydrogen embrittlement sensitivity, which affects their use efficiency under harsh conditions such as deep wells and heavy oil wells. .

Method used

Using a design scheme of low nickel, low chromium, vanadium-de-vacancies and titanium, the austenite grains are refined through titanium elements and the formation of irreversible hydrogen traps, combined with normalization + tempering or tempering heat treatment technology, high-strength and low-cost Steel for H-grade anti-corrosion suction rods reduces alloy cost and improves hydrogen resistance.

Benefits of technology

It achieves high strength, low cost and good hydrogen resistance, reduces the hydrogen embrittlement sensitivity index, improves the service capacity of materials, and is easy to promote and apply.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020691A_ABST
    Figure CN119020691A_ABST
Patent Text Reader

Abstract

The invention discloses titanium-containing H-grade anti-corrosion sucker rod steel and a preparation method thereof. The sucker rod steel comprises the following chemical components in percentage by mass: 0.30 to 0.35 percent of C, 0.20 to 0.30 percent of Si, 0.80 to 1.00 percent of Mn, 0.20 to 0.30 percent of Mo, 0.70 to 0.80 percent of Cr, 1.10 to 1.30 percent of Ni, 0.05 to 0.07 percent of Ti, less than or equal to 0.01 percent of P, less than or equal to 0.01 percent of S and the balance of iron and inevitable impurities. The preparation method comprises the procedures of smelting, heating, rolling and heat treatment. The heat treatment process can adopt a normalizing and tempering process, and also can adopt a hardening and tempering process. Through reasonable component design and a matched heat treatment process, the H-grade sucker rod steel which is high in strength and low in cost and has certain hydrogen resistance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of special steels, and in particular relates to a titanium-containing H-grade anti-corrosion pumping rod steel and a preparation method thereof. Background Art

[0002] Sucker rods are the most critical load-bearing and consumable components in rod pumping equipment. During crude oil extraction, sucker rods are subject to cyclic loads and corrosive environments, making them prone to breakage and impacting operational efficiency. With the increasing number of deep wells, heavy oil wells, high-pressure pumping wells, and corrosive wells, the service conditions of sucker rods are becoming increasingly stringent. Consequently, the oilfield services industry is placing higher demands on sucker rods, with high strength, corrosion resistance, and low cost being the primary development trends.

[0003] Currently, sucker rods are primarily divided into two categories: steel and non-metallic. Non-metallic sucker rods offer high strength and corrosion resistance, but their high cost limits their application, making steel rods more market-leading. To meet the demands of both upstream and downstream customers, developing high-performance, corrosion-resistant, and low-cost sucker rod steel is crucial.

[0004] 30Ni2CrMnMoVA sucker rod steel is a KD / HL grade steel. It contains 1.65% to 2.00% nickel and 0.85% to 1.10% chromium to enhance corrosion resistance, but the nickel addition significantly increases the alloy's cost. The 0.05% to 1.00% vanadium provides precipitation strengthening, but also comes at a high cost. The present invention removes vanadium and adds titanium. This not only utilizes titanium to refine austenite grains, but also allows titanium precipitates to form irreversible hydrogen traps, effectively improving the material's hydrogen resistance. Summary of the Invention

[0005] The problem to be solved by the present invention is to reduce the alloy cost of 30Ni2CrMnMoVA steel, and to provide a titanium-containing H-grade anti-corrosion pump rod steel and a preparation method thereof. Through reasonable composition design and matching heat treatment process, a high-strength, low-cost H-grade pump rod steel with certain hydrogen resistance is obtained.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A titanium-containing H-grade anti-corrosion sucker rod steel has the following chemical composition and mass percentages: C: 0.30-0.35%, Si: 0.20-0.30%, Mn: 0.80-1.00%, Mo: 0.20-0.30%, Cr: 0.70-0.80%, Ni: 1.10-1.30%, Ti: 0.05-0.07%, P≤0.01%, S≤0.01%, and the balance being iron and unavoidable impurities.

[0008] In the sucker rod steel of the present invention, the content of precious metals nickel and chromium is lower than that of 30Ni2CrMnMoVA sucker rod steel, and titanium replaces vanadium, so it has cost advantages.

[0009] The steel for the pumping rod of the present invention has a yield strength of 850 MPa or more, a tensile strength of 1000 MPa or more, an elongation of 15% or more, a cross-sectional shrinkage of 55% or more, and an impact energy KV2 of 60 J or more.

[0010] The hydrogen embrittlement sensitivity index of the steel for the sucker rod of the present invention is I under the condition of full hydrogen filling. HE ≤75%, with 30Ni2CrMnMoVA steel (I HE ≥88%), the hydrogen embrittlement sensitivity is improved by at least 13%.

[0011] The method for preparing titanium-containing H-grade anti-corrosion pump rod steel of the present invention includes smelting, rolling, and heat treatment steps, which are specifically as follows:

[0012] (1) Smelting: Smelting in a vacuum electromagnetic induction furnace, hot casting of molten steel to obtain steel ingots;

[0013] (2) Heating: Heat the steel ingot to 1050-1150°C and keep it warm for 2.0-2.5 hours;

[0014] (3) Rolling: The steel ingot is rolled into a smooth round bar of specified specifications in multiple passes. The temperature of the hot rolling process is kept in the range of 950-1050℃, and air cooling is used after rolling;

[0015] (4) Heat treatment: Either normalizing + tempering process or quenching and tempering process can be adopted; the normalizing + tempering process is specifically as follows: normalizing temperature is 850-900℃, holding time is 50-60min, air cooling to room temperature, tempering temperature is 550-640℃, holding time is 50-60min, air cooling to room temperature; the quenching and tempering process is specifically as follows: quenching temperature is 850-900℃, holding time is 50-60min, water quenching to room temperature; tempering temperature is 550-640℃, holding time is 50-60min, air cooling to room temperature.

[0016] Furthermore, in the preparation method of the present invention, the diameter of the round bar in the rolling process is Ф16 to Ф25 mm.

[0017] The inventive principle of the present invention is:

[0018] The sucker rod steel described in this invention utilizes a low-nickel, low-chromium design, replacing vanadium with titanium. Compared to 30Ni2CrMnMoVA steel, this reduction in nickel and chromium effectively reduces production costs while maintaining adequate hydrogen resistance. Replacing vanadium with titanium reduces alloy costs, while ensuring strength through titanium's grain refinement and hydrogen resistance through the irreversible hydrogen trapping effect of titanium precipitates. Experimental verification demonstrates that both normalizing and tempering and quenching and tempering heat treatment processes can produce H-grade sucker rod steel that meets both mechanical and hydrogen resistance requirements.

[0019] After the sucker rod steel of the present invention undergoes a normalizing + tempering heat treatment process, the obtained structure is granular bainite, and fine irregular flaky and granular carbides are evenly dispersed on the ferrite matrix, and the strength-toughness matching is further improved; at the same time, the titanium precipitate phase generated during the tempering process is evenly distributed at the grain boundaries and within the grains, and together with the carbides, increases the number of irreversible hydrogen traps in the steel, thereby achieving good strength-toughness matching and a low hydrogen embrittlement sensitivity index.

[0020] After the sucker rod steel of the present invention is subjected to a quenching and tempering heat treatment process, the obtained structure is tempered bainite, and carbides are evenly distributed on the martensite matrix. Compared with normalizing+tempering, the material strength is more advantageous.

[0021] The beneficial effects of adopting the above technical solution are:

[0022] 1. The composition ratio of the present invention adopts a design scheme of low nickel and low chromium, de-vanadium and titanium, which greatly reduces the alloy cost and has far-reaching significance for improving the comprehensive performance of H-grade anti-corrosion pumping rod steel and reducing costs and increasing efficiency.

[0023] 2. The titanium-containing H-grade corrosion-resistant pump rod steel provided by this invention meets the mechanical property requirements for H-grade pump rod steel within a wide tempering temperature range (550-640°C), regardless of whether it is treated with normalizing and tempering or quenching and tempering heat treatment. Compared to the heat treatment system for 30Ni2CrMnMoVA steel, the heat treatment process of this invention offers greater versatility and is more suitable for production line application.

[0024] 3. The microstructure of the sucker rod steel obtained by the present invention may contain a large number of carbides and precipitates, which increases the number of irreversible hydrogen traps in the structure and has lower hydrogen embrittlement sensitivity. While ensuring the mechanical properties, the hydrogen resistance of the material during service can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The metallographic structure of the sucker rod steel of Example 1 (1000X)

[0026] Figure 2 The metallographic structure of the sucker rod steel of Example 5 (1000X);

[0027] Figure 3 is the metallographic structure of comparative sucker rod steel (1000X);

[0028] Figure 4 This is the TEM precipitate morphology (26KX) of the sucker rod steel in Example 5. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described in detail below with reference to specific embodiments.

[0030] Examples 1-6 and Comparative Examples

[0031] The chemical composition of the steel for the pumping rod of each embodiment and comparative example is shown in Table 1. The preparation method thereof includes smelting, heating, rolling and heat treatment steps, which are specifically as follows:

[0032] (1) Smelting: A vacuum induction furnace is used for smelting, and the molten steel is hot-cast to obtain a rectangular ingot with a cross-section of 150 mm × 150 mm;

[0033] (2) Heating and rolling: The ingot was heated to 1050-1150°C, kept warm for 2.0-2.5 h, and then rolled into smooth round bars with a diameter of 16-25 mm through multiple passes. The reduction ratio of each pass was ≥20%. The temperature during the hot rolling process was maintained in the range of 950-1050°C, and air cooling was performed after rolling. The specific process parameters of the hot rolling process of each embodiment and comparative example are shown in Table 2.

[0034] (4) Heat Treatment: Each embodiment can adopt a normalizing + tempering process or a quenching and tempering process. The normalizing + tempering process is specifically as follows: the normalizing temperature is 850-900°C, the holding time is 50-60 minutes, and the steel is air-cooled to room temperature; the tempering temperature is 550-640°C, the holding time is 50-60 minutes, and the steel is air-cooled to room temperature; the quenching and tempering process is specifically as follows: the quenching temperature is 850-900°C, the holding time is 50-60 minutes, and the steel is water-quenched to room temperature; the tempering temperature is 550-640°C, the holding time is 50-60 minutes, and the steel is air-cooled to room temperature. The heat treatment processes of each embodiment and comparative example are shown in Table 3.

[0035] Table 1 Chemical composition (wt%) of the steel used for sucker rods in various embodiments and comparative examples

[0036] Example C Si Mn Mo Cr Ni Ti V P S 1 0.32 0.25 0.82 0.20 0.80 1.23 0.06 / 0.0088 0.0048 2 0.31 0.24 0.88 0.28 0.76 1.23 0.07 / 0.0083 0.0050 3 0.30 0.30 1.02 0.30 0.70 1.10 0.05 / 0.0081 0.0047 4 0.33 0.26 0.89 0.25 0.75 1.19 0.06 / 0.0085 0.0058 5 0.35 0.22 0.80 0.22 0.78 1.25 0.06 / 0.0082 0.0059 6 0.31 0.20 0.90 0.26 0.72 1.30 0.06 / 0.0082 0.0053 Comparative Example 0.31 0.24 0.85 0.25 0.88 1.72 / 0.08 0.0086 0.0056

[0037] Table 2 Hot rolling process parameters of each embodiment and comparative example

[0038] Example Heating temperature / ℃ Holding time / h Rolling diameter / mm Single pass reduction rate / % Hot rolling temperature / ℃ 1 1085 2.0 Ф22 24 980-1020 2 1150 2.0 Ф16 29 950-1035 3 1080 2.5 Ф22 24 974-1005 4 1100 2.0 Ф19 25 960-1024 5 1090 2.0 Ф22 23 985-1030 6 1050 2.5 Ф25 23 991-1040 Comparative Example 1050 2.5 Ф22 23 990-1032

[0039] Table 3 Heat treatment process parameters of each embodiment and comparative example

[0040]

[0041]

[0042] Mechanical property test and pre-hydrogenation slow rate tensile test (SSRT) were carried out on the sucker rod steel of each embodiment and comparative example. The SSRT test process is as follows: first, 5mA / cm 2 The constant current was used for 24 h pre-charging with hydrogen and the stretching rate was 1×10 -6 / s, hydrogen embrittlement sensitivity I HE Calculated using elongation after break and tensile strength, i.e. I HE =1-[σ H (1+δ H ) / σ0(1+δ0)].

[0043] Mechanical properties and hydrogen embrittlement sensitivity index I of the sucker rod steels of various embodiments and comparative examples HE (%)See Table 4.

[0044] Table 4 Performance test results of steel used for pumping rods in various embodiments and comparative examples

[0045]

[0046] As shown in Table 4, the strength and toughness of the steel for sucker rod provided by the present invention are better than those of the comparative example; the hydrogen embrittlement sensitivity index I H ≤75%, the hydrogen embrittlement sensitivity is significantly reduced, indicating that its hydrogen embrittlement resistance is significantly improved.

[0047] The microstructures of the sucker rod steels of Example 1, Example 5 and the comparative example are as follows: Figure 1 、 Figure 2 and Figure 3 shown.

[0048] Depend on Figure 1 and Figure 3 It can be seen that after quenching and tempering heat treatment, the microstructure of the sucker rod steel is lath bainite + a small amount of granular bainite, while the microstructure of the comparative example is granular bainite. The strength and toughness of lath bainite are higher than those of granular bainite. Under the conditions of Example 1, the lath bainite structure is fine, with more grain boundaries and subgrain boundaries, and the number of phase interfaces increases, which acts as a hydrogen trap. Compared with the comparative example, the hydrogen embrittlement sensitivity is reduced to a certain extent.

[0049] Depend on Figure 2 and Figure 3 It can be seen that after normalizing + tempering heat treatment, its microstructure is granular bainite, which is a ferrite matrix with fine irregular strips, granular, fine, and dispersed carbides evenly dispersed; transmission electron microscopy TEM found that there is a certain amount of precipitated phase evenly distributed at the grain boundaries and in the grains, such as Figure 4As shown in the figure, these fine dispersed carbides and precipitated phases form irreversible hydrogen traps with a high content, which can firmly capture hydrogen atoms and play a pinning role, thereby reducing the content of free hydrogen in the material, reducing hydrogen embrittlement sensitivity, and improving the material's resistance to hydrogen embrittlement.

[0050] The microstructures of the sucker rod steels in Examples 2 and 3 are the same as those in Example 1, and the microstructures of Examples 4 and 6 are the same as those in Example 5, and they are not shown one by one.

[0051] Example 5 and the comparative example use the same heat treatment process, but the grains of the sucker rod steel in Example 5 are smaller, indicating that the addition of the Ti element has a significant effect on grain refinement; the microstructure of the comparative example sucker rod steel shows carbide aggregation, larger size, and reduced number, resulting in an increase in its hydrogen embrittlement sensitivity index, which is not conducive to resisting hydrogen embrittlement.

[0052] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A titanium-containing H-grade anti-corrosion steel for oil pumping rods, characterized in that: The chemical composition and mass percentage of the sucker rod steel are as follows: C: 0.30-0.35%, Si: 0.20-0.30%, Mn: 0.80-1.00%, Mo: 0.20-0.30%, Cr: 0.70-0.80%, Ni: 1.10-1.30%, Ti: 0.05-0.07%, P≤0.01%, S≤0.01%, and the remainder is iron and unavoidable impurities.

2. The titanium-containing H-grade anti-corrosion sucker rod steel according to claim 1, characterized in that: The yield strength of the sucker rod steel is ≥850MPa, the tensile strength is ≥1000MPa, the elongation is ≥15%, the cross-sectional shrinkage is ≥55%, and the impact energy KV2 is ≥60J.

3. The titanium-containing H-grade anti-corrosion sucker rod steel according to claim 1, characterized in that: The hydrogen embrittlement sensitivity index of the sucker rod steel under full hydrogen filling condition is I HE ≤75%.

4. A method for preparing titanium-containing H-grade anti-corrosion sucker rod steel according to any one of claims 1 to 3, characterized in that: The invention comprises smelting, heating, rolling and heat treatment processes; the heat treatment process can adopt normalizing + tempering process or quenching and tempering process; the normalizing + tempering process is specifically as follows: the normalizing holding temperature is 850-900°C, the holding time is 50-60min, and the process is air-cooled to room temperature; the tempering temperature is 550-640°C, the holding time is 50-60min, and the process is air-cooled to room temperature; the quenching and tempering process is specifically as follows: the quenching temperature is 850-900°C, the holding time is 50-60min, and the process is water-quenched to room temperature; the tempering temperature is 550-640°C, the time is 50-60min, and the process is air-cooled to room temperature.

5. The method for preparing titanium H-grade anti-corrosion steel for sucker rod according to claim 4, characterized in that: The smelting process comprises smelting in a vacuum electromagnetic induction furnace and hot casting of molten steel to obtain a steel ingot.

6. The method for preparing titanium H-grade anti-corrosion steel for sucker rod according to claim 4, characterized in that: In the heating process, the steel ingot is heated to 1050-1150° C. and kept warm for 2.0-2.5 hours.

7. The method for preparing titanium H-grade anti-corrosion steel for sucker rod according to claim 4, characterized in that: In the rolling process, the steel ingot is rolled into a smooth round bar of specified specifications in multiple passes, the temperature of the hot rolling process is maintained in the range of 950-1050° C., and air cooling is performed after rolling.

8. The method for preparing titanium H-grade anti-corrosion steel for sucker rods according to claim 7, characterized in that: The diameter of the round rod is Φ16-Φ25 mm.

Citation Information

Patent Citations

  • Novel sucker rod steel

    CN102051524A

  • Hydrogen sulfide corrosion-resistant steel for petroleum drill rod and manufacturing method for hydrogen sulfide corrosion-resistant steel

    CN102409240A

  • H-grade sucker rod steel and heat treatment process thereof

    CN116445816A

  • HL-grade novel sucker rod steel and preparation method thereof

    CN116855851A

  • High-toughness sucker rod steel and preparation process thereof

    CN117701988A