TiAl alloy ultra-fine grain preparation method based on multidirectional circulation thermomechanical treatment

Through the multi-directional cyclic deformation heat treatment method, the problems of TiAl alloy being prone to cracking and oxidation at low temperature deformation are solved, high strain accumulation and dynamic recrystallization are achieved, ultrafine crystal structure is obtained, and the plasticity and mechanical properties of the alloy are improved. Suitable for a variety of casting processes.

CN119020710APending Publication Date: 2024-11-26SICHUAN UNIV

Patent Information

Application Number
CN202411161757.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

TiAl alloys are prone to cracking at low temperature deformation, while oxidation is prone to occur during heat treatment of high temperature deformation, and it is difficult for the prior art to achieve efficient grain refinement and tissue refinement.

Method used

The multi-directional cyclic deformation heat treatment method is adopted to achieve high strain accumulation and dynamic recrystallization by controlling deformation passages, deformation temperature and deformation amount, and the ultrafine crystal structure of TiAl alloy is obtained. The method includes smelting and densification treatment, compression deformation in the vertical direction of the α2+γ phase region multiple times, and cyclic deformation in the heat treatment furnace, and finally rapid cooling to retain crystal defects.

Benefits of technology

It effectively improves the plasticity and mechanical properties of TiAl alloys and avoids oxidation problems during high temperature deformation. It is suitable for TiAl alloys with different components and casting processes, realizing the preparation of ultrafine crystal structures, and has a simple process and high versatility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020710A_ABST
    Figure CN119020710A_ABST
Patent Text Reader

Abstract

The invention discloses a TiAl alloy ultrafine grain preparation method based on multidirectional cyclic thermomechanical treatment, which comprises the following steps: firstly, smelting and densifying alloy to obtain a dense TiAl alloy workpiece; then, after the TiAl alloy workpiece is subjected to pre-heat-preservation treatment for 5-20 min, the TiAl alloy workpiece is subjected to compression deformation in the A direction, the B direction and the C direction which are perpendicular to one another in sequence under the constant-temperature condition, and one-time multi-direction deformation treatment is completed; repeating the steps according to the multi-directional deformation processing method for multiple times to realize multi-directional cyclic deformation; and after the multidirectional circulating deformation is completed, a sample is rapidly taken out of the heat treatment furnace and placed in air to be naturally cooled to the room temperature, and the ultrafine TiAl alloy is obtained. According to the method, high strain accumulation is achieved by controlling technological parameters such as deformation pass and deformation temperature, the crystal defect density and the dynamic recrystallization degree of the material are continuously improved, and infinite circulation thermomechanical treatment of the TiAl alloy is achieved, so that the TiAl alloy ultra-fine grain structure is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal processing of high-temperature structural materials, in particular to a method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment. Background Art

[0002] TiAl alloy has the characteristics of low density, excellent comprehensive mechanical properties, good oxidation resistance and high temperature resistance. The target service temperature is 650-1000℃. Since TiAl alloy has the excellent properties of light weight and heat resistance, it is widely considered to be an ideal material for manufacturing important hot end components such as aerospace. It can greatly reduce structural weight, improve the thrust-to-weight ratio and maneuverability of aircraft, and has great engineering value and application prospects.

[0003] The mechanical properties of TiAl alloys are strongly dependent on grain size. For example, as the grain size of the full lamellar structure is refined from 2600μm to 250μm, the room temperature yield strength of the alloy increases from 380MPa to 500MPa, and its plasticity can increase from 0.2% to 2.0%. TiAl alloys have the advantages of light weight and high strength, but their low room temperature plasticity and insufficient processing and forming capabilities limit the widespread application of TiAl alloys. Studies have shown that for cast structures, as the grain size of the structure decreases, its plasticity can be significantly improved, which means that refining the structure is a necessary condition for effectively improving the plasticity of the alloy.

[0004] Patent CN117845098A discloses a TiAl alloy, a method and application of deformation heat treatment, which uses pre-deformation and isothermal heat treatment to refine the alloy grains to obtain fine-grained dual-state structure and fine-grained near-lamellar structure. The deformation amount of this method can be adjusted in a small range. Since the TiAl alloy has low plasticity and poor deformation capacity, unidirectional compression at this temperature can easily cause cracking of the sample when the deformation amount is large; and low deformation makes it difficult to introduce sufficient crystal defects, and there is a lack of nucleation centers during the subsequent isothermal heat treatment process, which limits the degree of alloy structure refinement. Therefore, unidirectional deformation heat treatment at a certain temperature requires high precision control of the deformation amount.

[0005] Patent CN107952922B discloses a method for forging TiAl alloy, which adopts a three-way sheathed forging method and uses dynamic recrystallization to refine the structure. This method is sheathed forging, that is, the ingot needs to be sheathed, and after the insulation is completed, it is transferred to the compressor. During the transfer process, the sample will have a certain temperature loss. The insulation temperature range used is the α+γ two-phase region, and the temperature is relatively high. Similarly, patent CN116219338A discloses a method for regulating fine dual-state or full-lamellar structure of niobium-containing TiAl alloy, which uses multi-directional forging combined with heat treatment to prepare a method for regulating fine dual-state or full-lamellar structure. This method uses a sheath, and after heat treatment, it is transferred from the heat treatment furnace to the hot pressing equipment for deformation. Heat will be lost during the transfer process, and the sample temperature may be uneven due to cooling, resulting in uneven deformation. Moreover, the insulation temperature is the middle temperature of the α+γ two-phase region. At this temperature, hot pressing not only causes recrystallization, but also complex organizational evolutions such as ordered and disordered transformation of the α phase and γ→α phase transformation will occur.

[0006] In summary, the existing TiAl alloy crystal structure has intrinsic brittleness and difficulty in low-temperature plastic deformation. In addition, excessively high deformation temperature can easily cause grain growth and oxidation in the alloy. At the same time, the high deformation temperature also places high demands on the working conditions of the equipment. Summary of the invention

[0007] In view of the problems of easy cracking during low-temperature deformation and oxidation during high-temperature deformation heat treatment in the existing TiAl alloy processing technology, the present invention provides a TiAl alloy ultrafine grain preparation method based on multi-directional cyclic deformation heat treatment. The method achieves high strain accumulation by controlling process parameters such as deformation passes and deformation temperature, continuously improves the crystal defect density and dynamic recrystallization degree of the material, realizes infinite cyclic deformation heat treatment of TiAl alloy, and thus obtains TiAl alloy ultrafine grain structure.

[0008] The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment provided by the present invention comprises the following steps:

[0009] S1. Perform alloy smelting and densification treatment to obtain a dense TiAl alloy workpiece.

[0010] The specific method is as follows: firstly, a TiAl alloy ingot is prepared by smelting, wherein the impurity O introduced into the TiAl alloy ingot does not exceed 0.05% by atomic percentage, and the TiAl alloy ingot is subjected to hot isostatic pressing to reduce solidification segregation and micro defects generated during the casting process, thereby obtaining a dense TiAl alloy workpiece.

[0011] S2, performing multi-directional deformation treatment on the TiAl alloy workpiece; comprising the following sub-steps:

[0012] S21. Heat the heat treatment furnace of the universal testing machine to temperature T, which is the upper temperature of the α2+γ phase region, and then place the TiAl alloy workpiece in a compression fixture in the heat treatment furnace for pre-heating. The temperature holding time is 5 to 20 minutes. The range of temperature T is: T α2→α -ΔT≤TemperatureT<T α2→α , T α2→α It is the temperature at which the α phase undergoes order-disorder transition, 100℃≤ΔT≤300℃.

[0013] S22. After the pre-heat preservation is completed, the TiAl alloy workpiece is subjected to compression deformation in three mutually perpendicular directions of A, B, and C in sequence under constant temperature conditions; first, the TiAl alloy workpiece is subjected to compression deformation along the A direction, the compression deformation amount is 10% to 25%, and the compression deformation rate is 0.1s -1 ~0.001s -1 ; In order to reduce heat loss during the experiment, the TiAl alloy workpiece was flipped 90° in the heat treatment furnace directly after deformation, and then the billet was compressed and deformed along the B direction; then the TiAl alloy workpiece was flipped 90° again, and the TiAl alloy workpiece was compressed and deformed along the C direction, completing a multi-directional deformation.

[0014] S3. Repeat the method of step S22 for multiple times for the sample obtained in step S22, i.e., realize multi-directional cyclic deformation; the size of the alloy hardly changes significantly before and after each deformation; finally, quickly take the sample out of the heat treatment furnace, place it in the air and naturally cool it to room temperature to obtain an ultrafine TiAl alloy.

[0015] Preferably, the atomic percentage content of the specific components of the TiAl alloy is in the range of: Ti-(43-49)Al-(0-8)X-(0-0.5)Z. The X element is selected from one or more of Nb, Cr, Mo, Ta, V, and Mn; the Z element is selected from one or more of Fe, C, N, O, B, and Si. In particular, since the specific component content of the TiAl alloy has an influence on the TiAl alloy α phase order-disorder transition temperature and the γ→α phase transition temperature, the specific component range of the TiAl alloy in the present invention should enable the TiAl alloy to meet the above-mentioned phase temperature range requirements.

[0016] Preferably, in step S1, the temperature of the hot isostatic pressing treatment is between T α2→α and T γ→α+γ Between α2→α is the temperature at which the α phase undergoes order-disorder transition, T γ→α+γ It is the temperature at which the γ→α phase transition begins, that is, the phase transition temperature at the lower end of the α+γ two-phase region.

[0017] Further preferably, after the hot isostatic pressing treatment, the square TiAl alloy workpiece is obtained by machining or wire cutting.

[0018] In the above method, step S21, pre-heating at the upper temperature of the α2+γ phase region for 5 minutes to 20 minutes, the purpose of which is to eliminate the lamellar structure and other phase structures and undesirable structures existing in the blank by heat preservation at the upper temperature of the α2+γ phase region for a certain period of time, while ensuring the uniformity of temperature in various parts of the compressed blank, preventing cracking caused by uneven temperature during deformation, and ensuring the controllability of organizational changes during deformation.

[0019] In step S22, the compression deformation amount of a single pass is controlled to be 10% to 25%, and the compression deformation rate is 0.1s -1 ~0.001s -1 , the deformation amount of a single compression deformation is small and the deformation rate is fast. The purpose is: a small strain cannot promote a large number of defects in the crystal, which is not conducive to the occurrence of ultrafine microstructures, and a large strain is easy to cause macroscopic defects in the material. Therefore, a small deformation amount is set for a single pass. Under the condition of ensuring that no cracking occurs, the accumulation of strain is increased by increasing the number of deformation passes. The diffusion rate of atoms is accelerated at high temperatures, and the number of point defects and dislocation density in the crystal will be reduced through the high-temperature recovery mechanism. The reduction of crystal defects is not conducive to the refinement of the microstructure, so a faster strain rate range is adopted. Through the precise control of the compression deformation amount and the compression deformation rate, while reducing the occurrence of cracks, dynamic recrystallization is introduced through high-temperature deformation to promote the formation of ultrafine grains.

[0020] In step S3, after the multi-directional cyclic deformation is completed, the sample is quickly taken out from the heat treatment furnace. The purpose is to retain the crystal defects caused by the deformation during the air cooling process and prevent the grain growth caused by too long holding time.

[0021] The TiAl alloy is treated by the multi-cycle isothermal multi-directional deformation treatment method of the present invention, and an ultrafine grain structure composed of recrystallized grains can be obtained. The original coarse lamellar clusters and blocky γ grains are replaced by fine equiaxed recrystallized grains, and the volume fraction of recrystallized grains increases with the increase of deformation passes and gradually approaches 100%, and the average recrystallized grain size is less than 2μm.

[0022] Compared with the prior art, the present invention is beneficial in that:

[0023] (1) The present invention adopts a thermomechanical treatment method that combines low temperature with a single small deformation amount, and achieves high strain accumulation by infinitely increasing the number of deformation passes, thereby ensuring that the sample is not easy to crack. This solves the problem of TiAl alloy being prone to cracking due to low-temperature deformation, while avoiding oxidation during high-temperature thermomechanical treatment. During this thermomechanical treatment process, while increasing the number of deformation passes, while maintaining the sample size and shape without significant changes, the crystal defect density and dynamic recrystallization degree of the material are continuously increased, causing the material to undergo severe plastic deformation, thereby improving the degree of alloy structure refinement and realizing the preparation of ultrafine grains of TiAl alloy.

[0024] (2) The present invention has a wide range of applications and is applicable to TiAl alloys of different compositions. It has no special requirements for the casting process for obtaining TiAl alloy billets and is applicable to TiAl alloys obtained by various casting processes such as gravity casting, counter-gravity casting, and centrifugal casting. The present invention can effectively eliminate lamellar structures and undesirable structures existing in billets through hot isostatic pressing and multi-pass deformation, thereby eliminating the influence of the hereditary nature of the casting structure. Therefore, there are no special requirements for the initial structure of the TiAl alloy obtained by casting. For TiAl alloys with different casting processes and different initial structures, multi-directional cyclic deformation heat treatment as described in the specific steps of the present invention can be controlled to obtain an ultrafine grain structure composed of fine recrystallized grains, and the process has high versatility.

[0025] (3) The present invention can achieve the regulation of recrystallization ratio and recrystallized grain size and obtain fine-grained structure by accurately designing and controlling the deformation passes, deformation amount, deformation rate and deformation temperature during the thermomechanical treatment process. In the examples of the present invention, in the obtained fine-grained structure, the refinement degree of the lamellar clusters exceeds 2 times, and the refinement degree of the equiaxed γ grains exceeds 15 times.

[0026] (4) The present invention can perform subsequent heat treatment on the basis of the ultrafine grain structure obtained by the deformation heat treatment to eliminate the residual internal stress after deformation. By adjusting the heat treatment temperature and time, the characteristic parameters of the structure can be accurately controlled to obtain fine-grained near-lamellar structure and fine-grained full-lamellar structure, thereby improving the comprehensive mechanical properties of the TiAl alloy.

[0027] (5) The deformation process of the present invention is carried out in a heat treatment furnace, so there is no need for sheathing treatment, and the operation steps are simple; at the same time, the temperature loss from the heat treatment furnace to the deformation equipment is avoided, the temperature error caused by the transfer of the sample is reduced, and the consistency of the test results is ensured. In addition, the operating principle of the present invention is simple, the engineering investment is low, and the deformation heat treatment method can be carried out on a general universal testing machine or press, and there are no special requirements for the heating and cooling processes. The deformation heat treatment process does not require complex processing equipment, and it is practically feasible.

[0028] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention is a flow chart of the method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment.

[0030] Figure 2 This is the process flow chart of deformation heat treatment.

[0031] Figure 3 Schematic diagram of the multi-directional cyclic deformation principle.

[0032] Figure 4 Microstructure diagrams of Ti-48Al-2Cr-2Nb at different treatment stages, (a) represents after hot isostatic pressing, (b) represents after unidirectional deformation, (c) represents after one multi-directional cyclic deformation, and (d) represents after four multi-directional cyclic deformation. DETAILED DESCRIPTION

[0033] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0034] Taking Ti-48Al-2Cr-2Nb alloy as an example, the method of obtaining ultrafine grains of TiAl alloy by multi-directional cyclic deformation of the present invention is as follows: Figure 1-3 As shown, the specific steps are as follows:

[0035] (1) The Ti-48Al-2Cr-2Nb alloy is obtained by a water-cooled copper crucible induction shell melting method, and the alloy composition is determined by an inductively coupled atomic emission spectrometer. The alloy is subjected to a hot isostatic pressing treatment at 1160° C., 140 MPa, and 4 h.

[0036] (2) Multi-directional cyclic deformation heat treatment: Heat the heat treatment furnace of the universal testing machine to 900°C, put the above Ti-48Al-2Cr-2Nb alloy into the heat treatment furnace of the universal testing machine, and keep it warm for 10 minutes. Figure 3 As shown in the figure, after the pre-insulation is completed, the TiAl alloy workpiece is compressed and deformed along the A direction under constant temperature conditions. After deformation, the sample is directly turned 90° in the heat treatment furnace, and then the TiAl alloy workpiece is compressed and deformed along the B direction; then the sample is turned 90° again, and the TiAl alloy workpiece is compressed and deformed along the C direction. The above deformation along the A, B, and C directions is defined as one multi-directional deformation. During the compression deformation process, the deformation speed is 0.01s -1Compression is carried out with a single-pass deformation of 20%, which ensures the uniformity of the sample temperature. The lower single-pass deformation ensures that the sample is not prone to cracking.

[0037] (3) Repeat the isothermal multidirectional deformation multiple times according to the multidirectional deformation method in step (2), that is, perform multidirectional cyclic deformation treatment. After each compression deformation, the sample is flipped 90°, that is, the compression deformation is continuously cycled along the three directions of A→B→C. After completing the multidirectional cyclic deformation treatment, the sample is quickly taken out of the heat treatment furnace, placed in the air and naturally cooled to room temperature to obtain an ultrafine TiAl alloy. This embodiment has undergone 4 cycles of multidirectional deformation (i.e., compression 4 times along the A, B, and C directions respectively).

[0038] Figure 4 The microstructure pictures of Ti-48Al-2Cr-2Nb alloy at different processing stages. Figure 4 a is a scanning electron microscope photograph of the hot isostatic pressing structure after step (1), and its organizational characteristics are bimodal structure, the average lamellar cluster size is about 200 μm, and the average grain size of the blocky γ grains is about 25 μm. Figure 4 b is a scanning electron microscope photo of the microstructure after uniaxial compression deformation treatment. The lamellae are obviously bent and kinked, γ recrystallization occurs at the boundaries of the lamellae clusters, and some lamellae are broken and γ recrystallized inside the lamellae clusters. The average lamellae cluster size is reduced to 145μm, the recrystallized grains are fine, the average grain size is about 1.2μm, and the volume of fine recrystallized γ grains accounts for about 5%; Figure 4 c is a scanning electron microscope photograph of the microstructure after one cycle of multi-directional deformation (i.e., compression once in directions A, B, and C, respectively) in step (2). The average lamellar cluster size is reduced to 138 μm, the average recrystallized γ grain size is about 1.4 μm, and the volume proportion of recrystallized γ grains is about 18%; Figure 4 d is a scanning electron microscope photo of the microstructure after 4 cycles of multi-directional deformation in step (3) (i.e., compression 4 times in directions A, B, and C, respectively). The average lamellar cluster size is reduced to 86 μm, the volume of recrystallized γ grains accounts for about 70%, the recrystallized grains are small, the average recrystallized γ grain size is about 1.4 μm, and twinning occurs in some recrystallized grains. It can be predicted that when the number of cyclic deformations is infinitely increased, an ultrafine grain structure with a volume of recrystallized grains close to 100% can be obtained.

[0039] The Ti-48Al-2Cr-2Nb alloy in this embodiment is subjected to the above-mentioned multi-directional cyclic deformation heat treatment control, and the microstructure is significantly refined to form an ultrafine grain structure composed of ultra-fine γ grains. The compression mechanical properties of the Ti-48Al-2Cr-2Nb alloy before and after the method are tested. Compared with the undeformed alloy, the yield strength is increased by 140% after 4 multi-directional cyclic deformations. This shows that the multi-directional cyclic deformation heat treatment control method can effectively improve the mechanical properties of TiAl alloys.

[0040] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment, characterized in that: The following steps are involved: S1, performing alloy smelting and densification treatment to obtain a dense TiAl alloy workpiece; S2, subjecting the TiAl alloy workpiece to multi-directional deformation treatment; It includes the following sub-steps: S21, heating the heat treatment furnace to a temperature T, and then placing the TiAl alloy workpiece in a compression fixture in the heat treatment furnace for pre-heat preservation, the heat preservation time being 5 to 20 minutes; S22. After the pre-heat preservation is completed, the TiAl alloy workpiece is subjected to compression deformation in three mutually perpendicular directions of A, B, and C in sequence under constant temperature conditions; first, the TiAl alloy workpiece is subjected to compression deformation along the A direction, the compression deformation amount is 10% to 25%, and the compression deformation rate is 0.1s -1 ~0.001s -1 ; After deformation, the TiAl alloy workpiece is directly turned 90° in the heat treatment furnace, and then the blank is compressed and deformed along the B direction; then the TiAl alloy workpiece is turned 90° again, and the TiAl alloy workpiece is compressed and deformed along the C direction, that is, a multi-directional deformation is completed; S3. Repeat the method of step S22 for multiple times for the sample obtained in step S22, i.e., realize multi-directional cyclic deformation; finally, quickly take the sample out of the heat treatment furnace, place it in the air and naturally cool it to room temperature to obtain an ultrafine TiAl alloy.

2. The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment according to claim 1, characterized in that: In step S21, the value range of temperature T is: T α2→α -ΔT≤TemperatureT<T α2→α , T α2→α It is the temperature at which the α phase undergoes order-disorder transition, 100℃≤ΔT≤300℃.

3. The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment according to claim 1, characterized in that: Step S1 specifically includes: preparing a TiAl alloy ingot by smelting, and performing hot isostatic pressing on the TiAl alloy ingot to obtain a dense TiAl alloy workpiece.

4. The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment according to claim 3, characterized in that: The atomic percentage content range of the specific components of the TiAl alloy is: Ti-(43-49)Al-(0-8)X-(0-0.5)Z. The X element is selected from one or more of Nb, Cr, Mo, Ta, V, and Mn; the Z element is selected from one or more of Fe, C, N, O, B, and Si.

5. The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment according to claim 3, characterized in that: The impurity O introduced into the TiAl alloy ingot does not exceed 0.05% by atomic percentage.

6. The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment according to claim 3, characterized in that: The temperature of the hot isostatic pressing treatment is between T α2→α and T γ→α+γ Between α2→α is the temperature at which the α phase undergoes order-disorder transition, T γ→α+γ is the temperature at which the γ→α phase transition begins.

7. The method for preparing ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment according to claim 6, characterized in that: After hot isostatic pressing, a square TiAl alloy workpiece is obtained by machining or wire cutting.

8. An ultrafine grain TiAl alloy, characterized in that: The ultrafine grains of TiAl alloy are prepared by the method for preparing the ultrafine grains of TiAl alloy based on multi-directional cyclic deformation heat treatment as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • A method for forging TiAl alloy billets

    CN107952922B

  • Method for regulating and controlling fine double-state or full lamellar structure of niobium-containing TiAl alloy

    CN116219338A

  • TiAl alloy, deformation-based heat treatment method and application

    CN117845098A

Cited By

  • Preparation method of TiAl alloy disc for high-temperature thermoforming engine

    CN122256737A