Method for improving hydrogen embrittlement resistance of austenitic stainless steel
The low-temperature two-stage carburizing method is used to form a high-stability carburizing layer and a high residual compression stress layer on the surface of austenitic stainless steel, which solves the brittleness problem of austenitic stainless steel in a hydrogen environment, significantly reduces the risk of hydrogen embrittlement failure and is applicable for complex shape parts.
Patent Information
- Application Number
- CN202411130686.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
Austenitic stainless steel is prone to brittle fracture in hydrogen environment, and the existing hydrogen-resistance coating and hydrogen-resistant embrittlement materials improvement methods are costly or difficult to adapt to complex shape parts, and shot peening will lead to the surface martensite phase. Change, increase hydrogen embrittlement sensitivity.
The low-temperature two-stage carburizing method is adopted to form a carbon-rich carburizing layer and a high residual compression stress layer through controlled atmosphere of low-temperature carburizing and carbon diffusion treatment, thereby improving the surface stability and hydrogen resistance of austenitic stainless steel. Crispy properties.
It significantly reduces the risk of hydrogen embrittlement failure of austenitic stainless steel parts, and reduces hydrogen embrittlement performance loss by at least 50%. It is suitable for complex-shaped parts and maintains high residual compression stress to hinder hydrogen penetration.
Smart Images

Figure CN119020720A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen energy, and in particular relates to a method for improving the hydrogen embrittlement resistance of austenitic stainless steel. Background Art
[0002] The realization of hydrogen energy technology is inseparable from the use of metal components. The storage, transportation, and supply of hydrogen all use a large number of steel tanks, pipelines, valves, compressors, etc. It is well known that in a hydrogen environment or when hydrogen atoms are dissolved inside the material, the plasticity and toughness of the metal will be greatly reduced, and unpredictable brittle fracture phenomena, namely hydrogen embrittlement, will occur. After long-term research, researchers have found that austenitic stainless steel exhibits better hydrogen embrittlement resistance than other materials at both high and low temperatures. Therefore, austenitic stainless steel has begun to be used in the field of hydrogen energy to manufacture valves, pipelines, and storage tanks. However, a large number of tests have shown that the hydrogen embrittlement sensitivity of austenitic stainless steel is still very high. For example, the technical report "Technical reference for hydrogen compatibility of materials" by San Marchi et al. mentioned that the maximum plasticity loss of austenitic stainless steel in a hydrogen environment is nearly 80%. It can be seen that it is urgent to improve the hydrogen embrittlement resistance of austenitic stainless steel through technology to improve the safety and reliability of hydrogen energy system components.
[0003] Traditionally, methods to improve the hydrogen embrittlement resistance of materials include the use of hydrogen embrittlement coatings and the development of new hydrogen embrittlement-resistant materials. These technologies are either vulnerable to damage or are far away or too costly. For example, hydrogen embrittlement coatings are prone to peeling. For austenitic stainless steel, Wang et al. pointed out in the article "Hydrogen embrittlement of catholically hydrogen-precharged 304Laustenitic stainless steel: Effect of plastic pre-strain" that the hydrogen embrittlement resistance of materials can be improved by increasing the stability of the austenite phase. The stability of the austenite phase increases with the increase in the content of austenite stabilizing elements, especially nickel, manganese, carbon and other elements. Therefore, it is necessary to control the content of alloying elements during the smelting of austenitic stainless steel, but this will lead to a significant increase in material costs. Recently, Song et al. pointed out in the article "Improvement of hydrogen embrittlement resistance of 2205duplex stainless steel by laser peening" that compressive residual stress can prevent hydrogen from entering the interior of the material. The commonly used method of applying residual compressive stress is mainly through shot peening, which has the defect of not being able to adapt to complex-shaped parts. It is difficult to introduce high residual stress using traditional carburizing methods, and this will cause the corrosion resistance of stainless steel to decrease. Mechanical surface strengthening using shot peening will introduce residual stress and cause martensitic transformation on the surface of austenitic stainless steel, thereby increasing hydrogen embrittlement sensitivity. Therefore, finding a suitable carburizing method and using these two methods to improve hydrogen embrittlement resistance, combining high-stable austenite and high residual stress on the surface, and controlling the residual stress while carburizing are technical problems that need to be solved urgently. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a method for improving the hydrogen embrittlement resistance of austenitic stainless steel. The method can form a hydrogen embrittlement resistance strengthening layer with ultra-high austenite stability and controllable ultra-high residual pressure stress below the surface of austenitic stainless steel parts, thereby greatly reducing the risk of hydrogen embrittlement failure of austenitic stainless steel parts.
[0005] To achieve the above object, the present invention provides a method for improving the hydrogen embrittlement resistance of austenitic stainless steel, comprising the following steps:
[0006] (a) degreasing austenitic stainless steel with a degreasing agent and then brightening it with a brightening agent;
[0007] (b) placing the brightened austenitic stainless steel in an atmosphere furnace, introducing nitrogen into the atmosphere furnace while raising the temperature to a first preset temperature, maintaining the temperature at the first preset temperature, performing an activation treatment, and introducing a first mixed gas into the atmosphere furnace during the first heat preservation treatment;
[0008] (c) introducing nitrogen into the atmosphere furnace and simultaneously raising the temperature to a second preset temperature; when the temperature of the atmosphere furnace reaches the second preset temperature, introducing a second mixed gas into the atmosphere furnace and maintaining the temperature at the second preset temperature to perform carburizing treatment;
[0009] (d) after the carburizing treatment is completed, nitrogen is introduced into the atmosphere furnace, and the temperature is maintained at the second preset temperature to perform carbon diffusion treatment;
[0010] (e) After the carbon diffusion treatment is completed, nitrogen is kept flowing to reduce the temperature;
[0011] (f) brightening the cooled austenitic stainless steel in the brightening agent.
[0012] Furthermore, the degreasing agent is a 20% mass fraction sodium hydroxide solution, and the brightening agent is a mixed solution of 50% volume concentration hydrochloric acid and 5g / L hexamethyltetramine.
[0013] Further, in step (b), the first preset temperature is 200-350° C., and the heating rate to the first preset temperature is 10° C. / minute.
[0014] Furthermore, in step (b), the heating rate of heating to the first preset temperature is 10° C. / minute.
[0015] Further, in step (b), the composition of the first mixed gas by volume is (2-10%) H2: (25-60%) HCl: (73-30%) N2.
[0016] Further, in step (c), the second preset temperature is 400-550° C., and the heating rate to the second preset temperature is 10° C. / minute.
[0017] Furthermore, in step (c), the heating rate of heating to the second preset temperature is 10° C. / minute.
[0018] Further, in step (c), the composition of the second mixed gas by volume is (0.1-3%) CO2: (15-35%) CO: (20-40%) H2: (64.9-22%) N2.
[0019] The present invention also provides an austenitic stainless steel processed by the above method.
[0020] The present invention also provides an application of the above method for improving the hydrogen embrittlement resistance of austenitic stainless steel.
[0021] Compared with the prior art, the present invention has the following advantages and technical effects:
[0022] After being treated by the method of the present invention, a carburized layer rich in carbon can be formed within the range of 0 to 40 microns below the surface of the austenitic stainless steel, and the mass fraction of the surface carbon element is not less than 1.8%, which can greatly improve the stability of the austenite phase within the range of 0 to 40 microns below the surface of the austenitic stainless steel.
[0023] The austenitic stainless steel treated by the method of the present invention has huge residual compressive stress within the range of 0 to 40 microns below the surface, and the residual compressive stress on the surface is not less than 1000 MPa. Such high residual compressive stress can significantly hinder hydrogen penetration.
[0024] The hydrogen embrittlement performance of the austenitic stainless steel parts treated by the method of the present invention is reduced by at least 50% calculated by elongation loss, thereby greatly reducing the risk of hydrogen embrittlement failure of the treated stainless steel parts.
[0025] At the same time, the method of the present invention is suitable for parts with complex shapes; and can simultaneously achieve improved austenite stability and ultra-high residual compressive stress in a layer below the surface of the part treated by the method of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The figure is a flow chart of the hydrogen embrittlement resistance surface treatment process of the present invention.
[0028] Figure 2 Schematic diagram and photograph of the austenitic stainless steel object parts of Example 1, the dimensions indicated in the figure are in mm.
[0029] Figure 3 The present invention is an atmosphere-time-temperature flow chart of the anti-hydrogen embrittlement surface treatment process.
[0030] Figure 4 The cross-sectional metallographic photographs of the parts before and after being treated by the anti-hydrogen embrittlement surface treatment process of Example 1.
[0031] Figure 5This is a diagram showing the residual stress distribution along the depth of the example after the anti-hydrogen embrittlement surface treatment process of Example 1.
[0032] Figure 6 The hydrogen contents of Example 1 with anti-hydrogen embrittlement surface treatment, Example 2 with only low residual stress carburized sample, and Comparative Example 1 with untreated sample after hydrogen charging.
[0033] Figure 7 The X-ray diffraction patterns of Example 1 treated by the anti-hydrogen embrittlement surface treatment process and Comparative Example 1, an untreated sample, before and after hydrogen charging.
[0034] Figure 8 The tensile curves of Example 1 treated with the anti-hydrogen embrittlement surface treatment process and Comparative Example 1, which is an untreated sample, under hydrogen filling and without hydrogen filling. DETAILED DESCRIPTION
[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0036] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0037] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0038] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0039] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0040] In view of the shortcomings of the prior art, the present invention proposes a surface treatment process for improving the hydrogen embrittlement resistance of austenitic stainless steel. The method innovatively adopts a low-temperature two-stage carburizing method to achieve supersaturated carburizing and control of ultra-high residual stress. The first stage adopts atmosphere-controlled low-temperature carburizing to achieve supersaturated carbon penetration and promote material surface expansion. The second stage adopts time-controlled carbon diffusion under nitrogen to stabilize the deformation of the carburized layer, thereby maintaining ultra-high residual stress.
[0041] Specifically, Figure 1 The figure is a process diagram of the surface treatment process for hydrogen embrittlement resistance of austenitic stainless steel according to the present invention. Figure 1 As shown, the hydrogen embrittlement resistance surface treatment process for austenitic stainless steel of the present invention comprises the following steps:
[0042] Step (a): Pre-treatment
[0043] Degreasing and brightening of target austenitic stainless steel parts;
[0044] Step (b): Activation treatment
[0045] The target austenitic stainless steel parts are placed in an atmosphere furnace and heated to a constant temperature and kept warm while the mixed gas is introduced in different stages;
[0046] Step (c): Carburizing
[0047] The temperature in the atmosphere furnace is raised to a set temperature and kept constant while the mixed gas is introduced in different stages;
[0048] Step (d): Carbon diffusion treatment
[0049] Keep the temperature in the atmosphere furnace constant and introduce only nitrogen gas at the same time;
[0050] Step (e): Cooling
[0051] The temperature in the atmosphere furnace is cooled down to below 50°C at a certain rate;
[0052] Step (f): Post-processing
[0053] The target austenitic stainless steel parts in the atmosphere furnace are taken out and immersed in the brightener.
[0054] Furthermore, the gas pressure in the atmosphere furnace in steps (b), (c), (d) and (e) is always maintained at a standard atmospheric pressure (i.e., 101 kPa).
[0055] Through the above-mentioned process treatment, a hydrogen embrittlement-resistant strengthening layer with ultra-high austenite stability and controllable ultra-high residual pressure stress can be formed below the surface of austenitic stainless steel parts, thereby greatly reducing the risk of hydrogen embrittlement failure of austenitic stainless steel parts.
[0056] Example 1
[0057] A method for improving the hydrogen embrittlement resistance of austenitic stainless steel comprises the following steps:
[0058] 1. Pre-treatment
[0059] The target parts are standard plate tensile specimens made of 304L austenitic stainless steel, such as Figure 2 As shown, sand it down to 600# with sandpaper.
[0060] First, the target part was immersed in a degreasing agent consisting of a 20% sodium hydroxide solution for 60 seconds, taken out, and washed with water.
[0061] Then, the target part was immersed in a brightener consisting of a mixed solution of 50% hydrochloric acid + 5g / L hexamethyltetramine for 30 seconds, taken out, and washed with water and alcohol in sequence and dried.
[0062] The purpose of the above steps is to remove oil, rust and reduce the thickness of the oxide film on the target parts.
[0063] 2. Activation treatment
[0064] Place the target parts in the atmosphere furnace and close the furnace door. Open the nitrogen valve to introduce nitrogen into the furnace, and at the same time increase the temperature to 250°C at 10°C / min, and keep it warm for 3 hours. When the furnace temperature reaches 250°C, turn off the nitrogen and instead introduce a mixed gas of 3% H2:25% HCl:72% N2 into the atmosphere furnace for 3 hours.
[0065] The process atmosphere-time-temperature flow chart of the above activation treatment step is as follows: Figure 3 The purpose of this step is to deeply remove the oxide film on the surface of the component.
[0066] 3. Carburizing treatment
[0067] The activation gas supply was turned off. The atmosphere furnace temperature was raised to 470°C at a heating rate of 10°C per minute and kept at that temperature for 25 hours, during which nitrogen was introduced until the temperature reached 470°C. When the atmosphere furnace temperature reached 470°C, the nitrogen supply was turned off and a mixed gas of 1% CO2:20% CO:40% H2:39% N2 was introduced for 25 hours.
[0068] The process atmosphere-time-temperature flow chart of the above carburizing treatment step is as follows Figure 3 The purpose of this step is to initially infiltrate a carburized layer with a high carbon mass fraction.
[0069] 4. Carbon diffusion treatment
[0070] Continue to keep the temperature at 470°C for 5 hours, close the mixed gas flow, and only open the nitrogen valve.
[0071] The process atmosphere-time-temperature flow chart of the above carbon diffusion treatment step is as follows: Figure 3 The purpose of this step is to increase the thickness of the carburized layer, reduce the surface brittleness and control the magnitude of the surface residual compressive stress.
[0072] 5. Cooling
[0073] Keep nitrogen flowing and lower the temperature of the atmosphere furnace to 50°C at 10°C / min. When the atmosphere furnace temperature reaches below 50°C, turn off the nitrogen flow and take out the target parts in the atmosphere furnace.
[0074] The process atmosphere-time-temperature flow chart of the above cooling step is as follows: Figure 3 shown.
[0075] 6. Post-processing
[0076] The object parts to be taken out were immersed in a mixed solution of 50% hydrochloric acid aqueous solution and 5g / L hexamethyltetramine for 180 seconds, and then the object parts were taken out and washed with water and alcohol in sequence and dried.
[0077] The purpose of this step is to remove carbon black and oxide layers on the surface of parts.
[0078] Example 2
[0079] A method for improving the hydrogen embrittlement resistance of austenitic stainless steel comprises the following steps:
[0080] 1. Pre-treatment
[0081] The object parts are 10mm×10mm×5mm cubic specimens made of 304L austenitic stainless steel, which are polished to 600# with sandpaper.
[0082] First, immerse the target parts in a degreasing agent composed of 20% sodium hydroxide solution for 10 seconds, take them out, and wash them with water; then immerse the target parts in a brightener composed of a mixed solution of 50% hydrochloric acid + 5g / L hexamethyltetramine for 20 seconds, take them out, and wash them with water and alcohol in turn, and then dry them.
[0083] 2. Activation treatment
[0084] Place the target parts in the atmosphere furnace and close the furnace door. Open the nitrogen valve to introduce nitrogen into the furnace, and at the same time raise the temperature to 300°C at 10°C / min, and keep it warm for 2 hours. When the furnace temperature reaches 300°C, turn off the nitrogen and instead introduce a mixed gas of 1% H2:35% HCl:63% N2 into the atmosphere furnace for 2 hours.
[0085] 3. Carburizing treatment
[0086] Turn off the activation gas supply. Raise the temperature of the atmosphere furnace to 450°C at a heating rate of 10°C per minute and keep it at that temperature for 30 hours. During the heating period, nitrogen is introduced until the temperature reaches 450°C. When the temperature of the atmosphere furnace reaches 450°C, turn off the nitrogen supply and introduce a mixed gas of 0.5% CO2:30% CO:40% H2:29.5% N2 for 30 hours.
[0087] 4. Carbon diffusion treatment
[0088] Continue to keep the temperature at 450°C for 120 hours, close the mixed gas flow, and only open the nitrogen valve.
[0089] 5. Cooling
[0090] Keep nitrogen flowing in and reduce the temperature of the atmosphere furnace to 50° C. at a rate of 10° C. / min. When the temperature of the atmosphere furnace reaches below 50° C., turn off the nitrogen flow and take out the components in the atmosphere furnace.
[0091] 6. Post-processing
[0092] The object parts to be taken out were immersed in a mixed solution of 50% hydrochloric acid aqueous solution and 5g / L hexamethyltetramine for 180 seconds, and then the object parts were taken out and washed with water and alcohol in sequence and dried.
[0093] After the above process parameters are processed, the residual compressive stress on the surface is measured by an X-ray residual stress tester to be 0.3 GPa, which is much lower than 1.5 GPa in Example 1. Figure 6 The hydrogen content test results after hydrogen charging show that the hydrogen barrier effect is reduced by about 30%, which indicates that the high residual compressive stress does play a good hydrogen barrier effect.
[0094] Example 3
[0095] A method for improving the hydrogen embrittlement resistance of austenitic stainless steel comprises the following steps:
[0096] 1. Pre-treatment
[0097] The object parts are 10mm×10mm×5mm cubic specimens made of 316L austenitic stainless steel, which are polished to 150# with sandpaper.
[0098] First, immerse the target parts in a degreasing agent consisting of a 20% sodium hydroxide solution for 10 seconds, take them out, and wash them with water; then immerse the target parts in a brightener consisting of a mixed solution of 50% hydrochloric acid + 5g / L hexamethyltetramine for 60 seconds, take them out, and wash them with water and alcohol in turn, and then dry them.
[0099] 2. Activation treatment
[0100] Place the target parts in the atmosphere furnace and close the furnace door. Open the nitrogen valve to introduce nitrogen into the furnace, and at the same time increase the temperature to 350℃ at 10℃ / min and keep it warm for 2 hours. When the furnace temperature reaches 350℃, turn off the nitrogen and introduce a mixed gas of 3% H2:30% HCl:67% N2 into the atmosphere furnace for 2 hours.
[0101] 3. Carburizing treatment
[0102] Turn off the activation gas supply. Raise the temperature of the atmosphere furnace to 470°C at a heating rate of 10°C per minute and keep it at that temperature for 35 hours. During the heating period, introduce nitrogen until the temperature reaches 470°C. When the temperature of the atmosphere furnace reaches 470°C, turn off the nitrogen supply and introduce a mixed gas of 0.5% CO2:30% CO:40% H2:29.5% N2 for 35 hours.
[0103] 4. Carbon diffusion treatment
[0104] Continue to keep the temperature at 450°C for 5 hours, close the mixed gas flow, and only open the nitrogen valve.
[0105] 5. Cooling
[0106] Keep nitrogen flowing and lower the temperature of the atmosphere furnace to 50°C at 10°C / min. When the atmosphere furnace temperature reaches below 50°C, turn off the nitrogen flow and take out the target parts in the atmosphere furnace.
[0107] 6. Post-processing
[0108] The object parts to be taken out were immersed in a mixed solution of 50% hydrochloric acid aqueous solution and 5g / L hexamethyltetramine for 180 seconds, and then the object parts were taken out and washed with water and alcohol in sequence and dried.
[0109] After the above process parameters are processed, the residual compressive stress on the surface is measured by X-ray residual stress tester to be 2.2 GPa, and the thickness of the carburized layer is 36 μm.
[0110] Comparative Example 1
[0111] The comparative example is the same object component as that of Example 1 without any treatment.
[0112] The object parts treated in Example 1, Example 2 and Comparative Example 1 were used as test samples, wherein in the comparative figures, Example 1 was marked as treated, Example 2 was marked as low residual stress carburizing, and Comparative Example 1 was marked as untreated.
[0113] The following describes the test results of the target parts after the above steps.
[0114] The cross section of the object part of the austenitic stainless steel treated in Example 1 was cut to obtain the metallographic structure, such as Figure 4 As shown, it can be seen that there is a carburized layer below the surface of the object component.
[0115] The residual stress on the surface of the carburized layer of the austenitic stainless steel object parts treated in Example 1 was tested by an X-ray residual stress tester. Figure 5 As shown in Figure 1, the carburized layer has high residual compressive stress, and the residual compressive stress on the surface is as high as 1.5 GPa. Such high residual compressive stress can effectively hinder the penetration of hydrogen.
[0116] Use a hydrogen analyzer to test the average hydrogen content on the surface of the target parts, such as Figure 6 As shown, the hydrogen content of the object parts treated in Example 1 after hydrogen filling is only about 33% of the hydrogen content of the object parts of the untreated comparative example 1 after hydrogen filling, which fully proves that the object parts treated by the present invention can significantly reduce the penetration of hydrogen.
[0117] Figure 7 The X-ray phase composition results of the object parts treated in Example 1 and the untreated object parts of Comparative Example 1 before and after hydrogen filling are given. It can be seen that the object parts treated in Example 1 did not undergo phase change after hydrogen filling, proving that the stability of austenite after treatment with the anti-hydrogen embrittlement surface treatment process of the present invention is greatly improved.
[0118] Figure 8 The engineering stress-engineering strain curves of the tensile test of the object parts treated in Example 1 and the untreated object parts of Comparative Example 1 before and after hydrogen filling are given. The hydrogen embrittlement sensitivity is calculated by the loss percentage of the elongation after hydrogen filling compared with the elongation without hydrogen filling. It can be seen that the hydrogen embrittlement sensitivity of the object parts treated by the anti-hydrogen embrittlement surface treatment process of the present invention is reduced by 50%. It can be seen that the anti-hydrogen embrittlement surface treatment process of the present invention can greatly improve the hydrogen embrittlement resistance of austenitic stainless steel parts.
[0119] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for improving the hydrogen embrittlement resistance of austenitic stainless steel, characterized in that: The following steps are involved: (a) degreasing austenitic stainless steel with a degreasing agent and then brightening it with a brightening agent; (b) placing the brightened austenitic stainless steel in an atmosphere furnace, introducing nitrogen into the atmosphere furnace while raising the temperature to a first preset temperature, maintaining the temperature at the first preset temperature, performing an activation treatment, and introducing a first mixed gas into the atmosphere furnace during the first heat preservation treatment; (c) introducing nitrogen into the atmosphere furnace and simultaneously raising the temperature to a second preset temperature; when the temperature of the atmosphere furnace reaches the second preset temperature, introducing a second mixed gas into the atmosphere furnace and maintaining the temperature at the second preset temperature to perform carburizing treatment; (d) after the carburizing treatment is completed, nitrogen is introduced into the atmosphere furnace, and the temperature is maintained at the second preset temperature to perform carbon diffusion treatment; (e) After the carbon diffusion treatment is completed, nitrogen is kept flowing to reduce the temperature; (f) brightening the cooled austenitic stainless steel in the brightening agent.
2. The method according to claim 1, characterized in that The degreasing agent is a sodium hydroxide solution with a mass fraction of 20%, and the brightening agent is a mixed solution of 50% volume concentration hydrochloric acid and 5g / L hexamethyltetramine.
3. The method according to claim 1, characterized in that In step (b), the first preset temperature is 200-350° C., and the heating rate to the first preset temperature is 10° C. / min.
4. The method according to claim 1, characterized in that: In step (b), the heating rate for heating to the first preset temperature is 10° C. / min.
5. The method according to claim 1, characterized in that In step (b), the composition of the first mixed gas is (2-10%) H2: (25-60%) HCl: (73-30%) N2 by volume.
6. The method according to claim 1, characterized in that In step (c), the second preset temperature is 400-550° C., and the heating rate to the second preset temperature is 10° C. / min.
7. The method according to claim 1, characterized in that In step (c), the heating rate for heating to the second preset temperature is 10° C. / min.
8. The method according to claim 1, characterized in that In step (c), the composition of the second mixed gas is (0.1-3%) CO2: (15-35%) CO: (20-40%) H2: (64.9-22%) N2 by volume.
9. Austenitic stainless steel treated by the method according to any one of claims 1 to 8.
10. Use of the method for improving the hydrogen embrittlement resistance of austenitic stainless steel according to any one of claims 1 to 8.