Short-process low-cost preparation method of large-size molybdenum tube target material
Through the process of combining powder metallurgy and cold isostatic pressing technology, the problem of high cost of molybdenum target preparation is solved, and the low cost preparation of large-size molybdenum tube targets is realized, which improves the density and strength of the material and reduces the equipment. invest.
Patent Information
- Application Number
- CN202411131441.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-18
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the production process of molybdenum targets is high and the equipment investment is large, making it difficult to achieve short-process and low-cost preparation of large-size molybdenum tube targets.
The molybdenum pipe targets are prepared by powder metallurgy. The mold is loaded through loose loading and vibration-shaping, and combined with the cold isostatic pressing technology of direct boosting and step pressure relief, followed by sintering, hollow forging and machining to shorten the process flow and reduce production costs.
The density and strength of molybdenum tube targets are improved, production costs are reduced, workpiece cracking is avoided, and the purity and density of molybdenum tube targets are close to those of foreign top companies, and the equipment investment is low.
Smart Images

Figure CN119020737A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of molybdenum target material preparation, in particular to a short-process and low-cost preparation method for large-size molybdenum tube targets. Background Art
[0002] As the raw material for preparing thin films by magnetron sputtering, molybdenum targets are emerging, high-end materials developed in response to market needs. Molybdenum targets are widely used in electronic components and electronic products, such as thin film semiconductor tubes-liquid crystal displays (TFT-LCD), plasma display screens, thin film solar cells, sensors, semiconductor devices, etc.
[0003] As the size of glass substrates in TFT-LCD panel production lines increases, the specifications of molybdenum sputtering targets are becoming increasingly demanding. Molybdenum sputtering targets of the G5, G5.5, G6, G7.5, and G8.5 generations are all used in a splicing manner, which increases the processing and manufacturing costs of molybdenum targets. In addition, different targets have certain differences in organizational structure, which to a certain extent affects the effect of sputtering coating, and the overall target is conducive to solving the problem of uniformity of the film layer. Therefore, the breakthrough in large-size molybdenum target manufacturing technology is to meet the electronics industry's demand for large panels.
[0004] At present, the preparation methods of molybdenum targets at home and abroad all use molybdenum powder as raw material, and adopt powder metallurgy + hot deformation densification + machining process. The top foreign molybdenum target manufacturers Plansee in Austria and H.C Starck in Germany use extrusion process to manufacture tube targets. The prepared tube targets are up to 4000mm in length, with a density of more than 99% and a purity of 99.97%. However, the investment in equipment for manufacturing molybdenum tube targets using extrusion process is large. A 7,000-ton extrusion production line requires about 600 million yuan, and patent protection has been applied for, with technology monopoly. How to provide a short-process and low-cost process method to prepare large-sized molybdenum targets is an urgent problem to be solved at this stage. Summary of the invention
[0005] The present invention aims to provide a short-process and low-cost preparation method for large-size molybdenum tube targets, so as to prepare large-size molybdenum tube targets by a method different from the prior art concept.
[0006] In order to solve the above technical problems, the specific scheme adopted by the present invention is: a short-process and low-cost preparation method for large-size molybdenum tube targets, wherein the screened high-purity molybdenum powder is loaded into a mold to obtain a molybdenum tube blank, and then the molybdenum tube blank is sequentially subjected to cold isostatic pressing, sintering, hollow forging and machining to obtain the molybdenum tube target, wherein the cold isostatic pressing is to first directly increase the pressing pressure to a target value, and then use a staged pressure relief method to press the molybdenum tube blank.
[0007] As a further optimization of the above technical solution: the target value is 180-220Mpa.
[0008] As a further optimization of the above technical solution: the stage pressure relief is a three-stage pressure relief.
[0009] As a further optimization of the above technical solution: the three-stage pressure relief is specifically:
[0010] Pressing pressure 180-220MPa, holding time 8-10min;
[0011] The first-stage pressure relief pressure is 140-170MPa, and the first-stage pressure relief holding time is 2-3min;
[0012] Secondary pressure relief pressure is 100-130MPa, and the secondary pressure relief holding time is 2-3min;
[0013] The third-level pressure relief pressure is 60-90MPa, and the third-level pressure relief holding time is 2-3min.
[0014] As a further optimization of the above technical solution: the forging temperature of the hollow forging is 1200-1300°C.
[0015] As a further optimization of the above technical solution: the hollow forging includes two heating forgings.
[0016] As a further optimization of the above technical solution: the sintering adopts staged heating, heating to 200-600℃, keeping warm for 1-3h, heating to 600-1200℃, keeping warm for 1-3h, heating to 1500-1800℃, keeping warm for 2-6h, heating to 2100-2250℃, keeping warm for 6-8h.
[0017] As a further optimization of the above technical solution: after the sintering is completed, natural cooling is adopted to reduce the molybdenum tube blank to room temperature before hollow forging.
[0018] As a further optimization of the above technical solution: the mold installation adopts a combination of loose installation and vibration compaction.
[0019] As a further optimization of the above technical solution: the purity of the high-purity molybdenum powder is ≥99.9wt%.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention prepares molybdenum tube target materials by powder metallurgy, adopts loose packing + vibration compaction mode to load molybdenum tube blanks, and adopts cold isostatic pressing combining direct pressure increase with step pressure relief. Direct pressure increase is adopted to improve the density and strength of the blank through high pressure action. In the process of pressure relief, sufficient time for releasing the internal stress of the pressing is given in stages to avoid the cracking phenomenon caused by the rapid release of the internal stress of the workpiece during the pressure relief process.
[0022] The preparation method of the present invention shortens the traditional preparation process, reduces the requirements of the molybdenum rotary sputtering tube target on equipment, and reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic flow chart of the preparation method of the present invention;
[0024] Figure 2 Microstructure diagram of molybdenum tube target prepared for hollow forging.
[0025] Figure 3 XRD pattern of molybdenum tube target prepared for hollow forging;
[0026] Figure 4 This is the microstructure diagram of the molybdenum tube target prepared by hollow forging in the prior art. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. The parts that are not described and disclosed in detail in the following embodiments of the present invention, such as the method of coating the inner hole of the tubular molybdenum target, should be understood as the prior art known or should be known to those skilled in the art.
[0028] The present invention discloses a short-process and low-cost preparation method for a large-size molybdenum tube target material. The selected high-purity molybdenum powder is loaded into a mold to obtain a molybdenum tube blank, and then the molybdenum tube blank is sequentially subjected to cold isostatic pressing, sintering, hollow forging and machining to obtain the molybdenum tube target material. The preparation process is as follows: Figure 1 shown.
[0029] Specifically, the purity of high-purity molybdenum powder is ≥99.9wt%. The high-purity molybdenum powder is loaded into the mold by loose packing + vibration compaction. Loose packing refers to the process of loosely filling the screened high-purity molybdenum powder into the mold. In this process, the powder particles mainly rely on their own gravity and mutual forces (such as van der Waals force, electrostatic force, etc.) to naturally accumulate. After loading into the mold, the powder particles are further tightly arranged by external vibration, thereby increasing the filling density of the molybdenum powder in the mold. The specific method of applying vibration is a prior art and will not be repeated here.
[0030] Cold isostatic pressing is to first increase the pressing pressure to the target value, and then use staged pressure relief to press the molybdenum tube billet. The target value of the pressing pressure is 180-220Mpa, and the staged pressure relief is three-level pressure relief. The three-level pressure relief is specifically as follows: pressing pressure 180-220MPa, holding time 8-10min; first-level pressure relief pressure 140-170MPa, first-level pressure relief holding time 2-3min; second-level pressure relief pressure 100-130MPa, second-level pressure relief holding time 2-3min; third-level pressure relief pressure 60-90MPa, third-level pressure relief holding time 2-3min, and then naturally release the pressure to normal pressure after the third-level pressure relief is completed.
[0031] In this embodiment, the molybdenum tube blank pressing process is shown in Table 1 below: Table 1 Molybdenum tube blank pressing process
[0032] Medium frequency induction sintering is adopted for sintering, and the heating process in the sintering stage adopts stage heating, heating to 200-600℃, keeping warm for 1-3h, heating to 600-1200℃, keeping warm for 1-3h, heating to 1500-1800℃, keeping warm for 2-6h, heating to 2100-2250℃, keeping warm for 6-8h. In this embodiment, the stage heating is specifically as follows: first heating to 200℃, keeping warm for 3h, then heating to 700℃, keeping warm for 3h, then heating to 1600℃, keeping warm for 4h, and finally heating to 2150℃, keeping warm for 8h. After sintering is completed, the temperature is cooled by natural cooling, and the molybdenum tube blank is cooled to room temperature before hollow forging.
[0033] The forging temperature of hollow forging is 1200-1300°C. Hollow forging includes two heating forgings. In this embodiment, the molybdenum tube blank is first heated to 1250°C and kept at 60°C for the first forging, and then returned to the furnace and continued to be heated to 1250°C and kept at 60°C for the second forging. After the hollow forging is completed, the tube blank is heat treated at a temperature of 1200°C, and then machined to obtain a tubular molybdenum target. Machining includes cutting, milling machine processing and grinding machine processing. The inner hole coating of the tubular molybdenum target is a molybdenum tube target.
[0034] The molybdenum tube target prepared by the present invention is compared with the prior art, and the results are shown in Table 2 below.
[0035] Table 2 Comparison with domestic and foreign technologies
[0036] It can be seen from Table 2 that the commercially available molybdenum tube target material (i.e., the molybdenum tube target material prepared by the technology of other domestic companies) has a purity ≥99.95%, a density ≥98.5%, and a grain size ≤100μm. The purity and density of the molybdenum tube target material prepared by the present invention are greater than those of the commercially available products, and the grain size is smaller than that of the commercially available products; the molybdenum tube target material prepared by the present invention is closer to that prepared by foreign companies in purity, density and grain size, but the foreign companies use extrusion densification, which requires large equipment investment and high cost, while the present invention uses forging densification, and the existing forging furnace can be used to control the forging time and temperature, with less equipment investment and lower cost.
[0001] The molybdenum tube target prepared by the present invention and the molybdenum tube target prepared by Starkey of Germany were tested. By comparing the two, it can be seen that the density of the tube target prepared by the present invention is slightly lower, and the density of the molybdenum tube target is 10.21 g / cm3 The density of the extruded molybdenum tube target of Starck, Germany, is close to the theoretical density of 10.22g / cm 3 .
[0002] Figure 2 This is the microstructure diagram of the molybdenum tube target prepared by the present invention. Figure 3 This is the XRD pattern of the molybdenum tube target prepared by the present invention. Figure 4 It is a molybdenum tube target prepared by the German company Stark through an extrusion molding process. It can be seen that the molybdenum tube target prepared by the present invention has a full-phase microstructure that is quasi-equiaxed, and the main crystal orientation is the close-packed (110) crystal plane, which is most easily sputtered, and the extrusion molding product has obvious directionality.
[0003] The present invention prepares molybdenum tube target materials by powder metallurgy + hollow forging densification, adopts loose loading + vibration compaction to load the molybdenum tube blank, and adopts cold isostatic pressing combining direct pressure increase with step pressure relief, so as to solve the problems that large-size hollow tube targets are prone to large shape and position tolerances, cracking, delamination, irregular formation and the like during powder loading technology and pressing process, and adopts direct pressure increase to improve the density and strength of the blank through high pressure. Compared with plate-shaped targets, the area of tubular targets is relatively small, and direct pressure increase can further shorten the processing time. In the process of pressure relief, sufficient time for releasing the internal stress of the pressing is given in stages to avoid the cracking phenomenon caused by the rapid release of the internal stress of the workpiece during the pressure relief process.
[0004] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A short-process and low-cost preparation method for large-size molybdenum tube targets, characterized in that: The screened high-purity molybdenum powder is filled into a mold to obtain a molybdenum tube blank, and then the molybdenum tube blank is subjected to cold isostatic pressing, sintering, hollow forging and machining in sequence to obtain the molybdenum tube target material, wherein the cold isostatic pressing is to first directly increase the pressing pressure to a target value, and then use a staged pressure relief method to press the molybdenum tube blank.
2. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 1, characterized in that: The target value is 180-220Mpa.
3. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 2, characterized in that: The stage pressure relief described is three-stage pressure relief.
4. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 3, characterized in that: The three-stage pressure relief is specifically: Pressing pressure 180-220MPa, holding time 8-10min; The first-stage pressure relief pressure is 140-170MPa, and the first-stage pressure relief holding time is 2-3min; Secondary pressure relief pressure is 100-130MPa, and the secondary pressure relief holding time is 2-3min; The third-level pressure relief pressure is 60-90MPa, and the third-level pressure relief holding time is 2-3min.
5. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 1, characterized in that: The forging temperature of the hollow forging is 1200-1300°C.
6. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 1, characterized in that: The hollow forging includes two heating forgings.
7. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 1, characterized in that: The sintering adopts stage heating, heating to 200-600°C, keeping warm for 1-3h, heating to 600-1200°C, keeping warm for 1-3h, heating to 1500-1800°C, keeping warm for 2-6h, heating to 2100-2250°C, keeping warm for 6-8h.
8. The short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 1 is characterized in that: After the sintering is completed, the molybdenum tube blank is cooled to room temperature by natural cooling before hollow forging.
9. A short-process and low-cost method for preparing large-size molybdenum tube targets according to claim 1, characterized in that: The mold installation adopts a combination of loose installation and vibration compaction.
10. A short-process and low-cost preparation method for large-size molybdenum tube targets according to claim 1, characterized in that: The purity of the high-purity molybdenum powder is ≥99.9wt%.