Preparation method of high-entropy alloy wear-resistant coating

By combining high-entropy alloy with traditional solder, a high-entropy alloy wear-resistant coating was prepared, which solved the problems of brazing brittleness and cost, and achieved high binding strength and wear resistance. However, due to the uncertainty of the high-entropy effect, it was found that the high-entropy effect was uncertain. performance improvement is difficult to predict.

CN119020772APending Publication Date: 2024-11-26ANHUI POLYTECHNIC UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410729904.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing brazing coating technology, the problems of low brittle phase, matrix hardness, poor corrosion resistance and high cost of the brazing material lead to poor coating performance stability and high production costs.

Method used

A high-entropy alloy is combined with traditional brazing materials, and a high-entropy alloy wear-resistant coating is prepared by mixing copper or nickel-based brazing materials with FeCoCrNiCu high-entropy alloy powder, adding WC powder, and a high-entropy alloy wear-resistant coating is prepared through vacuum brazing technology.

Benefits of technology

Improves the bond strength and thickness controllability of the coating and matrix, reduces the brittle phase and improves the content and wear resistance of hard particles, reduces production costs, and improves performance through high entropy effect, but due to the high entropy effect The uncertainty of performance improvement is difficult to predict.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020772A_ABST
    Figure CN119020772A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wear-resistant coating preparation, in particular to a high-entropy alloy wear-resistant coating preparation method which comprises the steps that copper or nickel-based brazing filler metal powder and FeCoCrNiCu high-entropy alloy powder are fully mixed and heated and dried under inert gas protection to form first mixed powder; the high-entropy alloy wear-resistant coating is prepared by the following steps: mixing the first mixed powder with ethanol, then adding WC powder and mixing to form second mixed powder, then stirring and mixing the second mixed powder and ethanol to form pasty mixed powder, finally coating a substrate with the pasty mixed powder, and performing vacuum brazing coating to obtain the high-entropy alloy wear-resistant coating. The coating prepared by the method is high in bonding strength with a matrix and controllable in thickness; compared with a traditional brazed coating, the coating prepared through the method is few in brittle phase, high in hard particle content, high in abrasion resistance, easy to operate and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wear-resistant coating preparation, and in particular to a method for preparing a high-entropy alloy wear-resistant coating. Background Art

[0002] At present, the coating preparation technologies commonly used in engineering include electroplating and chemical plating, thermal spraying, physical vapor deposition, chemical vapor deposition, surfacing, laser cladding, etc. However, these methods have problems such as low wear-resistant layer thickness, poor bonding with the substrate, high production cost, large environmental pollution, serious damage to the parent material, and low production efficiency. For example, electroplating and chemical plating methods cause serious environmental pollution, thermal spray coatings have high porosity and low bonding strength with the substrate, surfacing causes serious thermal damage to the parent material, and the coating prepared by vapor deposition is thin and has low production efficiency. Laser cladding has the disadvantage of easy cracking for a type of coating with high carbon equivalent and containing ceramic reinforcement phase. Relatively speaking, the coating prepared by brazing coating technology has the advantages of high bonding strength with the substrate, small thermal impact on the substrate, high hard phase content, good density, and easy control of coating thickness, which is particularly suitable for long-term and high-load service conditions. Especially in the fields of aerospace, agricultural machinery, oil drilling, mining, etc., it has broad application prospects.

[0003] In the existing brazing coating technology, nickel-based, iron-based, copper-based and other brazing materials are generally used as the base material, and hard particles such as WC, Cr3C2, SiC, diamond, etc. are added in a ratio of 30-50wt.%, and wear-resistant coatings are obtained by flame brazing, induction brazing, vacuum brazing and other technologies. However, nickel-based brazing materials have poor wettability to hard particles, and copper-based and iron-based brazing materials are soft and have poor wear resistance. The brittle phase between the brazing material and the hard particles will cause many coating defects and poor performance stability. Commonly used brazing materials have the disadvantages of significant brittle phase (nickel-based brazing material), low base hardness (copper-based and iron-based brazing materials), poor corrosion resistance (copper-based and iron-based brazing materials), and high cost (silver-based brazing material). Therefore, it is necessary to develop a new base brazing material for brazing coating technology.

[0004] Relatively speaking, high entropy alloys have higher hardness and wear resistance under the lattice distortion effect, better wettability and low melting point potential under the cocktail effect, can effectively hinder the growth of some brittle phases under the high entropy effect, and have a higher service temperature under the hysteresis diffusion effect. Using it as a filler solder in the brazing process is expected to break the performance bottleneck of traditional brazing coatings. However, as a new type of brazing material, high entropy alloys have been found to be inferior in wettability and fluidity to traditional brazing materials in application research. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a method for preparing a high entropy alloy wear-resistant coating, combining traditional brazing filler metal with high entropy brazing filler metal to develop a new type of brazing filler metal that has both the excellent mechanical properties of high entropy brazing filler metal and the excellent wettability of traditional brazing filler metal, and to prepare a wear-resistant coating suitable for long-term high-load service using brazing coating technology.

[0006] Based on the above purpose, the present invention provides a preparation method of a high entropy alloy wear-resistant coating, the preparation method comprising: firstly fully mixing a copper or nickel-based solder powder and a FeCoCrNiCu high entropy alloy powder, heating and drying the mixture under inert gas protection to form a first mixed powder, then adding WC powder and mixing the mixture to form a second mixed powder, then stirring and mixing the second mixed powder with ethanol to form a paste-like mixed powder, and finally coating the paste-like mixed powder on a substrate, and obtaining a high entropy alloy wear-resistant coating after vacuum brazing.

[0007] Preferably, the nickel-based solder powder is BNi7 powder, and the weight percentage of the BNi7 powder in the first mixed powder is 10-15%.

[0008] Preferably, the BNi7 powder is nearly spherical and has a particle size of 350-450 mesh, preferably 400 mesh.

[0009] Optionally, the weight percentage of the WC powder in the second mixed powder is 10-30%, preferably 20-30%.

[0010] Preferably, in the process of forming the first mixed powder, the time for sufficient mixing is 2 to 5 hours; the inert gas is argon or nitrogen, and the mixture is heated to 100 to 200° C. for drying.

[0011] Preferably, the FeCoCrNiCu high entropy alloy powder is a spherical powder with a particle size of 50 to 100 μm.

[0012] Preferably, the coating has a thickness of 0.5 to 1.5 mm.

[0013] Preferably, the process parameters of the vacuum brazing are: the vacuum degree reaches 5×10 -3 Pa, heat to 1150-1180°C at a rate of 5-10°C / min, keep warm for 30-60min, cool to 500°C at a rate of 3-5°C / min, and then cool to room temperature with the furnace.

[0014] Preferably, after the paste-like mixed powder is coated on the substrate, it is leveled with a scraper and then vacuum brazing is performed.

[0015] Preferably, the substrate comprises a steel substrate, and the substrate is ground, polished and cleaned before coating.

[0016] The beneficial effects of the present invention are as follows: compared with the coating prepared by the conventional process, the coating prepared by the method of the present invention has high bonding strength with the substrate and controllable thickness; compared with the conventional brazing coating, the coating prepared by the method of the present invention has less brittle phase, high content of hard particles, strong wear resistance, simple operation and low cost. In addition, due to the uncertainty of the high entropy effect, the improvement in the performance of the coating prepared by the brazing material proposed by the present invention cannot be predicted in advance in theory. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The cross-sectional SEM morphology images of the coatings of Examples 1-3 and Comparative Example 1 of the present invention; wherein (a) Example 1, (b) Example 2, (c) Comparative Example 1, (d) Example 3;

[0019] Figure 2 Schematic diagram of coating bonding strength and wear amount of Examples 1-3 of the present invention and Comparative Example 1;

[0020] Figure 3 The three-dimensional reconstructed wear morphology images of Examples 1-3 and Comparative Example 1 of the present invention; wherein, (a) Example 1, (b) Example 2, (c) Comparative Example 1, (d) Example 3;

[0021] Figure 4 The cross-sectional morphology of the FeCoCrNiCu coating under different brazing process parameters of the present invention;

[0022] Figure 5 The cross-sectional morphology of FeCoCrNiCu brazing coating with different BNi7 additions;

[0023] Figure 6 The porosity statistics of the cross section of FeCoCrNiCu brazing coating with different BNi7 additions;

[0024] Figure 7 Cross-sectional morphology of BNi7-FeCoCrNiCu coatings with different WC contents. DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0026] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components.

[0027] The present invention relates to a method for preparing a high entropy alloy wear-resistant coating, comprising the following steps:

[0028] (1) Selection and mixing of powders: FeCoCrNiCu high entropy alloy spherical powder with an atomic ratio of Fe, Co, Cr, Ni, and Cu of 1:1:1:1:1 is used, and the particle size is 50-100 μm. The BNi7 solder used is nearly spherical with a particle size of about 400 mesh. The WC powder is irregular with a particle size of 200 mesh. First, weigh BNi7 powder and FeCoCrNiCu powder, wherein the BNi7 powder accounts for 10-15wt.%. Subsequently, the two powders are placed in a three-dimensional powder mixer, and after being fully mixed for 2-5 hours, they are heated to 100-200°C and dried for 2 hours under the protection of an inert gas (argon or nitrogen) to form a BiN7-FeCoCrNiCu mixed powder. Finally, WC powder is added and mixed in the above manner, and the WC powder accounts for 10-30wt.% of the BiN7-FeCoCrNiCu mixed powder, and finally a WC-BNi7-FeCoCrNiCu mixed powder is formed.

[0029] (2) Pre-setting of powder: Stir and mix appropriate amount of alcohol and WC-BNi7-FeCoCrNiCu mixed powder to form slurry. Grind, polish and clean the brazing-coated steel substrate (45 steel, Q235 steel, 304 stainless steel, etc.), and evenly coat the surface with paste WC-BNi7-FeCoCrNiCu mixed powder, with a coating thickness of about 0.5 to 1.5 mm. After coating, use a scraper to flatten the surface.

[0030] (3) Vacuum brazing: The plate coated with WC-BNi7-FeCoCrNiCu mixed powder is placed in a vacuum brazing furnace with a vacuum degree of 5×10 -3 Pa, heat to 1150-1180°C at a rate of 5-10°C / min, keep warm for 30-60min, cool to 500°C at a rate of 3-5°C / min, and then cool to room temperature with the furnace.

[0031] Example 1

[0032] WC was added according to 20wt.% of the weight of BNi7-FeCoCrNiCu powder (BNi7:FeCoCrNiCu=12.5:87.5). The specific preparation method is as follows:

[0033] (1) Selection and mixing of powders: FeCoCrNiCu high entropy alloy spherical powder with an atomic ratio of Fe, Co, Cr, Ni, and Cu of 1:1:1:1:1 is used, and the particle size is 50-100μm. The BNi7 solder used is nearly spherical with a particle size of about 400 mesh. The WC powder is irregular with a particle size of 200 mesh. First, weigh BNi7 powder and FeCoCrNiCu powder, of which BNi7 powder accounts for 12.5wt.%. Subsequently, the two powders are placed in a three-dimensional powder mixer, and after being fully mixed for 2 hours, they are heated to 200℃ and dried for 2h under the protection of inert gas nitrogen to form BiN7-FeCoCrNiCu mixed powder. Finally, WC powder is added and mixed in the above manner, and the WC powder accounts for 20wt.% of the BiN7-FeCoCrNiCu mixed powder, and finally a WC-BNi7-FeCoCrNiCu mixed powder is formed.

[0034] (2) Pre-setting of powder: Absolute alcohol and WC-BNi7-FeCoCrNiCu powder were fully stirred and mixed in a ratio of 1:10 to form a slurry. 304 stainless steel was used as the substrate. The brazed steel substrate was ground, polished and cleaned, and then the paste WC-BNi7-FeCoCrNiCu mixed powder was evenly coated on the surface with a coating thickness of about 1.5 mm. After coating, the surface was flattened with a scraper.

[0035] (3) Vacuum brazing: The plate coated with WC-BNi7-FeCoCrNiCu mixed powder is placed in a vacuum brazing furnace with a vacuum degree of 5×10 -3 Pa, heat to 1160 °C at a rate of 10 °C / min, keep warm for 60 min, cool to 500 °C at a rate of 5 °C / min and then cool to room temperature with the furnace.

[0036] Obtain high coating density (see Figure 1 ), shear strength is 297.41MPa, wear volume is 0.44mm3 (see Figure 2 ), only produces wear marks on the surface (see Figure 3 ).

[0037] Example 2

[0038] WC was added according to 30wt.% of the weight of BNi7-FeCoCrNiCu powder (BNi7:FeCoCrNiCu=12.5:87.5). The specific preparation method is as follows:

[0039] (1) Selection and mixing of powders: FeCoCrNiCu high entropy alloy spherical powder with an atomic ratio of Fe, Co, Cr, Ni, and Cu of 1:1:1:1:1 is used, and the particle size is 50-100μm. The BNi7 solder used is nearly spherical with a particle size of about 400 mesh. The WC powder is irregular with a particle size of 200 mesh. First, weigh BNi7 powder and FeCoCrNiCu powder, of which BNi7 powder accounts for 12.5wt.%. Subsequently, the two powders are placed in a three-dimensional powder mixer, and after being fully mixed for 2 hours, they are heated to 200℃ and dried for 2h under the protection of inert gas nitrogen to form BiN7-FeCoCrNiCu mixed powder. Finally, WC powder is added and mixed in the above manner, and the WC powder accounts for 20wt.% of the BiN7-FeCoCrNiCu mixed powder, and finally a WC-BNi7-FeCoCrNiCu mixed powder is formed.

[0040] (2) Pre-setting of powder: Absolute alcohol and WC-BNi7-FeCoCrNiCu powder were fully stirred and mixed in a ratio of 1:10 to form a slurry. 304 stainless steel was used as the substrate. The brazed steel substrate was ground, polished and cleaned, and then the paste WC-BNi7-FeCoCrNiCu mixed powder was evenly coated on the surface with a coating thickness of about 1.5 mm. After coating, the surface was flattened with a scraper.

[0041] (3) Vacuum brazing: The plate coated with WC-BNi7-FeCoCrNiCu mixed powder is placed in a vacuum brazing furnace with a vacuum degree of 5×10 -3 Pa, heat to 1160 °C at a rate of 10 °C / min, keep warm for 60 min, cool to 500 °C at a rate of 5 °C / min and then cool to room temperature with the furnace.

[0042] Obtain coating defects (see Figure 1 ), the shear strength decreased to 176.74MPa, and the wear volume was very small (see Figure 2 ), only a few scratches are produced on the surface (see Figure 3 ).

[0043] Example 3

[0044] Cu-FeCoCrNiCu mixed powder is used as brazing filler metal, and WC is added as reinforcing particle powder. A WC-Cu-FeCoCrNiCu brazing coating can be obtained by vacuum brazing. The coating has good wear resistance, but the wear resistance is relatively low compared with the coatings obtained in Example 1 and Example 2.

[0045] In this embodiment, WC is added in a proportion of 20wt.% of the weight of Cu-FeCoCrNiCu powder (Cu:FeCoCrNiCu=12.5:87.5). The specific technical scheme is as follows:

[0046] (1) Selection and mixing of powders: FeCoCrNiCu high entropy alloy spherical powder with an atomic ratio of Fe, Co, Cr, Ni, and Cu of 1:1:1:1:1 is used, and the particle size is 50-100μm. The Cu solder used is nearly spherical and has a particle size of about 400 mesh. The WC powder is irregular and has a particle size of 200 mesh. First, weigh Cu powder and FeCoCrNiCu powder, of which the Cu powder accounts for 12.5wt.%. Subsequently, the two powders are placed in a three-dimensional powder mixer, and after being fully mixed for 2 hours, they are heated to 200℃ and dried for 2h under the protection of inert gas nitrogen to form a Cu-FeCoCrNiCu mixed powder. Finally, WC powder is added and mixed in the above manner, and the WC powder accounts for 20wt.% of the Cu-FeCoCrNiCu mixed powder, and finally a WC-Cu-FeCoCrNiCu mixed powder is formed.

[0047] (2) Pre-setting of powder: Absolute alcohol and WC-Cu-FeCoCrNiCu powder are fully stirred and mixed in a ratio of 1:10 to form a paste. Then, the brazed 304 stainless steel substrate (after grinding, polishing and cleaning) is evenly coated with the paste WC-Cu-FeCoCrNiCu mixed powder on the surface, with a coating thickness of about 1.5 mm. After coating, the surface is flattened with a scraper.

[0048] (3) Vacuum brazing: The plate coated with WC-Cu-FeCoCrNiCu mixed powder is placed in a vacuum brazing furnace with a vacuum degree of 5×10 -3 After Pa, it was heated to 1160 °C at a rate of 10 °C / min, kept at that temperature for 60 min, cooled to 500 °C at a rate of 5 °C / min, and then cooled to room temperature in the furnace.

[0049] The shear strength of the coating was slightly reduced, and the shear strength was 269.34MPa (see Figure 2 ), the wear volume is 0.55mm3 (see Figure 2 ), only produces wear marks on the surface (see Figure 3 ).

[0050] Comparative Example 1

[0051] BNi7 was added at a ratio of 12.5wt% of the FeCoCrNiCu powder, and no WC was added. 304 stainless steel was used as the substrate and brazed at 1160℃ for 60min. The obtained coating had a high density (see Figure 1), the shear strength is as high as 331.57MPa, and the wear volume is 2.57mm3 (see Figure 2 ), there are wear marks of a certain depth (see Figure 4 ).

[0052] The coating was prepared using different brazing process parameters. The cross-sectional morphology of the FeCoCrNiCu coating is shown in Figure 2. Figure 4 The results show that: (1) the FeCoCrNiCu coating has good wetting on the stainless steel substrate and excellent metallurgical bonding; (2) it is difficult to completely eliminate the holes in the FeCoCrNiCu coating by simply adjusting the welding process parameters.

[0053] Study on FeCoCrNiCu brazing coating with different BNi7 additions

[0054] Figure 5 The cross-sectional morphology of FeCoCrNiCu brazing coating with different BNi7 additions; Figure 6 The porosity statistics of the cross-section of FeCoCrNiCu brazing coatings with different BNi7 additions were conducted; the results showed that the porosity in the high entropy coating can be improved by adding an appropriate proportion of traditional BNi7 brazing filler metal, and the optimal addition ratio is 12.5wt.%.

[0055] Preparation of BNi7-FeCoCrNiCu coating with different WC contents

[0056] like Figure 7 As shown in the figure, it can be seen from the cross-sectional morphology of BNi7-FeCoCrNiCu coatings with different WC contents that as a wear-resistant coating, the proportion of added WC is preferably controlled between 20-30wt.%, otherwise the coating quality is poor and there are many holes, such as Figure 4 (d) as shown.

[0057] Most of the high entropy coatings in the prior art have two disadvantages. One is that they have many pores, and the other is that they do not wet WC and other ceramics sufficiently. The present invention solves the porosity problem by filling the high entropy alloy with BNi7, and by adding traditional BNi7 or Cu solder, the above two disadvantages can be basically eliminated. Compared with the coatings prepared by the traditional process, the coating prepared by the method of the present invention has high bonding strength with the substrate and controllable thickness; compared with the traditional brazing coating, the coating prepared by the method of the present invention has less brittle phase, high content of hard particles, strong wear resistance, simple operation and low cost.

[0058] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a high entropy alloy wear-resistant coating, characterized in that: The preparation method comprises the following steps: firstly, copper or nickel-based solder powder and FeCoCrNiCu high entropy alloy powder are fully mixed, and then heated and dried under the protection of an inert gas to form a first mixed powder; then, WC powder is added and mixed to form a second mixed powder; then, the second mixed powder is stirred and mixed with ethanol to form a paste-like mixed powder; finally, the paste-like mixed powder is coated on a substrate; and after vacuum brazing, a high entropy alloy wear-resistant coating is obtained.

2. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: The nickel-based solder powder is BNi7 powder, and the weight percentage of the BNi7 powder in the first mixed powder is 10-15%.

3. The method for preparing a high entropy alloy wear-resistant coating according to claim 2, characterized in that: The BNi7 powder is nearly spherical and has a particle size of 350-450 meshes.

4. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: The weight percentage of the WC powder in the second mixed powder is 10-30%.

5. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: In the process of forming the first mixed powder, the time for sufficient mixing is 2 to 5 hours; the inert gas is argon or nitrogen, and the mixture is heated to 100 to 200° C. for drying.

6. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: The FeCoCrNiCu high entropy alloy powder is spherical powder with a particle size of 50 to 100 μm.

7. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: The coating has a thickness of 0.5 to 1.5 mm.

8. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: The process parameters of vacuum brazing are: vacuum degree reaches 5×10 -3 Pa, heat to 1150-1180°C at a rate of 5-10°C / min, keep warm for 30-60min, then cool to 500°C at a rate of 3-5°C / min and cool to room temperature with the furnace.

9. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: After the paste-like mixed powder is coated on the substrate, it is scraped flat with a scraper and then vacuum brazing is performed.

10. The method for preparing a high entropy alloy wear-resistant coating according to claim 1, characterized in that: The substrate comprises a steel substrate, and the substrate is ground, polished and cleaned before coating.

Citation Information

Cited By

  • Method for assisting high-temperature alloy TLP connection by adding high-entropy alloy nanoparticles to middle layer

    CN119927400A

  • High-entropy composite brazing filler metal and preparation method and application thereof

    CN120533362A