Method for simply preparing self-supporting oxygen evolution electrocatalyst in large scale at room temperature

By etching and processing foam bimetallic materials at room temperature, a high-performance self-supported oxygen evolution electrocatalyst was prepared, which solved the problem of time-consuming and energy-consuming preparation of non-precious metal oxygen evolution electrocatalysts, and achieved excellent performance and large-scale application Hydrogen production technology of electrolytic water.

CN119020805APending Publication Date: 2024-11-26CHINA GASOLINEEUM PIPELINE ENG CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310584782.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The preparation method of non-precious metal oxygen evolution electrocatalysts in the prior art consumes a lot of energy and time, and the commercial oxygen evolution electrocatalysts are costly and cannot achieve large-scale application.

Method used

A self-supported oxygen evolution electrocatalyst was prepared by a simple method at room temperature, including obtaining the base material cutting, cleaning, etching and drying in a strong acid solution to obtain a high-performance non-precious metal material for electrocatalysis of oxygen evolution reaction.

Benefits of technology

It has achieved rapid and large-scale preparation of self-supported non-precious metal oxygen evolution electrocatalysts with excellent performance at room temperature, reducing preparation cost and energy consumption, and has better performance than commercial precious metal catalysts. It is suitable for electrolytic hydrogen production technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020805A_ABST
    Figure CN119020805A_ABST
Patent Text Reader

Abstract

The invention provides a method for simply preparing a self-supporting non-noble metal oxygen evolution electrocatalyst on a large scale at room temperature, which comprises the following steps: acquiring a substrate material, and cutting the substrate material according to a set size; the cut substrate material is subjected to cleaning treatment; immersing the cleaned substrate material into a strong acid solution with a set concentration at a set temperature for etching, and continuously stirring the strong acid solution to enable the strong acid solution to be in full contact with the substrate material; after etching is completed, the substrate material is taken out of the strong acid solution and cleaned and dried, and the self-supporting non-noble metal material is obtained; the self-supporting non-noble metal material can be directly used as a high-performance oxygen evolution reaction electrocatalyst. Based on a chemical etching principle, the self-supporting non-noble metal oxygen evolution electrocatalyst can be rapidly prepared in a strong acid solution. The preparation method is simple to operate and does not need a high-energy-consumption and long-time-consumption process. And large-scale preparation is easy, and wide development prospects and huge industrial application potential are shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of hydrogen production by electrolysis of water, and specifically relates to a method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature. Background Art

[0002] With the continuous development of the economy and society, human demand for energy is also increasing. At present, my country's energy structure is dominated by fossil fuels. The large-scale consumption of fossil fuels inevitably brings a series of environmental problems, such as the emission of greenhouse gas carbon dioxide. To this end, my country continues to optimize its energy structure to gradually increase the proportion of new energy. Among them, hydrogen energy has attracted much attention due to its advantages such as high combustion calorific value, no carbon emissions, and rich application scenarios. However, hydrogen does not exist in nature, so there are many hydrogen production processes in industry, such as natural gas hydrogen production, methanol cracking hydrogen production, coke oven gas hydrogen production, and water electrolysis hydrogen production. Compared with other hydrogen production technologies, the energy conversion efficiency of water electrolysis hydrogen production technology is very high (>70%), and the coupling of renewable energy power generation with water electrolysis technology to produce hydrogen can achieve zero carbon emissions throughout the life cycle of the technology. Therefore, water electrolysis hydrogen production technology has a very bright application prospect.

[0003] The technology of producing hydrogen by electrolysis of water includes two half reactions, namely the hydrogen evolution reaction (HER) and the oxygen evolution reaction (OER). The hydrogen evolution reaction is a two-electron transfer process, while the oxygen evolution reaction is a four-electron transfer process. Therefore, the kinetics of the oxygen evolution reaction is slower, which has become the main challenge of the technology of producing hydrogen by electrolysis of water.

[0004] Commercial oxygen evolution electrocatalysts are mainly iridium and ruthenium oxides, but they are expensive and scarce, and cannot be used on a large scale. Therefore, it is urgent to develop a non-precious metal oxygen evolution electrocatalyst that can drive the oxygen evolution reaction at a high current density under the lowest possible overpotential.

[0005] In addition, most of the current non-precious metal oxygen evolution electrocatalysts are synthesized using multi-step methods, and the synthesis methods such as hydrothermal method, annealing treatment, electrochemical deposition method, etc. consume a lot of energy and time. Therefore, the development of a simple, fast and large-scale synthesis method is crucial for the application of non-precious metal oxygen evolution electrocatalysts. Summary of the invention

[0006] In order to solve the above problems in the prior art, that is, to solve the challenges of high energy consumption and long consumption faced in the preparation of non-precious metal oxygen evolution electrocatalysts, the present invention proposes a method for large-scale and simple preparation of self-supporting oxygen evolution electrocatalysts at room temperature, the method comprising:

[0007] Step S10, obtaining a base material, and cutting the base material according to a set size;

[0008] Step S20, cleaning the cut base material;

[0009] Step S30, immersing the cleaned substrate material in a strong acid solution of a set concentration at a set temperature for etching, and continuously stirring the strong acid solution to make it fully contact with the substrate material;

[0010] Step S40, after etching is completed, the substrate material is taken out from the strong acid solution, and is cleaned and dried to obtain a self-supporting non-precious metal material; the self-supporting non-precious metal material can be directly used as a high-performance oxygen evolution reaction electrocatalyst.

[0011] Furthermore, in the method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature as described above, the substrate material is a foam bimetallic material; the foam bimetallic material includes foam iron nickel, foam cobalt nickel and foam nickel molybdenum.

[0012] Furthermore, in the method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, the cut substrate material is cleaned by alternately cleaning the cut substrate material with anhydrous ethanol and deionized water.

[0013] Furthermore, in the above-mentioned method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, the set temperature for etching the substrate material is 20°C to 60°C.

[0014] Furthermore, in the method for preparing a self-supporting oxygen evolution electrocatalyst in a large scale and in a simple manner at room temperature as described above, the strong acid solution comprises hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid.

[0015] Furthermore, in the above-mentioned method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, the etching time of the substrate material in the strong acid solution is 0.5 min to 10 min.

[0016] Furthermore, in the above-mentioned method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, when stirring the strong acid solution, the stirring speed is 120 to 600 rpm.

[0017] Furthermore, according to the method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature as described above, after etching is completed, the substrate material is taken out from the strong acid solution, and is cleaned and dried to obtain a self-supporting non-precious metal material, and the method is: rinse the etched substrate material with deionized water, and stand it for drying at room temperature; wherein the room temperature condition is 20°C to 30°C, and the standing drying time is not less than 60 minutes.

[0018] Furthermore, in the above-mentioned method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, the pore size of the foam bimetallic material is 0.1 mm to 10 mm and the porosity is 95% to 98%.

[0019] Furthermore, in the above-mentioned method for simply preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, the concentration of the strong acid solution is 0.01 mol / L to 5 mol / L.

[0020] Beneficial effects of the present invention:

[0021] The present invention can rapidly and on a large scale prepare a self-supporting non-precious metal oxygen evolution electrocatalyst with excellent performance at room temperature without complicated preparation methods, thus filling the gap in the corresponding field.

[0022] Compared with the preparation method of the traditional oxygen evolution electrocatalyst, the preparation method of the present invention is simple to operate, the raw materials are easily available, the cost is low, and the high temperature and high pressure reaction conditions of the hydrothermal method and annealing treatment and the high energy consumption of the electrochemical deposition method are not required; and it is easy to prepare for large-scale amplification and can be directly configured to the industrial electrolysis water hydrogen production equipment for large-scale application. Under the same overpotential (0.5V) condition, the oxygen evolution electrocatalyst provided by the present invention, such as the iron-nickel based oxygen evolution electrocatalyst (current density 528mA / cm 2 ) is much better than the commercial precious metal IrO 2 (Current density 213mA / cm 2 ) and foamed Fe-Ni substrate (current density 175 mA / cm 2 ), effectively reducing the power consumption of hydrogen production by alkaline water electrolysis, thus having important application value in the field of hydrogen production by water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings.

[0024] Figure 1 It is a schematic diagram of a process for preparing a self-supporting oxygen evolution electrocatalyst in a large scale and in a simple manner at room temperature according to an embodiment of the present invention.

[0025] Figure 2This is a physical picture of a self-supporting iron-nickel based oxygen evolution electrocatalyst with different reaction times prepared in an embodiment of the present invention.

[0026] Figure 3 This is an X-ray diffraction pattern of a self-supporting iron-nickel based material prepared in an embodiment of the present invention at -5min.

[0027] Figure 4 This is a scanning electron microscope image of a base foamed iron-nickel material prepared in an embodiment of the present invention at 50 μm.

[0028] Figure 5 This is a scanning electron microscope image of a self-supporting iron-nickel based material prepared in an embodiment of the present invention at 50 μm for -5 min.

[0029] Figure 6 This is a scanning electron microscope image of a self-supporting iron-nickel based material prepared in an embodiment of the present invention at 10 μm for -5 min.

[0030] Figure 7 The self-supporting iron-nickel-based material, the base foamed iron-nickel material and IrO prepared by an embodiment of the present invention 2 Polarization curve of the oxygen evolution reaction of the material.

[0031] Figure 8 The area of ​​10×10 cm prepared by an embodiment of the present invention is 2 Physical picture of self-supporting iron-nickel based material-5min.

[0032] Fig. 9 The area of ​​0.5×0.5 cm is prepared in one embodiment of the present invention. 2 and 10×10cm 2 Polarization curve of oxygen evolution reaction of self-supporting iron-nickel based material-5min. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant inventions, rather than to limit the invention. It should be noted that, in the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other.

[0035] A method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature is provided in accordance with an embodiment of the present invention. Figure 1 As shown, the method includes:

[0036] Step S10, obtaining a base material, and cutting the base material according to a set size;

[0037] Step S20, cleaning the cut base material;

[0038] Step S30, immersing the cleaned substrate material in a strong acid solution of a set concentration at a set temperature for etching, and continuously stirring the strong acid solution to make it fully contact with the substrate material;

[0039] Step S40, after etching is completed, the substrate material is taken out from the strong acid solution, and is cleaned and dried to obtain a self-supporting non-precious metal material; the self-supporting non-precious metal material can be directly used as a high-performance oxygen evolution reaction electrocatalyst.

[0040] In order to more clearly illustrate the method of the present invention for preparing a self-supporting oxygen evolution electrocatalyst in a large scale and in a simple manner at room temperature, the following is combined with the attached Figure 1 , each step in the embodiment of the present invention is described in detail.

[0041] Step S10, obtaining a base material, and cutting the base material according to a set size.

[0042] In this embodiment, the substrate material is a foam bimetal material, and the foam bimetal material includes foam iron nickel, foam cobalt nickel and foam nickel molybdenum. The present invention is preferably foam iron nickel. The pore size of the foam iron nickel is preferably set to 0.1mm to 10mm, and the porosity is preferably set to 95% to 98%.

[0043] Step S20, cleaning the cut base material.

[0044] In this embodiment, the cut substrate material is cleaned alternately with anhydrous ethanol and deionized water for a set number of times. The number of cleaning times of the substrate material of the present invention is preferably set to 3 times to ensure that the surface of the substrate material is clean before etching.

[0045] Step S30, immersing the cleaned substrate material in a strong acid solution of a set concentration at a set temperature for etching, and continuously stirring the strong acid solution to allow it to fully contact with the substrate material.

[0046] In this embodiment, a strong acid solution of a certain concentration is prepared. The strong acid solution includes hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid. The present invention is preferably hydrochloric acid, and the concentration of hydrochloric acid is preferably set to 0.01mol / L to 5mol / L.

[0047] In this embodiment, the cleaned substrate material is immersed in a strong acid solution of a set concentration at a set temperature for etching. The etching temperature of the substrate material of the present invention in the strong acid solution is preferably set to 20°C to 60°C, and the etching time is preferably set to 0.5min to 10min.

[0048] In this embodiment, the strong acid solution is continuously stirred to make it fully contact with the base material. When the strong acid solution is stirred in the present invention, the stirring speed is preferably set to 120 to 600 rpm.

[0049] Step S40, after etching is completed, the substrate material is taken out from the strong acid solution, and is cleaned and dried to obtain a self-supporting non-precious metal material; the self-supporting non-precious metal material can be directly used as a high-performance oxygen evolution reaction electrocatalyst.

[0050] In this embodiment, the etched substrate material is rinsed with deionized water and left to dry at room temperature, wherein the room temperature is 20° C. to 30° C., and the drying time is not less than 60 minutes.

[0051] In this embodiment, the self-supporting non-precious metal material can be directly used as an electrolytic cell anode / battery cathode to catalyze the oxygen evolution reaction, including but not limited to water electrolysis, renewable fuel cells, and oxygen evolution reactions in rechargeable metal-air batteries.

[0052] In order to explain the present invention more clearly, the present invention has carried out the preparation of self-supporting iron-nickel based materials and the oxygen evolution performance test of self-supporting iron-nickel based materials under different preparation conditions, as follows:

[0053] Application Example 1

[0054] Self-supporting Fe-Ni-based materials, Fe-Ni foam materials and IrO with different reaction times 2 Preparation and characterization of materials.

[0055] Cut the base material FeNi foam into 0.5×0.5cm 2 The size of the foam was 7 parts in total, and the foamed iron-nickel was washed 3 times with anhydrous ethanol and deionized water respectively; and a 1 mol / L hydrochloric acid solution was prepared.

[0056] Two portions of the foamed iron-nickel were used as a control group, and one portion was dried without any further treatment to obtain a base foamed iron-nickel material.

[0057] The other 1 part is loaded with precious metal catalyst IrO 2 The method is as follows: first, prepare a dispersant by mixing 450 μL of ethanol, 50 μL of Nafion solution and 500 μL of ultrapure water; then, 5 mg of active substance (IrO 2) was added to the dispersant and subjected to intense ultrasonic treatment to make the mixed solution uniform. Then the pre-cut foamed iron-nickel was soaked in the mixed solution for 5 minutes to make the active material evenly cover the surface of the substrate. Finally, the sample was dried at 60°C to obtain IrO 2 Material.

[0058] The remaining 5 portions of nickel-iron foam were immersed in the hydrochloric acid solution at room temperature for 2 min, 3 min, 4 min, 5 min and 6 min respectively, and the solution was stirred continuously to make it fully contacted. The nickel-iron foam was then taken out of the solution, rinsed with deionized water and left to dry at room temperature to obtain self-supporting nickel-based materials with different reaction times, such as Figure 2 As shown. In the figure, 1-base foamed iron-nickel material, 2-self-supporting iron-nickel-based material reacting for 2 minutes (abbreviated as self-supporting iron-nickel-based material-2min), 3-self-supporting iron-nickel-based material reacting for 3 minutes (abbreviated as self-supporting iron-nickel-based material-3min), 4-self-supporting iron-nickel-based material reacting for 4 minutes (abbreviated as self-supporting iron-nickel-based material-4min), 5-self-supporting iron-nickel-based material reacting for 5 minutes (abbreviated as self-supporting iron-nickel-based material-5min), 6-self-supporting iron-nickel-based material reacting for 6 minutes (abbreviated as self-supporting iron-nickel-based material-6min). Figure 2 It can be seen that new substances appear on the surface of the foamed iron-nickel after being immersed in the hydrochloric acid solution.

[0059] The X-ray diffraction pattern of the prepared self-supporting iron-nickel based material-5min, such as Figure 3 As shown. It can be seen that the diffraction peaks 44.9° and 52.2° correspond to the (111) and (200) crystal planes of Ni respectively; large peaks appear near the diffraction peaks 13.1° and 21°. This shows that the new substance appearing on the surface of the substrate foamed iron-nickel is an amorphous material.

[0060] The scanning electron microscope image of the substrate foam iron-nickel material at 50μm, as shown in Figure 4 The prepared self-supporting iron-nickel based material -5min scanning electron microscope image at 50μm, as shown in Figure 5 As shown; the scanning electron microscope image of the prepared self-supporting iron-nickel based material-5min at 10μm, as shown Figure 6 As shown. Figure 4 , 5 It can be seen from Figure 6 that the new substance appearing on the surface of the foamed iron-nickel is an amorphous flocculent structure, which is consistent with the X-ray diffraction data.

[0061] Application Example 2

[0062] Self-supporting Fe-Ni-based materials, Fe-Ni foam materials and IrO with different reaction times 2 Comparative test of oxygen evolution performance of materials.

[0063] Preparation of electrolyte: Take 40 ml of water, add 2.24 g of KOH solid and make it completely dissolved to prepare 1 mol / L KOH electrolyte.

[0064] The oxygen evolution performance of the material was tested using a three-electrode system. The working electrodes were self-supporting Fe-Ni-based materials, foamed Fe-Ni materials, and IrO 2 Materials: the counter electrode is a graphite rod and the reference electrode is a Hg / HgO electrode.

[0065] The electrochemical data of different materials were measured by linear sweep voltammetry using Chenhua CHI760E and compared.

[0066] Self-supporting Fe-Ni-based materials, Fe-Ni foam materials and IrO with different reaction times 2 The polarization curve of the oxygen evolution reaction of the material, such as Figure 7 As shown in the figure, the self-supporting Fe-Ni-based material has the best oxygen evolution performance of -5min, which can drive 500mA / cm at an overpotential of 0.49V. 2 The current density is 1000 mA / cm at an overpotential of 0.69 V. 2 And under the same overpotential (0.5V), the self-supporting iron-nickel-based material -5min (current density 528mA / cm 2 ) is much better than the commercial precious metal IrO 2 (Current density 213mA / cm 2 ) and foamed Fe-Ni substrate (current density 175 mA / cm 2 ).

[0067] Application Example 3

[0068] Large-area preparation of self-supporting Fe-Ni-based materials.

[0069] Cut the base material foamed iron nickel into 10×10cm 2 The size of the foamed iron-nickel was cleaned with anhydrous ethanol and deionized water for 3 times respectively; and a 1 mol / L hydrochloric acid solution was prepared;

[0070] The nickel-iron foam was immersed in a hydrochloric acid solution at room temperature for 5 min, and the solution was stirred continuously to ensure full contact; the nickel-iron foam was then taken out of the solution, rinsed with deionized water and dried at room temperature to obtain a 10×10 cm 2 Self-supporting Fe-Ni based materials such as Figure 8 As shown, it can be seen that the present invention has the ability to scale up the preparation of oxygen evolution electrocatalysts.

[0071] Application Example 4

[0072] The preparation area is 0.5×0.5cm2 and 10×10cm 2 Comparative test of oxygen evolution performance of self-supporting Fe-Ni based materials.

[0073] Preparation of electrolyte: Take 40 ml of water, add 2.24 g of KOH solid to completely dissolve it, and thus obtain 1 mol / L KOH electrolyte.

[0074] The oxygen evolution performance of the material was tested using a three-electrode system. The working electrodes were self-supporting iron-nickel based materials with different preparation areas, ensuring that the working area was 0.5×0.5cm during the electrochemical performance test. 2 , the counter electrode is a graphite rod, and the reference electrode is a Hg / HgO electrode.

[0075] The electrochemical data of self-supporting iron-nickel based materials with different preparation areas were measured by linear sweep voltammetry of Chenhua CHI760E and compared.

[0076] Preparation area: 0.5×0.5cm 2 and 10×10cm 2 The polarization curve of oxygen evolution reaction of self-supporting iron-nickel based material-5min, such as Fig. 9 As shown, it can be seen that enlarging the preparation area does not have much effect on the oxygen evolution performance of the sample.

[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature, characterized in that: The following steps are involved: Step S10, obtaining a base material, and cutting the base material according to a set size; Step S20, cleaning the cut base material; Step S30, immersing the cleaned substrate material in a strong acid solution of a set concentration at a set temperature for etching, and continuously stirring the strong acid solution to make it fully contact with the substrate material; Step S40, after etching is completed, the substrate material is taken out from the strong acid solution, and is cleaned and dried to obtain a self-supporting non-precious metal material; the self-supporting non-precious metal material can be directly used as a high-performance oxygen evolution reaction electrocatalyst.

2. A method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: The substrate material is a foam bimetal material; the foam bimetal material includes foam iron nickel, foam cobalt nickel and foam nickel molybdenum.

3. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: The cut base material is cleaned by using anhydrous ethanol and deionized water alternately to clean the cut base material.

4. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: The set temperature for etching the substrate material is 20°C to 60°C.

5. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: The strong acid solution includes hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid.

6. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: The etching time of the base material in the strong acid solution is 0.5min to 10min.

7. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: When the strong acid solution is stirred, the stirring speed is 120 to 600 rpm.

8. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 1, characterized in that: After etching is completed, the base material is taken out from the strong acid solution, and is cleaned and dried to obtain a self-supporting non-precious metal material. The method is: rinse the etched base material with deionized water, and let it stand and dry at room temperature; wherein the room temperature is 20°C to 30°C, and the standing and drying time is not less than 60 minutes.

9. The method for preparing a self-supporting oxygen evolution electrocatalyst on a large scale at room temperature according to claim 2, characterized in that: The pore size of the foam bimetallic material is 0.1 mm to 10 mm, and the porosity is 95% to 98%.

10. The method for preparing a self-supporting oxygen evolution electrocatalyst in a large scale and in a simple manner at room temperature according to claim 5, characterized in that: The concentration of the strong acid solution is 0.01 mol / L to 5 mol / L.