Preparation of MOF composite NiPdCu catalyst NiPdCu ZIF-8 for preparing urea through electro-catalysis
Through the MOF composite catalyst NiPdCu@ZIF-8, the problems of high energy consumption and large CO2 emissions in the existing urea production process are solved, and efficient electrocatalytic urea synthesis under mild conditions is achieved, and the Faraday efficiency and urea production of the catalyst are improved. , and enhances stability.
Patent Information
- Application Number
- CN202411135981.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing urea production process relies on the high temperature and high pressure Haber-Bosch process, resulting in high energy consumption and large CO2 emissions, and the electrocatalytic urea synthesis technology at room temperature is not yet mature.
NiPdCu alloy nanospheres were synthesized by electrosubstitution reaction by electrosubstitution reaction, and combined with ZIF-8 to adjust the C-N bond coupling activity and improve the urea synthesis efficiency.
Efficient electrocatalytic urea synthesis under mild conditions is achieved, which improves the Faraday efficiency and urea yield of the catalyst, and enhances the stability of the catalyst.
Smart Images

Figure HDA0004999446630000011 
Figure HDA0004999446630000012 
Figure HDA0004999446630000013
Abstract
Description
Technical Field
[0001] The present invention relates to a MOF composite NiPdCu catalyst NiPdCu@ZIF-8 for preparing urea by electrocatalysis, which belongs to electrocatalytic CO 2 The field of catalytic technology for synthesizing urea by coupling carbon-nitrogen bonds with nitrate. Background Art
[0002] As one of the most important organic chemicals, urea (CO(NH 2 ) 2 ) contains 46% nitrogen and is widely used in the fields of chemical industry, dyes, fertilizers, etc., greatly supporting the development of global agriculture and society. So far, the industrial production of urea depends on ammonia (NH 3 ) and carbon dioxide, which occurs under extreme conditions (150-200°C and 150-250 bar). Industrial NH produced by the Haber-Bosch process 3 It accounts for about 2% of global energy consumption and is accompanied by a large amount of CO 2 Emissions will aggravate the problem of global warming. In view of the concept of sustainable development of society, the development of a clean urea production technology under mild conditions is the prospect of industrial urea production in the future.
[0003] At room temperature and atmospheric conditions, the electrocatalytic synthesis of nitrate and carbon dioxide into urea is in line with the concept of sustainable development of society. 3 RR) is a tandem reaction, first reduced to *NO 2 - , further reaction intermediates (*NO, *N, *NH, *NH 2 、*NHO、*COHN 2 ), by NO 3 - Reduction to produce CO(NH 2 ) 2 Involving 16e - Transfer. Operando synchrotron radiation-Fourier transform infrared spectroscopy showed that *CONH 2Protonation is the potential-determining step in the process of preparing urea by coupling the CN bond of nitrate and carbon dioxide. The electronic structures of the metals in the alloy material are different, and electron transfer occurs between the metals, which can adjust the adsorption energy of the active center to the intermediate state of the catalytic reaction, reduce the energy barrier of the rate-determining step, and improve the activity of the catalytic reaction. The hollow sphere structure can increase the specific surface area of the alloy material, expose more active sites, and promote the catalytic reaction. Metal organic frameworks (MOFs) have unique pore structures and adjustable morphologies, and are widely used in the fields of catalysis, adsorption, and separation. Among them, the composite of MOFs materials and alloy catalysts can not only improve the catalytic activity, but also use the unique stability of MOFs materials to make the catalyst have a better life. Summary of the invention
[0004] Technical issues to be solved:
[0005] The present invention provides a method for preparing a MOF composite hollow nano alloy sphere (NiPdCu@ZIF-8) catalyst with different precursor concentrations for electrocatalytic preparation of urea. The present invention uses Ni spheres as templates, utilizes galvanic replacement reaction to synthesize NiPd alloy, further dopes Cu to synthesize NiPdCu alloy nanospheres, and finally composites NiPdCu hollow spheres with ZIF-8, which enables highly selective CN bond coupling with outstanding electrocatalytic urea synthesis activity. The effects of different ZIF-8 precursor concentrations on the performance of the NiPdCu@ZIF-8 catalyst are discussed. The NiPdCu@ZIF-8 catalyst prepared by the present invention has the advantages of high Faraday efficiency, high urea yield, strong stability, etc.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for preparing a hollow nano alloy sphere (NiPdCu@ZIF-8) composited with a MOF material and catalytically preparing urea, the steps of which are as follows:
[0008] (1) NiPdCu synthesis: A one-pot synthesis method was used to add a certain amount of PdCl according to the stoichiometric ratio. 2 and CuCl 2 Add 98 ml of deionized water, add 2 ml of 0.1 mol / L HCl solution, stir in a 60°C oil bath for 1 hour to make PdCl 2 and CuCl 2 Fully dissolved to form H 2 PdCl 4 With CuCl 2 Weigh 12.96 mg NiCl 2and 51.62 mg of sodium citrate were dissolved in a round-bottom flask containing 100 mL of deionized water, followed by stirring for 30 min under an Ar atmosphere to exclude air, and 10 mL of freshly prepared NaBH was added to the flask at a rate of 1 mL / min using a syringe pump. 4 The solution (4 mg / mL) was stirred for 10 minutes, and then 10 mL of the above-prepared H 2 PdCl 4 With CuCl 2 After the addition is completed, the Ar gas is stopped 10 minutes after stirring, and the stirring is continued for 40 minutes. Centrifuge at 12000 rpm for 8 minutes, wash three times with deionized water, and dry at 60°C for 12 hours for later use.
[0009] (2) ZIF-8 synthesis: Prepare 30 ml of 1.86 mg / L Zn(NO 3 ) 2 methanol solution and 30 ml of 4.1 mg / L dimethyl imidazole (MeIM) methanol solution, weigh 60 mg of polyvinyl pyrrolidone (PVP) and add Zn(NO 3 ) 2 The mixture was evenly dispersed in methanol solution by ultrasonic treatment for 5 minutes, and then the MeIM methanol solution was added dropwise under stirring, and stirred for about 2 hours. The mixture was centrifuged at 10,000 rpm for 8 minutes, washed with methanol three times, and dried at 60°C overnight for use.
[0010] (3) Preparation of NiPdCu@ZIF-8 with different precursor concentrations: The amount of NiPdCu particles synthesized once was used for composite experiments. 30 ml of Zn(NO 3 ) 2 methanol solution and MeIM methanol solution, weigh 60 mg of PVP and add Zn(NO 3 ) 2 The prepared NiPdCu particles were added to the methanol solution, and ultrasonication was performed until the particles were evenly dispersed. Then, the MeIM methanol solution was added dropwise under stirring, and stirred for about 2 hours. The mixture was centrifuged at 10,000 rpm for 8 minutes, washed with methanol three times, and dried at 60°C overnight for use.
[0011] (4) Preparation of working electrode: 5 mg of the prepared catalyst was dispersed in 490 μl of ethanol and 490 μl of deionized water, and ultrasonicated for about 1 hour to completely disperse it. Then, 20 μl of DuPont membrane solution was added and ultrasonicated for 10 minutes. 200 μl of catalyst slurry was taken with a pipette and placed on a pretreated carbon paper (1×1.5 cm 2 ) and dried completely at room temperature to obtain the working electrode required for the electrochemical catalytic reaction.
[0012] (5) Electrochemical tests were conducted in an H-type electrolytic cell under a three-electrode system. The counter electrode was a Pt sheet electrode, and the reference electrode was a saturated silver-silver chloride electrode. The proton exchange membrane used to isolate the cathode chamber and the anode chamber was a Nafion 117 perfluorosulfonic acid ion membrane. The CO 2 The flow rate is 30mL / min.
[0013] (6) Quantitative detection of urea: The reaction of the electrolytic cell was carried out using a constant potential electrolysis method, and the reaction time was 1 hour. The urea concentration was quantitatively detected using the DAMO-TSC method. After the reaction was completed, 1 ml of the electrolyte in the cathode tank was taken and mixed evenly with 2 ml of developer a and 1 ml of developer b, and heated at 110°C under condensation reflux conditions for 15 minutes. After the solution was cooled to room temperature, its absorbance was tested at 525 nm using a UV spectrophotometer.
[0014] In step (1) (3), the H required for preparing NiPdCu particles 2 PdCl 4 With CuCl 2 H 2 PdCl 4 With CuCl 2 The concentration was 5mmol / L.
[0015] In steps (2) and (3), Zn(NO 3 ) 2 The concentration gradients of methanol solution and MeIM methanol solution from high to low are 3.72 mg / L, 8.2 mg / L; 1.86 mg / L, 4.1 mg / L; 0.93 mg / L, 2.05 mg / L respectively.
[0016] In step (4), the purchased conductive carbon paper is cut into pieces with an area of 1×1.5 cm 2 shape, ultrasonically treated in anhydrous ethanol for 3 times, each time for 5 minutes to remove particles on the surface of carbon paper; heated at 60°C for 24 hours in a mixture of concentrated sulfuric acid: concentrated nitric acid: deionized water with a volume ratio of 1:1:1 to remove chemical impurities; rinsed several times with an equal volume of deionized water and ethanol mixture to remove residual acid and other impurities, and dried at room temperature for use.
[0017] In step (5), the formula for converting the standard hydrogen electrode potential (SHE) to the reversible hydrogen electrode potential (RHE) is:
[0018] E(versus RHE)=E(versus Ag / AgCl)+0.197V+0.059V×pH
[0019] The saturated CO 2The pH value of the electrolyte in the cathode chamber is 7.28. The pretreatment process of the proton exchange membrane Nafion 117 is as follows: 2 O 2 Boiled in water for 1 hour, washed with deionized water and soaked for 30 minutes; 5wt% H 2 SO 4 Boil for 1 hour, wash again with deionized water and soak for 30 minutes, and store in deionized water for later use. The original electrolyte in the cathode chamber is 60 ml of 0.2 M KHCO 3 With 0.02M KNO 3 The original electrolyte in the anode chamber was 60 ml of 0.2 M KHCO 3 Before the reaction started, CO was introduced into the cathode chamber at a flow rate of 30 mL / min. 2 , and in CO 2 The mixture was stirred for 30 minutes under atmosphere to exclude air.
[0020] In step (6), 10 ml of 85wt% concentrated phosphoric acid, 30 ml of 98% concentrated sulfuric acid, and 60 ml of deionized water are measured, the solutions are mixed, 10 mg of ferric chloride trihydrate is weighed and added to the mixed solution, shaken to dissolve, and fixed to volume with a 100 ml volumetric flask, which is recorded as developer a. 0.25 g of diacetyl monoxime (DAMO) and 5 mg of thiosemicarbazide (TSC) are weighed and dissolved in deionized water, shaken to dissolve, and fixed to volume with a 50 ml volumetric flask, which is recorded as developer b. The measured urea standard solution curve is A=0.09717c+0.0523(R 2 =0.9996), A is the absorbance at 525nm of the UV spectrophotometer, c is the urea concentration in ppm (mg / L). The absorbance of the color developing solution measured after the reaction is put into the standard curve to calculate the urea concentration.
[0021] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0022] The NiPdCu trimetallic alloy catalyst prepared by the present invention has a larger specific surface area and more active sites than a bimetallic alloy catalyst.
[0023] The NiPdCu prepared by the present invention isolates water molecules in the solution to a certain extent, thereby inhibiting the occurrence of hydrogen evolution reaction and improving the Faraday efficiency of the catalytic reaction, by virtue of the flexible and adjustable structure, high specific surface area and hydrophobic property of the outer surface of ZIF-8.
[0024] The prepared NiPdCu hollow nanospheres have a hollow structure and ultrathin and porous walls, which are beneficial to maximizing the atomic utilization rate, and the specific crystal faces exposed by the hollow structure can be used to optimize the adsorption energy of the metal active sites to the reaction intermediate species, thereby increasing the urea yield and improving the Faraday efficiency of the catalytic reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the TEM image of NiPdCu catalyst.
[0026] Figure 2 This is the TEM image of 0.93ppmNiPdCu@ZIF-8 catalyst.
[0027] Figure 3 This is the TEM image of 1.86 ppm NiPdCu@ZIF-8 catalyst.
[0028] Figure 4 This is the TEM image of 3.72 ppm NiPdCu@ZIF-8 catalyst.
[0029] Figure 5 This is the absorbance curve of urea standard solution.
[0030] Figure 6 It is the UV-visible absorption spectrum of urea standard solution.
[0031] Figure 7 It is the LSV linear sweep voltammetry curve of different catalysts.
[0032] Figure 8 This is the non-Faraday interval cyclic voltammetry curve of NiPdCu catalyst.
[0033] Fig. 9 This is the non-Faraday interval cyclic voltammetry curve of 0.93ppm NiPdCu@ZIF-8 catalyst.
[0034] Fig.10 This is the non-Faraday interval cyclic voltammetry curve of 1.86ppm NiPdCu@ZIF-8 catalyst.
[0035] Fig.11 This is the non-Faraday interval cyclic voltammetry curve of 3.72ppm NiPdCu@ZIF-8 catalyst.
[0036] Fig.12 This is a graph showing the relationship between current density and scan rate for different catalysts.
[0037] Fig.13 It is a graph showing the yield of electrocatalytically preparing urea using the catalysts in Examples 1, 2, 3, 4, and 5 at different voltages.
[0038] Fig.14 This is the Faraday efficiency diagram of the electrocatalytic preparation of urea by NiPdCu@ZIF-8 catalyst with different precursor concentrations at different voltages.
[0039] Fig.15 This is the stability diagram of the NiPdCu@ZIF-8 catalyst with a precursor concentration of 1.86 ppm after 5 cycles of reaction at a voltage of -0.6 V (vs. RHE). DETAILED DESCRIPTION
[0040] The present invention is further described in detail and completely below in conjunction with the embodiments:
[0041] Example 1
[0042] (1) Prepare 30 ml of Zn(NO 3 ) 2 methanol solution and 30 ml of MeIM methanol solution with a concentration of 4.1 mg / L;
[0043] (2) Weigh 60 mg of PVP and add Zn(NO 3 ) 2 In methanol solution, ultrasonicate for 5 minutes to make it evenly dispersed;
[0044] (3) Add MeIM methanol solution dropwise under stirring, stir for 2 hours, centrifuge at 10000 rpm for 8 minutes, wash three times with methanol, and dry at 60°C overnight to obtain ZIF-8 catalyst;
[0045] (4) Disperse 5 mg of ZIF-8 catalyst in 490 μl of ethanol and 490 μl of deionized water, sonicate for 1 hour to completely disperse it, then add 20 μl of DuPont membrane solution, and continue sonicating for 10 minutes. Use a pipette to draw 200 μl of catalyst slurry and place it on pretreated carbon paper (1×1.5 cm 2 ) and dried completely at room temperature to obtain a working electrode.
[0046] (5) Constant potential electrolysis was performed in an H-type electrolytic cell under a three-electrode system. The voltage gradient during constant potential electrolysis was converted into a reversible hydrogen electrode potential (vs. RHE) of -0.3 V, -0.4 V, -0.5 V, -0.6 V, and -0.7 V.
[0047] (6) After the reaction is completed, take 1 ml of the electrolyte after the reaction in the cathode chamber, mix it evenly with 2 ml of color developer a and 1 ml of color developer b, and heat it at 110°C under condensation reflux conditions for 15 minutes. After the solution is cooled to room temperature, its absorbance is measured at 525 nm on a UV spectrophotometer and substituted into the standard curve to calculate the urea concentration.
[0048] Example 2
[0049] (1) Weigh 12.96 mg NiCl 2 and 51.62 mg of sodium citrate were dissolved in a round-bottom flask filled with 100 ml of deionized water, and then stirred for 30 minutes under an Ar atmosphere;
[0050] (2) Use a syringe pump to add 10 ml of freshly prepared NaBH to the flask at 1 mL / min. 4 solution (4 mg / mL), stirred for 10 min;
[0051] (3) Use a syringe pump to add 10 mL of 5 mmol / L H into the flask at 1 mL / min. 2 PdCl 4 With 5mmol / L CuCl 2 The mixed solution was stirred for 10 minutes;
[0052] (4) Stop the introduction of Ar gas and continue stirring for 40 minutes. Centrifuge at 12000 rpm for 8 minutes, wash three times with deionized water, and dry at 60°C for 12 hours to obtain a NiPdCu catalyst;
[0053] (5) Disperse 5 mg of NiPdCu catalyst in 490 μl of ethanol and 490 μl of deionized water, sonicate for 1 hour to completely disperse it, then add 20 μl of DuPont membrane solution, and continue sonicating for 10 minutes. Use a pipette to draw 200 μl of catalyst slurry and place it on a pretreated carbon paper (1×1.5 cm 2 ) and dried completely at room temperature to obtain a working electrode. (6) Perform constant potential electrolysis in an H-type electrolytic cell under a three-electrode system. The voltage gradient during constant potential electrolysis is converted into a reversible hydrogen electrode potential (vs. RHE): -0.3V, -0.4V, -0.5V, -0.6V, -0.7V.
[0054] (7) After the reaction is completed, take 1 ml of the electrolyte after the reaction in the cathode chamber, mix it evenly with 2 ml of color developer a and 1 ml of color developer b, and heat it at 110°C under condensation reflux conditions for 15 minutes. After the solution is cooled to room temperature, measure its absorbance at 525 nm on a UV spectrophotometer and substitute it into the standard curve to calculate the urea concentration.
[0055] Example 3
[0056] (1) Weigh 12.96 mg NiCl 2 and 51.62 mg of sodium citrate were dissolved in a round-bottom flask filled with 100 ml of deionized water, and then stirred for 30 minutes under an Ar atmosphere;
[0057] (2) Use a syringe pump to add 10 ml of freshly prepared NaBH to the flask at 1 mL / min. 4 solution (4 mg / mL), stirred for 10 min;
[0058] (3) Use a syringe pump to add 10 mL of H into the flask at 1 mL / min. 2 PdCl 4 (5mmol / L) and CuCl 2 (5mmol / L) mixed solution, and continued stirring for 10 minutes;
[0059] (4) Stop the introduction of Ar gas and continue stirring for 20 minutes. Centrifuge at 12000 rpm for 8 minutes, wash three times with deionized water, and dry completely at 60°C to obtain NiPdCu particles for use;
[0060] (5) Prepare 30 ml of Zn(NO 3 ) 2 methanol solution and 30 ml of MeIM methanol solution with a concentration of 2.05 mg / L;
[0061] (6) Weigh 60 mg of PVP and add Zn(NO 3 ) 2 The prepared NiPdCu particles were added to the methanol solution and ultrasonicated for 20 minutes to make the particles dispersed evenly;
[0062] (7) Add MeIM methanol solution dropwise under stirring, stir for 2 hours, centrifuge at 10000 rpm for 8 minutes, wash three times with methanol, and dry at 60°C overnight to obtain a precursor concentration (in terms of Zn(NO 3 ) 2 Concentration represents) is 0.93ppmNiPdCu@ZIF-8 catalyst;
[0063] (8) 5 mg of 0.93 ppm NiPdCu@ZIF-8 catalyst was dispersed in 490 μL of ethanol and 490 μL of deionized water, and ultrasonicated for 1 hour to completely disperse it. Then, 20 μL of DuPont membrane solution was added and ultrasonicated for 10 minutes. 200 μL of catalyst slurry was taken with a pipette and spread on pretreated carbon paper (1×1.5 cm 2 ) and dried completely at room temperature to obtain a working electrode.
[0064] (9) Constant potential electrolysis was performed in an H-type electrolytic cell under a three-electrode system. The voltage gradient during constant potential electrolysis was converted into a reversible hydrogen electrode potential (vs. RHE) of -0.3 V, -0.4 V, -0.5 V, -0.6 V, and -0.7 V.
[0065] (10) After the reaction is completed, 1 ml of the electrolyte after the reaction in the cathode chamber is taken and mixed evenly with 2 ml of color developer a and 1 ml of color developer b, and heated at 110°C for 15 minutes under condensation reflux conditions. After the solution is cooled to room temperature, its absorbance is measured at 525 nm using a UV spectrophotometer and substituted into the standard curve to calculate the urea concentration.
[0066] Example 4
[0067] (1) Weigh 12.96 mg NiCl 2 and 51.62 mg of sodium citrate were dissolved in a round-bottom flask filled with 100 ml of deionized water, and then stirred for 30 minutes under an Ar atmosphere;
[0068] (2) Use a syringe pump to add 10 mL of freshly prepared NaBH to the flask at 1 mL / min. 4 solution (4 mg / mL), stirred for 10 min;
[0069] (3) Use a syringe pump to add 10 mL of 5 mmol / L H into the flask at 1 mL / min. 2 PdCl 4 With 5mmol / L CuCl 2 The mixed solution was stirred for 10 minutes;
[0070] (4) Stop the introduction of Ar gas and continue stirring for 20 minutes. Centrifuge at 12000 rpm for 8 minutes, wash three times with deionized water, and dry completely at 60°C to obtain NiPdCu particles for use;
[0071] (5) Prepare 30 ml of Zn(NO 3 ) 2 methanol solution and 30 ml of MeIM methanol solution with a concentration of 4.1 mg / L;
[0072] (6) Weigh 60 mg of PVP and add Zn(NO 3 ) 2 The prepared NiPdCu particles were added to the methanol solution and ultrasonicated for 20 minutes to make the particles dispersed evenly;
[0073] (7) Add MeIM methanol solution dropwise under stirring, stir for 2 hours, centrifuge at 10000 rpm for 8 minutes, wash three times with methanol, and dry at 60°C overnight to obtain a precursor concentration (in terms of Zn(NO 3 ) 2 Concentration indicated) is 1.86 ppm NiPdCu@ZIF-8 catalyst;
[0074] (8) 5 mg of 1.86 ppm NiPdCu@ZIF-8 catalyst was dispersed in 490 μL of ethanol and 490 μL of deionized water, and ultrasonicated for 1 hour to completely disperse it. Then, 20 μL of DuPont membrane solution was added and ultrasonicated for 10 minutes. 200 μL of catalyst slurry was taken with a pipette and spread on pretreated carbon paper (1×1.5 cm 2 ) and dried completely at room temperature to obtain a working electrode.
[0075] (9) Constant potential electrolysis was performed in an H-type electrolytic cell under a three-electrode system. The voltage gradient during constant potential electrolysis was converted into a reversible hydrogen electrode potential (vs. RHE) of -0.3 V, -0.4 V, -0.5 V, -0.6 V, and -0.7 V.
[0076] (10) After the reaction is completed, 1 ml of the electrolyte after the reaction in the cathode chamber is taken and mixed evenly with 2 ml of color developer a and 1 ml of color developer b, and heated at 110°C for 15 minutes under condensation reflux conditions. After the solution is cooled to room temperature, its absorbance is measured at 525 nm using a UV spectrophotometer and substituted into the standard curve to calculate the urea concentration.
[0077] Example 5
[0078] (1) Weigh 12.96 mg NiCl 2 and 51.62 mg of sodium citrate were dissolved in a round-bottom flask filled with 100 ml of deionized water, and then stirred for 30 minutes under an Ar atmosphere;
[0079] (2) Use a syringe pump to add 10 ml of freshly prepared NaBH to the flask at 1 mL / min. 4 solution (4 mg / mL), stirred for 10 min;
[0080] (3) Use a syringe pump to add 10 mL of 5 mmol / L H into the flask at 1 mL / min. 2 PdCl 4 With 5mmol / L CuCl 2 The mixed solution was stirred for 10 minutes;
[0081] (4) Stop the introduction of Ar gas and continue stirring for 20 minutes. Centrifuge at 12000 rpm for 8 minutes, wash three times with deionized water, and dry completely at 60°C to obtain NiPdCu particles for use;
[0082] (5) Prepare 30 ml of Zn(NO 3 ) 2 methanol solution and 30 ml of MeIM methanol solution with a concentration of 8.2 mg / L;
[0083] (6) Weigh 60 mg of PVP and add Zn(NO 3 ) 2 The prepared NiPdCu particles were added to the methanol solution and ultrasonicated for 20 minutes to make the particles dispersed evenly;
[0084] (7) Add MeIM methanol solution dropwise under stirring, stir for 2 hours, centrifuge at 10000 rpm for 8 minutes, wash three times with methanol, and dry at 60°C overnight to obtain a precursor concentration (in terms of Zn(NO 3 ) 2 Concentration indicated) is 3.72 ppm NiPdCu@ZIF-8 catalyst;
[0085] (8) 5 mg of 3.72 ppm NiPdCu@ZIF-8 catalyst was dispersed in 490 μL of ethanol and 490 μL of deionized water, and ultrasonicated for 1 hour to completely disperse it. Then, 20 μL of DuPont membrane solution was added and ultrasonicated for 10 minutes. 200 μL of catalyst slurry was taken with a pipette and spread on pretreated carbon paper (1×1.5 cm 2 ) and dried completely at room temperature to obtain a working electrode.
[0086] (9) Constant potential electrolysis was performed in an H-type electrolytic cell under a three-electrode system. The voltage gradient during constant potential electrolysis was converted into a reversible hydrogen electrode potential (vs. RHE) of -0.3 V, -0.4 V, -0.5 V, -0.6 V, and -0.7 V.
[0087] (10) After the reaction is completed, 1 ml of the electrolyte after the reaction in the cathode chamber is taken and mixed evenly with 2 ml of color developer a and 1 ml of color developer b, and heated at 110°C for 15 minutes under condensation reflux conditions. After the solution is cooled to room temperature, its absorbance is measured at 525 nm using a UV spectrophotometer and substituted into the standard curve to calculate the urea concentration.
[0088] Figure 1 The sample NiPdCu catalyst is in the shape of a hollow sphere with an average particle size of about 20 nm. Figure 2 For the NiPdCu@ZIF-8 catalyst with a MOF precursor concentration of 0.93ppm, a small amount of rod-shaped ZIF-8 particles can be observed on the surface of the nanospheres, and there are no scattered particles around the hollow nanosphere clusters. Figure 3 The NiPdCu@ZIF-8 catalyst with a precursor concentration of 1.86 ppm is Figure 2 The ZIF-8 rod-shaped crystals in the sample grew more uniformly, indicating that the NiPdCu hollow nano alloy sphere catalyst and the ZIF-8 rod-shaped particles were successfully composited. The concentration of MOF precursor was further adjusted to 3.72 ppm. Figure 4As shown in the figure, the rod-like particles on the surface of the hollow nanosphere clusters disappeared, and a denser and rougher MOF film was formed on its surface.
[0089] Figure 5 At a wavelength of 525nm, in 0.2M KHCO 3 and 0.02M KNO 3 Absorbance curves of standard solutions of urea with different concentrations under electrolyte background. Figure 6 In 0.2M KHCO 3 and 0.02M KNO 3 UV-visible absorption spectra of standard solutions of urea with different concentrations under electrolyte background.
[0090] Figure 7 The LSV linear sweep voltammetry curves of NiPdCu, 0.93ppm NiPdCu@ZIF-8, 1.86ppm NiPdCu@ZIF-8, and 3.72ppm NiPdCu@ZIF-8. 3 and 0.02M KNO 3 In the electrolyte, the same potential was applied, and the corresponding currents obtained by different catalysts were different. Among them, the corresponding response current value of 1.86ppm NiPdCu@ZIF-8 was the largest, indicating that in the same concentration of electrolyte and the same CO 2 Under the flow rate conditions, 1.86ppm NiPdCu@ZIF-8 responds more strongly to nitrate than the other three catalysts. It can be preliminarily concluded that 1.86ppm NiPdCu@ZIF-8 has more advantages than the other three catalysts.
[0091] Figure 8 , Fig. 9 , Fig.10 , Fig.11 The non-Faraday range cyclic voltammetry curves are respectively for NiPdCu, 0.93ppm NiPdCu@ZIF-8, 1.86ppm NiPdCu@ZIF-8, and 3.72ppm NiPdCu@ZIF-8. The electrochemically active area (ECSA) reflects the actual area where the catalyst material contacts the solution and undergoes electrochemical reaction. It is used to measure the difference in the active surface of the catalyst and has a reference role in explaining the law of change in catalytic reaction performance. By testing the cyclic voltammetry curves of the catalyst at different scan rates (5, 10, 20, 30, 40, 50, 60mV / s) in the non-Faraday range, the current scan rate density difference (y) of the median potential in the test interval is taken, and a linear fit is performed relative to the scan rate (x). The slope k of the curve is the value of the catalyst double layer capacitance (C dl ).
[0092] Fig.12is the relationship between current density and scan rate for different catalysts. dl / Cs, Cs is the specific capacitance of the corresponding surface smooth sample under the same conditions (related to the material properties, generally a certain value), so ECSA is positively correlated with the double layer capacitance, that is, ECSA is positively correlated with the slope k of the fitting curve, and the size of the electrochemical specific surface area can be judged by the value of the slope k. The size law of the slope k value is 1.86ppm NiPdCu@ZIF-8>3.72ppm NiPdCu@ZIF-8>0.93ppmNiPdCu@ZIF-8>NiPdCu, which is basically consistent with the size law of the yield of electrocatalytic preparation of urea. The size of the double layer capacitance of 1.86ppm NiPdCu@ZIF-8 is 11.07mF·cm -2 , NiPdCu is 4.07mF·cm -2 This shows that at this precursor concentration, the use of MOF composite alloy materials can better expose catalytic active sites, which is beneficial to promote the conversion of nitrate and the synthesis of urea.
[0093] Fig.13 The graph is the yield of electrocatalytic preparation of urea by the catalysts prepared in Examples 1, 2, 3, 4, and 5. It can be seen that ZIF-8 alone does not have a catalytic effect, while the NiPdCu alloy catalyst doped with Pd and Cu has the performance of catalytic preparation of urea. At -0.5 V (vs. RHE), its urea yield is 27.43 mg·h -1 ·g cat -1 The urea yield of the three catalysts composited with MOF materials of different precursor concentrations basically showed a trend of first increasing and then decreasing in the range of -0.3 to -0.7 V (vs. RHE), and the catalytic performance was the best at -0.6 V (vs. RHE). The urea yield of 1.86 ppm NiPdCu@ZIF-8 at -0.6 V (vs. RHE) was 78.89 mg·h -1 ·g cat -1 Compared with the NiPdCu alloy catalyst not composited with MOF material, the yield was increased by 2.88 times.
[0094] Fig.14 Figure 2 is the Faradaic efficiency diagram of different catalysts. The Faradaic efficiency of 1.86 ppm NiPdCu@ZIF-8 reached 15.78% at -0.6 V (vs. RHE).
[0095] Fig.15 Figure 2 shows the stability of the NiPdCu@ZIF-8 catalyst after five cycles of reaction at -0.6 V (vs. RHE). It is found that the urea yield and Faradaic efficiency can be stably maintained at 78 mg·h-1 ·g cat -1 and about 15.5%, which shows that the catalyst has good cycle stability.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. The present invention discloses a MOF composite NiPdCu catalyst NiPdCu@ZIF-8 for electrocatalytically preparing urea, characterized in that: The catalyst is a NiPdCu hollow nano alloy composited with ZIF-8 of different precursor concentrations. The method comprises the following steps: (1) Dissolve the designed amount of nickel chloride and sodium citrate in deionized water, introduce Ar gas and stir for about 30 minutes to exclude air, and add 10 ml of sodium borohydride solution into the mixed solution with a syringe pump and stir; (2) Add 10 ml of chloropalladic acid and copper chloride mixed solution into the above mixed solution using a syringe pump and continue stirring for 20 to 40 minutes. Wash with deionized water and dry completely at 60°C to obtain NiPdCu particles; (3) preparing zinc nitrate hexahydrate methanol solution and dimethylimidazole methanol solution of different gradient concentrations; weighing 60 mg of polyvinyl pyrrolidone and adding it to the zinc nitrate hexahydrate methanol solution, then adding the NiPdCu particles prepared in steps (1) and (2) to the mixed solution, and ultrasonicating for 20 minutes to evenly disperse the particles; (4) Add dimethylimidazole methanol solution dropwise under stirring, continue stirring for 2 hours, wash with methanol, and dry at 60°C overnight to obtain NiPdCu@ZIF-8 catalysts with different precursor concentrations.
2. The catalyst according to claim 1, characterized in that When the catalyst is used for electrocatalytic preparation of urea, the reactants are carbon dioxide and nitrate, and the maximum urea yield and Faraday efficiency are stably maintained at 78 mg·h -1 ·g cat -1 The catalyst life is greater than 50 hours.
3. The preparation of the MOF composite NiPdCu catalyst NiPdCu@ZIF-8 for electrocatalytic preparation of urea according to claim 1, characterized in that: The catalyst is a composite structure composed of alloy and MOF material. The metal types of the catalyst alloy are nickel, palladium and copper, among which nickel is used as the template of hollow nanospheres, the molar ratio of palladium and copper metal elements is 1:1, and the morphology of the alloy is the shape of hollow nanospheres; the MOF material used in the catalyst is ZIF-8, and the molar concentration ratio of metal ions to ligands in ZIF-8 is 1:
8.
4. The method for preparing the MOF composite NiPdCu catalyst NiPdCu@ZIF-8 for electrocatalytically preparing urea according to claim 1, characterized in that: The amount of nickel chloride and sodium citrate added in step (1) is 12.96 mg and 51.62 mg respectively, the amount of deionized water added is 100 ml, the concentration of sodium borohydride solution is 4 mg / mL, and the injection rate of the syringe pump is 1 mL / min.
5. The method for preparing the MOF composite NiPdCu catalyst NiPdCu@ZIF-8 for electrocatalytically preparing urea according to claim 1, characterized in that: The concentrations of chloropalladic acid and cupric chloride in the mixed solution of chloropalladic acid and cupric chloride described in step (2) are both 5 mmol / L, and the injection rate of the syringe pump is 1 mL / min.
6. The method for preparing the MOF composite NiPdCu catalyst NiPdCu@ZIF-8 for electrocatalytically preparing urea according to claim 1, characterized in that: The concentrations of the zinc nitrate hexahydrate methanol solution and the dimethylimidazole methanol solution of different gradient concentrations described in step (3) are 0.93 mg / L, 2.05 mg / L; 1.86 mg / L, 4.10 mg / L; 3.72 mg / L, 8.20 mg / L, respectively.
7. The use according to claim 2, characterized in that: The evaluation method of the catalytic performance of the catalyst is as follows: 1 mg of the catalyst is loaded on the carbon paper of the working electrode, and constant potential electrolysis is performed in an H-type electrolytic cell of a three-electrode system for 1 hour. The voltage gradient during constant potential electrolysis is converted into a reversible hydrogen electrode potential (vs. RHE): -0.3V, -0.4V, -0.5V, -0.6V, -0.7V.