Pulse electrodeposition nickel-iron plating process for wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy
By adjusting the pulse electrodeposition parameters and pretreatment steps, the problem of poor nickel ferroplating on the surface of aluminum or aluminum silicon alloy is solved, and a nickel ferroplating with excellent wear and corrosion resistance is prepared, which improves the surface of aluminum or aluminum silicon alloy. comprehensive performance.
Patent Information
- Application Number
- CN202411241455.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-26
AI Technical Summary
On the surface of aluminum or aluminum-silicon alloys, it is difficult for the prior art to effectively prepare high-quality pulsed electrodeposited nickel-iron plating, resulting in uneven coating, leakage plating and weak adhesion, affecting its wear-resistant and corrosion-resistant properties.
By adjusting the pulse electrodeposition parameters, a nickel and iron plating solution is prepared and specific pretreatment steps are carried out, including grinding, polishing, oil removal, grease removal, zinc dipping, etc., combined with the rectangular wave pulse current deposition process, the concentration of nickel and iron ions is controlled. and current density, optimize the hardness and corrosion resistance of nickel-iron plating.
The hardness, corrosion resistance and surface morphology of the nickel-iron plating are adjusted, which significantly improves the comprehensive performance of the nickel-iron plating, and enhances the mechanical properties and wear resistance of the surface of aluminum or aluminum-silicon alloys.
Smart Images

Figure CN119020835A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum or aluminum-silicon alloy surface treatment, and in particular to a pulsed electrodeposition nickel-iron plating process for the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy. Background Art
[0002] With the emphasis on sustainability and resource utilization, aluminum or aluminum silicon alloy materials are favored in many fields such as aerospace, shipbuilding and vehicle engineering due to their excellent mechanical properties, processing performance, and lightweight characteristics. Especially in the automotive field, aluminum or aluminum silicon alloys are gradually used to replace cast iron materials for internal combustion engine piston power components to reduce the overall weight of the engine and improve fuel efficiency and power performance. However, due to the poor thermal stability and high thermal expansion coefficient of aluminum or aluminum silicon alloys, thermal expansion is very likely to occur when working in a medium and high temperature environment of 300-450℃, which will aggravate the friction and wear between the piston and the cylinder wall to a certain extent, thereby affecting the normal operation of the internal combustion engine. In addition, in the field of marine engineering, the oxide film formed on the surface of aluminum or aluminum silicon alloy cannot meet the increasingly high anti-corrosion requirements. In the marine environment, the surface of aluminum or aluminum silicon alloy is prone to corrosion, which reduces the service life of the material. Therefore, it is necessary to modify the surface of aluminum or aluminum silicon alloy to improve the mechanical properties, wear resistance and corrosion resistance of aluminum or aluminum silicon alloy.
[0003] At present, in the surface processing technology of aluminum or aluminum silicon alloy, anodizing, electrodeposition or anodizing + electrodeposition process is usually used. The cost of the electrodeposition process is low, and it can be precisely processed on complex components such as piston heads and microelectronic devices. Compared with anodizing, electrodeposition has lower requirements for workpiece pretreatment, so it is better to use electrodeposition. In the early stage, nickel metal plating has good corrosion resistance and heat resistance, and is used as a protective-decorative plating of materials. However, nickel plating with a thickness greater than 25μm can meet the requirements of non-porous and dense. Therefore, in order to improve the comprehensive performance of the coating, in recent years, researchers have added other alloying elements or particles to a single metal coating to form an alloy coating or a composite coating. Among them, the nickel-iron alloy coating has a low thermal expansion coefficient. When the mass fraction of iron in the coating is close to 60%, the thermal expansion coefficient is close to that of the ceramic coating, which is better adapted to aluminum or aluminum-silicon piston alloys and can play a certain role in heat insulation. In addition, the addition of iron can increase the hardness of the coating, thereby improving the tribological properties of the aluminum alloy surface. At present, most scholars' research on nickel-iron alloy coatings is mainly focused on the fields of functional magnetic materials and electronic products, and no systematic study has been conducted on the influence of nickel-iron alloy coatings on the friction and corrosion properties of the substrate under some special working conditions (cylinder reciprocating motion). Pulse electrodeposition can control the iron content in the nickel-iron coating, so as to prepare a nickel-iron alloy coating with better comprehensive properties such as heat resistance, wear resistance and corrosion resistance. Therefore, studying the process of pulse electrodeposition of nickel-iron coating on the surface of aluminum or aluminum-silicon alloy is of great significance to improving the surface properties of aluminum or aluminum-silicon alloy.
[0004] Electrochemical deposition is the process of depositing a layer of metal or non-metallic material on the cathode surface (aluminum or aluminum-silicon alloy) to form a single or composite coating with corrosion resistance, wear resistance and uniform composition on the deposited surface. The pulse electrodeposition process is widely used in electrochemical deposition. Compared with other technologies, the pulse electrodeposition process is suitable for manufacturing various single or multi-element alloy coatings due to its low equipment cost, simple control of coating shape and thickness, and minimum geometric restrictions on the substrate. The working principle of pulse electrodeposition is to periodically change the magnitude and direction of the current density. When the current is in the on state, the electrolyte has a very high pulse current density, the nickel-iron nucleation rate is greater than the growth rate, and the nickel-iron ions close to the cathode are fully deposited; when the current is in the off state, the discharge ions around the cathode return to the initial concentration, and the nickel-iron ions quickly diffuse in the electrolyte, weakening the concentration polarization. This method of controlling the periodic on and off of the current can not only improve the performance of the coating, refine the grains, and make the coating dense, but also improve the current efficiency and reduce side reactions such as hydrogen evolution.
[0005] At present, pulse electrodeposition is widely used in single precious metal deposition. Since the coating quality of pulse electrodeposition in different alloys is different, the plating solution formula and production process of different alloys are not perfect, which increases the difficulty of pulse electrochemical deposition of nickel-iron coating on the surface of aluminum or aluminum-silicon alloy to a certain extent. On the other hand, there are many parameters in pulse electrodeposition, and changing a single parameter often leads to problems such as no obvious improvement in coating quality. Only by optimizing the combination of pulse process parameters can the nickel-iron coating with the best comprehensive performance be obtained.
[0006] At present, nickel-iron coating can be directly electrodeposited on copper or iron substrates without copper as the bottom layer or other intermediate layers, and the process is relatively simple. However, the process of processing nickel-iron coating on aluminum alloy is relatively complicated and requires specific process treatment. A relatively mature process system has not yet been proposed at home and abroad. Because the oxide film produced on the surface of substrates such as aluminum or aluminum-silicon alloys or the material itself contains silicon and other components that affect the quality of the coating, it is easy to cause defects such as leakage plating and uneven coating caused by weak adhesion between the substrate and the electroplating layer. Therefore, it is sometimes difficult to prepare an ideal coating on the surface of aluminum and aluminum-silicon alloys using conventional pulse electrodeposition processes. In order to improve the quality of the coating on the surface of aluminum or aluminum-silicon alloys, certain pretreatment is a prerequisite for pulse electrodeposition. Summary of the invention
[0007] Technical problem to be solved: The present invention provides a pulse electrodeposition nickel-iron plating process for wear-resistant and corrosion-resistant surfaces of aluminum or aluminum-silicon alloys. By changing the pulse electrodeposition parameters, nickel-iron plating layers with different hardness and corrosion resistance can be obtained.
[0008] Technical solution: A pulse electrodeposition nickel-iron plating process for wear-resistant and corrosion-resistant surfaces of aluminum or aluminum-silicon alloys, comprising the following steps: (1) preparing a nickel sulfate aqueous solution and a sodium chloride conductive salt aqueous solution, wherein the nickel sulfate concentration is 180-220 g / L and the sodium chloride conductive salt concentration is 18-25 g / L; (2) preparing an aqueous solution containing citric acid, sodium citrate complexing agent and ferrous sulfate, wherein the citric acid concentration is 2-4 g / L and the sodium citrate complexing agent concentration is 22-30 g / L, and the ferrous sulfate concentration is 15 ~30g / L; (3) preparing a sodium dodecyl sulfate aqueous solution, and then adding a boric acid buffer to the solution, wherein the sodium dodecyl sulfate concentration is 0.2~0.4g / L, and the boric acid buffer concentration is 20~40g / L; (4) adding the solution obtained in step (2) to the solution obtained in step (1), stirring, and then adding the solution obtained in step (3) to obtain a nickel-iron plating solution; the volume ratio of the solution obtained in step (1): the solution obtained in step (2): the solution obtained in step (3) is 1:2 :1:1, controlling the concentration of nickel ions in the final solution to be 15wt.% to 25wt.%, and the concentration of iron ions to be 1wt.% to 3wt.%; (5) grinding and polishing the surface of the aluminum or aluminum silicon alloy sample to a roughness not exceeding 50nm; (6) preparing an aqueous solution of sodium carbonate and sodium phosphate, wherein the concentration of sodium carbonate is 25 to 30g / L and the concentration of sodium phosphate is 30 to 35g / L, and immersing the sample obtained in step (5) in the solution to remove oil and grease; (7) immersing the sample obtained in step (6) in a 100 ~120g / L sodium hydroxide aqueous solution; (8) preparing a suspension containing 50-60g / L sodium hydroxide, 50-60g / L zinc oxide and 60-70g / L potassium sodium tartrate, and immersing the sample obtained in step (7) in the suspension; (9) using a nickel plate as an anode and a cathode as the sample obtained in step (8) in a nickel-iron plating solution, pulse electrodeposition is performed, and the cathode and the anode are placed vertically in an electrolytic cell with a distance of 5cm; the pulse waveform of the pulse electrodeposition is a rectangular wave, and the single pulse square wave current is defined as on The current density flowing through the p The current at t off No current flows during this time; the duty cycle is defined as t on / (t on +t off ), the frequency is 1 / (t on +t off ); After connecting to the pulse power supply, set the average current density to 2-6.5A / dm 2 , pulse width is 1-10ms, duty cycle is 30%-90%, pulse electrodeposition time is 20min, and the final product is obtained.
[0009] The pulse electrodeposition described above uses a single pulse square wave current.
[0010] The pH of the nickel-iron plating solution is adjusted to 2.5-3 with ammonia water or hydrochloric acid, and the temperature of the nickel-iron plating solution is maintained at 50° C. during the pulse electrodeposition process.
[0011] The above samples were immersed in different solutions for pretreatment and then cleaned with water.
[0012] The temperature of the suspension was maintained at 30°C.
[0013] The transition layer is pre-processed on the surface of aluminum or aluminum-silicon alloy. The suspension used to prepare the transition layer is a suspension containing zinc oxide. Tetrahydroxy zinc ions formed by zinc oxide in a strong alkaline solution react chemically with aluminum or aluminum oxide to form a transition zinc layer on the surface.
[0014] Preferably, the current density in the pulse electrodeposition is 2A / dm 2 , the frequency is 2000Hz and the duty cycle is 50%.
[0015] Beneficial effects: (1) The preparation process is simple and easy to operate; (2) The hardness, corrosion resistance and surface morphology of the nickel-iron alloy coating can be adjusted by the pulse electrodeposition process. The hardness can be adjusted by the duty cycle, and the corrosion resistance and surface morphology can be adjusted by the current density and frequency. (3) The duty cycle in pulse electrodeposition can adjust the nickel-iron nucleation rate, inhibit the abnormal co-deposition of nickel-iron, and further optimize the comprehensive performance of the nickel-iron alloy coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the pulse electrodeposition nickel-iron coating of the present invention.
[0017] Figure 2 The electrochemical curves of the coating prepared under different process parameters of the present invention are: (a) polarization curve; (b) electrochemical impedance spectrum.
[0018] Figure 3 The tribological properties of the nickel-iron coating prepared by the present invention under different process parameters are: (a) friction coefficient; (b) wear rate
[0019] Figure 4 It is a SEM picture of the nickel-iron coating prepared by the present invention.
[0020] Figure 5 The nickel-iron coating prepared by the present invention is scanned by EDS (2A / dm 2 , when the frequency is 2000Hz, the duty cycle is 50%). DETAILED DESCRIPTION
[0021] The bright nickel-iron alloy coating with both anti-corrosion and mechanical properties is prepared by a single-pulse electrochemical deposition method, which can deposit the nickel-iron alloy coating on an aluminum or aluminum-silicon alloy substrate under simple manual operation.
[0022] The embodiments of the present invention are specifically implemented according to the following steps:
[0023] Examples 1-16 are used to study the effects of the main process parameters of pulse electrodeposition, current density, duty cycle, and frequency on the surface quality and performance of the coating. Specifically, after the nickel-iron plating solution is prepared and the solution is stabilized, a single-pulse square wave power supply is used to study the effects of the pulse parameters on the hardness, corrosion resistance, and wear resistance of the coating. At the same time, an aluminum-silicon alloy substrate (M142 aluminum-silicon alloy) is set as a comparative example to see the effects of the electrochemical deposition of nickel-iron coating on the hardness, corrosion resistance, and wear resistance of aluminum or aluminum-silicon alloy.
[0024] Example 1
[0025] (1) Dissolve 180 g / L nickel sulfate and 18 g / L sodium chloride conductive salt in deionized water in turn and stir to dissolve;
[0026] (2) dissolving 2 g / L citric acid, 22 g / L sodium citrate complexing agent, and 15 g / L ferrous sulfate in deionized water in sequence and stirring to dissolve;
[0027] (3) 0.2 g / L sodium dodecyl sulfate was dissolved in deionized water at 30-40° C. by stirring, and after cooling to room temperature, 20 g / L boric acid buffer was added;
[0028] (4) adding the solution obtained in step (2) to the solution in step (1), stirring, and then adding to the solution obtained in step (3), stirring. The pH of the final nickel-iron solution is adjusted to 2.5-3 with ammonia or hydrochloric acid, and the plating solution temperature is maintained at 50° C. during the pulse electrodeposition process;
[0029] (5) Grind and polish the sample surface to remove the surface oxide film and obtain a uniform, low-roughness aluminum or aluminum-silicon alloy surface. When grinding, use 800-1000-1200-2000 mesh sandpaper to process the sample in sequence. After cleaning, use a polishing machine to polish the aluminum or aluminum-silicon alloy surface again for 20 minutes; polish until the surface is mirror-like and the roughness is reduced by less than 50nm;
[0030] (6) Dissolve 25g / L sodium carbonate and 30g / L sodium phosphate in deionized water, and immerse the polished sample in the solution for 5 minutes at a temperature of 55°C. The glycerol and fatty acids on the surface of the substrate react to form glycerol and soap solution through saponification reaction, which separates from the surface of the substrate, allowing the coating to better adhere to the substrate. After the sample is immersed in different solutions for pretreatment (oil and grease removal, alkaline washing, zinc immersion), it needs to be washed three times in a row with running water to ensure that the sample surface is clean in the next process;
[0031] (7) Place the sample that has been degreased and deoiled in step (6) into a 100 g / L sodium hydroxide aqueous solution for 30 seconds at a temperature of 25° C. Etching is an important step in pretreatment, and its purpose is to further remove surface dirt, scale, and inclusions;
[0032] (8) Prepare a suspension containing 50g / L sodium hydroxide, 50g / L zinc oxide, and 60g / L potassium sodium tartrate. Place the sample after etching in step (7) into the suspension and soak for 30s. Stir the prepared zinc-immersion suspension in a magnetic stirrer to evenly disperse the zinc oxide particles in the solution, and keep the temperature at 30°C. In the electrochemical deposition of aluminum or aluminum-silicon alloy, it is also necessary to pre-process the intermediate transition layer to prevent the rapid formation of an oxide film on the surface of the aluminum-silicon alloy, among which the zinc-immersion process is the most widely used. Zinc-immersion mainly further removes the natural oxide film on the surface of the aluminum-silicon parts, so that the crystals exposed on the surface of the aluminum-silicon alloy undergo a substitution reaction with zinc ions. The deposited layer of zinc can prevent the re-oxidation of the aluminum surface and ensure the bonding strength between the coating and the substrate. At the same time, it avoids the reaction between aluminum and the coating, thereby affecting the quality of the coating;
[0033] (9) The nickel-iron plating solution uses a nickel plate as the anode and a zinc-treated aluminum-silicon alloy as the cathode. The cathode and the anode are placed vertically in the electrolytic cell at a distance of 5 cm. Pulse electrodeposition mainly uses a single pulse square wave current. The sample after pulse electrodeposition needs to be rinsed in distilled water and dried with a hair dryer. Pulse electrodeposition mainly uses a single pulse square wave current. Figure 1 As shown, the pulse waveform is a rectangular wave, and the single pulse square wave current is defined as on The current density flowing through the p The current at t off No current flows during this time. The duty cycle is defined as t on / (t on +t off ), the frequency is 1 / (t on +t off ). After connecting to the pulse power supply, set the average current density to 2-6.5A / dm 2 , pulse width is 1-10ms, duty cycle is 30-90%, and pulse electrodeposition time is 20min.
[0034] Pulse plating process conditions: set the frequency of the single pulse square wave to 200Hz, the duty cycle to 30%, and the average current density to 2A / dm 2 .
[0035] Example 2
[0036] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 200 Hz, the duty cycle is 50%, and the average current density is 3.5 A / dm 2 .
[0037] Example 3
[0038] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 200 Hz, the duty cycle is 70%, and the average current density is 5 A / dm 2 .
[0039] Example 4
[0040] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 200 Hz, the duty cycle is 90%, and the average current density is 6.5 A / dm 2 .
[0041] Example 5
[0042] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 800 Hz, the duty cycle is 30%, and the average current density is 3.5 A / dm 2 .
[0043] Example 6
[0044] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 800 Hz, the duty cycle is 50%, and the average current density is 2 A / dm 2 .
[0045] Example 7
[0046] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 800 Hz, the duty cycle is 70%, and the average current density is 6.5 A / dm 2 .
[0047] Example 8
[0048] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 800 Hz, the duty cycle is 90%, and the average current density is 5 A / dm 2 .
[0049] Example 9
[0050] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 1400 Hz, the duty cycle is 30%, and the average current density is 5 A / dm 2 .
[0051] Example 10
[0052] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 1400 Hz, the duty cycle is 50%, and the average current density is 6.5 A / dm 2 .
[0053] Embodiment 11
[0054] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 1400 Hz, the duty cycle is 70%, and the average current density is 2 A / dm 2 .
[0055] Example 12
[0056] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 1400 Hz, the duty cycle is 90%, and the average current density is 3.5 A / dm 2 .
[0057] Embodiment 13
[0058] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 2000 Hz, the duty cycle is 30%, and the average current density is 6.5 A / dm 2 .
[0059] Embodiment 14
[0060] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 2000 Hz, the duty cycle is 50%, and the average current density is 5 A / dm 2 .
[0061] Embodiment 15
[0062] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 2000 Hz, the duty cycle is 70%, and the average current density is 3.5 A / dm 2 .
[0063] Example 16
[0064] The process is the same as in Example 1, wherein the pulse plating process conditions are: the frequency of the single pulse square wave is set to 2000 Hz, the duty cycle is 90%, and the average current density is 2A / dm 2 .
[0065] Embodiment 1-16 carries out pulse electrodeposition, and the specific steps are as follows:
[0066] (1) Substrate (cathode) preparation
[0067] The cathode is 20mm×10mm×5mm M142 aluminum silicon alloy. The aluminum silicon alloy is first ground with 800-1000-1200-2000 mesh and then polished with a polishing machine until the surface presents a mirror gloss, and then degreased with a chemical alkali solution at a temperature of 65°C (5min), rinsed with running water, alkaline etched with an alkaline solution at a temperature of 25°C (30s), zinc dipped with a zinc solution at a temperature of 25°C (30s), and rinsed with running water. The composition of the chemical alkali solution is 25g / L sodium carbonate and 30g / L sodium phosphate; the composition of the alkaline solution is 100g / L sodium hydroxide; the composition of the zinc solution is 50g / L sodium hydroxide, 50g / L zinc oxide, and 65g / L potassium sodium tartrate.
[0068] (2) Anode preparation
[0069] A 60 mm × 70 mm × 5 mm nickel plate was used as the anode, which was smoothed with sandpaper, rinsed with deionized water and dried before electrodeposition.
[0070] (3) Coating preparation
[0071] Immerse the pretreated cathode and anode in the electrodeposition solution, adjust the water bath temperature to maintain the electrodeposition solution temperature at 50°C, and control the distance between the cathode and the anode to be 5 cm. After the pulse power supply is turned on, the process parameter range is selected: the frequency of the pulse current is 200-2000Hz, the duty cycle is 30-90%, and the average current density is 2-6.5A / dm 2 After 20 minutes of power on, cut off the power supply of the electrodeposition device. Take out the cathode aluminum silicon parts, wash and dry them with distilled water.
[0072] (4) Detection of coating
[0073] The coating appearance quality of Examples 1-16 was tested with reference to the following method:
[0074] 1) Hardness test: Use a Vickers hardness tester to measure the hardness by applying a load of 0.05 kgf at five different positions for 15 seconds, and calculate the average hardness value.
[0075] 2) Corrosion resistance test: Use an electrochemical workstation to perform electrochemical tests, and fit the impedance spectrum to obtain the charge transfer resistance R ct , draw the polarization curve and get the corrosion current I corr When R ct The bigger, I corr The smaller it is, the better the corrosion resistance of the coating.
[0076] 3) Wear resistance test: A reciprocating friction tester was used to apply a constant normal load of 0.5 N, a reciprocating motion sliding length of 5 mm, a reciprocating frequency of 3 Hz, and a time of 20 min. The friction coefficient between the nickel-iron coating and the 304 stainless steel ball was recorded, and the wear rate was calculated.
[0077] The test results of the tribological properties, corrosion properties and average hardness of Examples 1-16 and M142 aluminum silicon alloy are as follows:
[0078]
[0079] It can be seen from the above table that the hardness of the coating of Examples 1-16 is significantly higher than the hardness of the M142 aluminum silicon alloy substrate (164HV), which indicates that the nickel-iron coating increases the hardness of the substrate and improves the mechanical properties of the substrate to a certain extent. In terms of wear resistance, the wear rate of the examples (43.52-65.58×10 -4 mm 3 / N·m) is significantly lower than the wear rate of M142 aluminum-silicon alloy (124.95×10 -4 mm 3 / N·m), indicating that the improvement of the hardness of the nickel-iron coating improves the wear resistance of the substrate itself. In addition, in terms of corrosion resistance, the self-corrosion current of the embodiment is one order of magnitude smaller than that of the M142 aluminum-silicon alloy, which also indicates that the nickel-iron coating improves the corrosion resistance of the substrate.
[0080] In addition, the change of current density can significantly change the corrosion resistance of the coating. In terms of corrosion resistance, the higher the current density, the worse the corrosion resistance. When the current density is the lowest 2A / dm 2 Self-corrosion current (0.0536~0.0710μA / cm 2 ) is less than the self-corrosion current of M142 aluminum-silicon alloy (0.2149μA / cm 2 ), charge transfer resistance (16842~28756Ω·cm 2 ) is greater than the charge transfer resistance of M142 aluminum silicon alloy (11646Ω·cm 2 ), indicating that the electrochemical deposition of nickel-iron coating improves the corrosion resistance of the material surface. In addition, the current density is 2A / dm 2 The nickel-iron coating has the best corrosion resistance compared to other embodiments.
[0081] In Examples 1-16, during the frequency change from 200-2000 Hz, as the frequency increases, the hardness, corrosion resistance and wear resistance of the nickel-iron coating are improved. In particular, in terms of wear resistance, when the frequency is 200 Hz, the friction coefficient of the nickel-iron coating is generally large (1.2-1.58), and the wear resistance is poor. When the frequency is a maximum of 2000 Hz, that is, in Examples 13-16, the coating hardness, corrosion resistance and wear resistance reach a relatively optimal level. corr Can reach 0.0536μA / cm 2 , R ct 28756Ω·cm 2 , hardness is 294.3HV, and the lowest friction coefficient is 1.00. The reason is that the increase in frequency can inhibit the growth of grains and play a role in refining grains. Grain refinement can not only reduce the contact between the surface and the external corrosive medium and improve corrosion resistance, but also fine crystallization can improve the hardness of the coating to a certain extent, thereby improving the wear resistance of the coating.
[0082] It can be seen from Examples 1-16 that the change in duty cycle mainly affects the hardness of the coating. When the duty cycle changes between 30% and 90%, the overall hardness of the coating shows a trend of first increasing and then decreasing. In Examples 13-16, Example 13 (duty cycle of 30%) has a hardness of 275.1HV, while in Example 14 (duty cycle of 50%), the hardness reaches a maximum of 300.7HV. This is because as the duty cycle increases from 30% to 50%, the on-time increases, and the cathode polarization is less affected by concentration polarization, which inhibits the hydrogen evolution reaction of pulse electrodeposition to a certain extent, plays a certain role in refining the grains and reducing the porosity of the coating surface. In Examples 13-16, the hardness is significantly reduced to 278.4HV in Example 15 (duty cycle of 50%). However, when the duty cycle is too large (50-90%), the on-time is too large, and the concentration polarization has a greater impact on the electrochemical deposition process, resulting in the growth of grains. Therefore, when the duty ratio is 50%, the surface hardness is greater.
[0083] In Examples 1-16, considering the comprehensive test results of the coating, the relevant preferred performance parameters are as follows:
[0084]
[0085] On this basis, the nickel-iron coating under the optimal parameters was prepared and compared with the above-mentioned embodiment 16 with the best comprehensive performance, and the relevant performance test results are as follows:
[0086]
[0087] like Figure 2 (a) shows the polarization curve, the self-corrosion current of the optimized coating (0.057μA / cm2 ) and the self-corrosion current of Example 16 in the horizontal axis (0.054 μA / cm 2 ) is consistent. At the same time, in the electrochemical impedance spectrum of 2(b), the optimized coating (28296Ω·cm 2 ) and the coating prepared in Example 16 (28756Ω·cm 2 ) The semicircle diameters are almost the same, indicating that the impedance modulus of the coating is large. Therefore, from the experimental results of Example 16 and the optimized parameters, the coating prepared after parameter optimization has good corrosion resistance. From the perspective of the hardness of the coating, the optimized parameters significantly improve the hardness of the coating, from 290.3HV in Example 16 to 301HV. When the duty cycle in pulse electrodeposition is optimized from 90% to 50%, the hardness of the coating is further improved. Figure 3 As shown in the figure, the optimized tribological performance is further improved compared with Example 16, and the wear rate is increased from 54.04×10 -4 mm 3 / N·m is reduced to 51.45×10 -4 mm 3 / N·m, and the friction coefficient also decreased from 1.29 to 1.06.
[0088] In summary, it can be concluded that when the current density in pulse electrodeposition is 2A / dm 2 When the frequency is 2000Hz and the duty cycle is 50%, the coating prepared not only has a bright surface, but also has the best comprehensive performance in corrosion resistance, wear resistance and hardness.
[0089] The microstructure of the nickel-iron coating prepared under the optimal parameters and Example 16 is as follows Figure 4 As shown, the nickel-iron coating mainly generates the form of grains covering the coating surface, and the surface is formed by a large number of distorted asymmetric spheres stacked. The coating surface crystallization prepared under the preferred parameters is more meticulous, and the grain distribution is more uniform. And the nickel-iron coating prepared under embodiment 16, the grain distribution is uneven on the microscopic surface, and the grains are more coarse. Therefore, it can be seen from the coating microstructure prepared under the preferred parameters that the refinement of the grains improves the hardness and corrosion resistance of the coating.
[0090] Figure 5 The energy spectrum of the nickel-iron coating shows that the nickel-iron coating is evenly distributed on the surface, which covers the M142 aluminum-silicon alloy very well and plays a certain protective role. In addition, among the mass percentages of nickel-iron in the coating, the surface nickel content is relatively high relative to iron, and the atomic percentage of nickel-iron is 3:2, indicating that the abnormal co-deposition phenomenon is suppressed to a certain extent. Therefore, more nickel is deposited on the surface of the substrate to suppress the co-deposition of iron, thereby improving the corrosion resistance of the coating.
[0091] In summary, it can be concluded that the nickel-iron plating solution for aluminum or aluminum-silicon alloy and its pulse electrodeposition process of the present invention can prepare a nickel-iron alloy coating with good mechanical properties and good corrosion resistance, and to a certain extent improve the physical and chemical properties of the surface of aluminum or aluminum-silicon alloy.
[0092] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. Pulse electrodeposition nickel-iron plating process for wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy. It is characterized in that The method comprises the following steps: (1) preparing a nickel sulfate aqueous solution and a sodium chloride conductive salt aqueous solution, wherein the nickel sulfate concentration is 180-220 g / L and the sodium chloride conductive salt concentration is 18-25 g / L; (2) preparing an aqueous solution containing citric acid, sodium citrate complexing agent and ferrous sulfate, wherein the citric acid concentration is 2-4 g / L and the sodium citrate complexing agent concentration is 22-30 g / L, and the ferrous sulfate concentration is 15-30 g / L; (3) preparing a sodium dodecyl sulfate aqueous solution, and then adding a boric acid buffer to the solution, wherein the sodium dodecyl sulfate concentration is 0.2-0.4 g / L and the boric acid buffer concentration is 20-40 g / L; (4) adding the solution obtained in step (2) to the solution obtained in step (1), stirring, and then adding the solution obtained in step (3) to obtain a nickel-iron plating solution; the solution obtained in step (1): the solution obtained in step (2): the solution obtained in step (3) The volume ratio of the obtained solution is 12:1:1, and the concentration of nickel ions in the final solution is controlled to be 15wt.%~25wt.%, and the concentration of iron ions is 1wt.%~3wt.%; (5) The surface of the aluminum or aluminum silicon alloy sample is ground and polished, and the roughness does not exceed 50 nm; (6) Sodium carbonate and sodium phosphate aqueous solutions are prepared, wherein the concentration of sodium carbonate is 25~30 g / L and the concentration of sodium phosphate is 30~35 g / L, and the sample obtained in step (5) is immersed in the solution to remove oil and grease; (7) The sample obtained in step (6) is immersed in 100~120 g / L sodium hydroxide aqueous solution; (8) A mixture containing 50~60 g / L sodium hydroxide, 50~60 g / L zinc oxide and 60~70 g / L potassium sodium tartrate suspension, immersing the sample obtained in step (7) in the suspension; (9) using a nickel plate as an anode and the sample obtained in step (8) as a cathode in a nickel-iron plating solution, performing pulse electrodeposition, wherein the cathode and the anode are placed vertically in the electrolytic cell at a distance of 5 cm; the pulse waveform of the pulse electrodeposition is a rectangular wave, and the single pulse square wave current is defined as on The current density flowing through the time is J p The current at t off No current flows during this time; the duty cycle is defined as t on / (t on +t off ), the frequency is 1 / (t on +t off ); After connecting to the pulse power supply, set the average current density to 2-6.5 A / dm 2 , pulse width is 1-10 ms, duty cycle is 30%-90%, pulse electrodeposition time is 20 min, and the final product is obtained.
2. According to the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy, the pulse electrodeposition nickel-iron plating process is used, It is characterized in that Pulse electrodeposition uses a single pulse square wave current.
3. According to the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy, the pulse electrodeposition nickel-iron plating process is used, It is characterized in that The pH of the nickel-iron plating solution is adjusted to 2.5-3 with ammonia water or hydrochloric acid, and the temperature of the nickel-iron plating solution is maintained at 50° C. during the pulse electrodeposition process.
4. According to the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy, the pulse electrodeposition nickel-iron plating process is used, It is characterized in that The samples were immersed in different solutions for pretreatment and then cleaned with water.
5. According to the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy, the pulse electrodeposition nickel-iron plating process is used, It is characterized in that The suspension temperature was maintained at 30°C.
6. The process for pulse electrodeposition of nickel-iron coating on the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy according to claim 1, It is characterized in that The transition layer is pre-processed on the surface of aluminum or aluminum-silicon alloy. The suspension used to prepare the transition layer is a suspension containing zinc oxide. Tetrahydroxy zinc ions formed by zinc oxide in a strong alkaline solution react chemically with aluminum or aluminum oxide to form a transition zinc layer on the surface.
7. The process for pulse electrodeposition of nickel-iron coating on the wear-resistant and corrosion-resistant surface of aluminum or aluminum-silicon alloy according to claim 1, It is characterized in that The current density in pulse electrodeposition is 2 A / dm 2 , the frequency is 2000 Hz and the duty cycle is 50%.
Citation Information
Patent Citations
Surface treatment process for electroplating iron-nickel alloy and electroplating solution thereof
CN101311322A
Single-pulse electrodeposition method for Ni-Fe alloy magnetic coatings
CN105780068A
Method of electro plating on aluminum and its alloys
GB770503A
Method for manufacturing cobalt iron alloy and plated magnetic thin-film of cobalt iron alloy, and method for manufacturing quaternary alloy and plated magnetic thin-film of cobalt iron molybdenum alloy
JP2003034891A
Fe-ni-p alloy electroplating solution, electro-deposition method for fe-ni-p alloy coating, and alloy coating
WO2022267384A1
Cited By
Method for improving metal deposition effect of TGV glass substrate
CN119776935A
Preparation method of electroplated nickel-based amorphous polishing coating for ultra-precision machining of metal surface
CN120888995A