Method for improving SiC single crystal and epitaxial growth quality
By electrochemical etching pretreatment of SiC substrate, the problems of SiC single crystal and medium and high defect layers in epitaxial growth are solved, and higher quality crystal and epitaxial growth are achieved. By optimizing the substrate surface, two-dimensional nucleation is reduced. Improves the overall performance of the material.
Patent Information
- Application Number
- CN202411150485.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
SiC single crystals and epitaxials are prone to high defect layers during growth, which limits the improvement of material quality, especially due to the misalignment problem caused by two-dimensional nucleation on large-area substrates.
Before SiC crystal growth, the SiC substrate material is subjected to electrochemical etching pretreatment to remove surface damage and defects, improve substrate surface quality, reduce the probability of two-dimensional nucleation, optimize the initial nucleation of growth, and adopt electrochemical etching Form step flow to improve crystal and epitaxial quality.
It effectively improves the growth quality of SiC single crystal and epitaxial, reduces defect density, improves product qualification rate and production capacity, avoids misalignment caused by two-dimensional nucleation, and achieves higher quality crystal and epitaxial growth.
Smart Images

Figure CN119020868A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a method for improving the quality of SiC single crystal and epitaxial growth. Background Art
[0002] Compared with the first and second generation semiconductor materials represented by Si and GaAs, the third generation semiconductor represented by SiC has the characteristics of wide band gap, high saturated electron mobility, high breakdown electric field strength, and high thermal conductivity. Due to its superior performance such as high frequency, high temperature resistance, chemical etching resistance, high efficiency, strong radiation resistance, and high voltage resistance, it is regarded as one of the most promising materials in the field of semiconductor materials. With the increasing maturity of semiconductor preparation technology, SiC has become a supporting material for core electronic devices in the fields of intelligent communications, new energy vehicles, aerospace, Internet of Things, intelligent transportation, smart grid, nuclear energy technology, oil exploration, etc. Therefore, there is an urgent need for higher quality and larger SiC crystals to meet the huge application scenarios and market demand. At present, the mainstream growth methods of SiC single crystals are physical vapor transport (PVT), top solution seeding (TSSG), and high temperature chemical vapor deposition (HTCVD), while the mainstream growth method of SiC epitaxy is homogeneous / heteroepitaxial chemical vapor deposition (CVD).
[0003] The basic principle of single crystal growth by PVT method is to use a closed or semi-closed crucible system. The crucible material can be isostatic graphite, tantalum carbide, tantalum carbide coating or metal tungsten, etc. During growth, the powder sublimates and decomposes in the high temperature area, and condenses at the low temperature seed crystal (seed crystal holder) to form a single crystal through the material transport process in the growth chamber.
[0004] The basic principle of single crystal growth by TSSG method is to use a closed or semi-closed crucible system, with a graphite crucible as a heating component (heating method is not limited), and carbon felt to provide insulation. Through the heating system, the crucible provides the heat source required for crystal growth, and the Si source in the crucible and the C source provided by the graphite crucible are precipitated at the seed crystal interface through convection transmission to form SiC single crystal.
[0005] The HTCVD method for growing SiC crystals is similar to the PVT method. The reaction vessel is a graphite crucible, and the precursor (e.g. SiH 4 +C 3 H 8 ) The gas enters the heating zone of the graphite crucible through the gas channel at the bottom of the crucible. A seed crystal is installed on the top of the crucible. The gas is deposited and grows silicon carbide crystals at the seed crystal with a lower temperature. The growth temperature of the HTCVD method is generally above 2300℃.
[0006] At present, the epitaxial growth of silicon carbide generally adopts the CVD method, in which Si-containing gas source and C-containing gas source (for example: SiH 4 +C2 H 4 , TCS+C 3 H 8 etc.), in H 2 Under the action of carrier gas, N 2 It can be used as doping gas, mixed together and introduced into the reactor. The temperature of the reaction chamber is about 1500°C. The Si source gas and the C source gas react preferentially on the silicon carbide substrate to achieve the growth of the silicon carbide epitaxial layer.
[0007] Different from the traditional Si and GaAs single crystal growth, whether it is the PVT, TSSG, HTCVD method to grow silicon carbide single crystals, or the CVD method to grow silicon carbide epitaxial layers, the crystal growth is carried out on a large-sized seed crystal or substrate, and the seed crystal size is basically the same as the size of the growing crystal. It is impossible to use the traditional small seed crystal necking, shouldering and other processes to obtain single crystals with low defect density. On a large-area silicon carbide seed crystal or substrate, multi-point two-dimensional nucleation often occurs during the initial growth. Single crystal growth starts from these two-dimensional nucleation centers. After the growth, many defects are often introduced due to misalignment, resulting in the silicon carbide single crystal / epitaxial layer often having a high defect layer during the initial growth of the seed crystal, which seriously limits the improvement of the quality of the silicon carbide single crystal / epitaxial. Therefore, the present invention provides a method for improving the quality of SiC single crystal and epitaxial growth. Summary of the invention
[0008] The purpose of the present invention is to provide a method for improving the quality of SiC single crystal and epitaxial growth, improve the surface quality of the substrate, avoid the probability of misalignment caused by two-dimensional nucleation on the substrate surface, optimize nucleation in the early stage of growth, thereby improving the crystal and epitaxial quality.
[0009] To achieve the above-mentioned purpose, the present invention provides a method for improving the quality of SiC single crystal and epitaxial growth. Before SiC crystal growth, the SiC substrate material is pretreated by electrochemical etching to improve the surface quality of the substrate and avoid the probability of misalignment caused by two-dimensional nucleation on the substrate surface, thereby improving the quality of SiC single crystal and epitaxial growth.
[0010] Preferably, the specific steps of performing electrochemical etching pretreatment on the SiC substrate material are:
[0011] (1) Exposing the growth surface of the SiC substrate to be pretreated and covering the other surface;
[0012] (2) The shielded surface of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode;
[0013] (3) The anode and cathode are placed symmetrically, the silicon carbide substrate is placed in the electrolyte, a power source is connected and energized, and the growth surface of the substrate is electrochemically etched;
[0014] (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.
[0015] Preferably, in step (2), the substrate masking surface and the graphite electrode are connected by conductive adhesive bonding or vacuum adsorption.
[0016] Preferably, in step (3), the distance between the cathode and the anode is 1-20 cm, the power supply voltage is 0-50 V, and the current is 0-500 mA.
[0017] Preferably, in step (3), the electrolyte is an HF solution with a concentration of 0-60wt%, a temperature of 0-50°C, and an electrochemical etching time of 0-5h.
[0018] Preferably, in step (4), the electrolyte is immersed for 0-12 hours, and the ultrasonic immersion is performed in deionized water for 0-10 hours.
[0019] Preferably, in step (4), the inert gas is Ar or He.
[0020] The electrochemical etching process basically includes two parts: In the first part, holes are generated during the etching process, current is formed at the SiC-electrolyte interface, and SiC is oxidized to SiO x Thin Films, Part II, SiO x The film is dissolved in the electrolyte. The type / concentration of the electrolyte, electrochemical etching time / temperature, additional auxiliary conditions (such as ultraviolet light irradiation, ultrasonic vibration, etc.), load voltage / current, and electrode spacing will all affect the electrochemical etching effect.
[0021] The main method of the present invention is to perform electrochemical etching pretreatment on the SiC substrate material before crystal growth, and then perform corresponding crystal or epitaxial growth. The basic principle of electrochemical etching pretreatment is: using electrochemical etching to preferentially remove defects such as substrate surface damage, improve substrate surface quality, and reduce the probability of inheriting original defects and dislocations in the substrate during crystal growth; during pretreatment, shallow etching pits can be left on the smooth substrate growth surface, which can provide more nucleation sites, reduce surface nucleation energy, optimize substrate growth surface, improve step flow, make the step flow delicate, gentle, and small in height, which is conducive to promoting the "flow" of steps, thereby optimizing the nucleation in the early stage of crystal growth, avoiding the probability of misalignment caused by two-dimensional nucleation on the smooth substrate surface, so that the crystal grows in a step flow manner from the early stage of crystal growth, and improving the quality of crystal growth. Utilizing the principles and advantages of electrochemical etching pretreatment and applying it to the growth of silicon carbide single crystals and epitaxy can effectively improve the product qualification rate and increase production capacity.
[0022] Therefore, the present invention provides a method for improving the quality of SiC single crystal and epitaxial growth, targeting the source of defects and dislocations, selecting a suitable substrate pretreatment scheme, etching to remove defects such as substrate surface damage, improving the surface quality of the substrate, and making steps appear on the surface to avoid the probability of dislocation caused by two-dimensional nucleation on the smooth substrate surface, so that the crystal grows in a step flow manner from the early stage of growth, thereby improving the crystal quality.
[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A diagram of the device used for electrochemical etching of the present invention;
[0025] Figure 2 This is a comparison of the rocking curves of the etched area and the unetched area in the single crystal growth experiment of the same crystal;
[0026] Figure 3 This is a comparison diagram of the rocking curves of the etched area and the unetched area in the same crystal epitaxial growth experiment;
[0027] Reference Numbers
[0028] 1-anode electrode; 2-cathode electrode; 3-tetrafluoroethylene cover plate; 4-power supply; 5-electrolyte; 6-SiC substrate; 7-graphite threaded rod; 8-conducting wire. DETAILED DESCRIPTION
[0029] The present invention provides a method for improving the quality of SiC single crystal and epitaxial growth. Before the SiC crystal grows, the SiC substrate material is pretreated by electrochemical etching to improve the surface quality of the substrate, avoid the probability of misalignment caused by two-dimensional nucleation on the substrate surface, optimize the nucleation in the early stage of growth, thereby improving the quality of SiC single crystal and epitaxial growth.
[0030] In the present invention, the specific steps of electrochemical etching pretreatment of SiC substrate material are:
[0031] (1) Exposing the growth surface of the SiC substrate to be pretreated and covering the other surface;
[0032] (2) The shielded surface of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode;
[0033] (3) The anode and cathode are placed symmetrically, the silicon carbide substrate is placed in the electrolyte, a power source is connected and energized, and the growth surface of the substrate is electrochemically etched;
[0034] (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.
[0035] In the present invention, the device used for electrochemical etching is as follows Figure 1 As shown, it includes an anode electrode 1, a cathode electrode 2, a tetrafluoroethylene cover plate 3, a power source 4, an electrolyte 5, a SiC substrate 6, a graphite threaded rod 7, and a wire 8, wherein the anode and the cathode are placed symmetrically up and down, the graphite threaded rod 7 and the tetrafluoroethylene cover plate 3 are fixed and adjusted by threads between the two electrodes, the distance between the cathode and the anode is 1-20 cm, the masking surface of the SiC substrate 6 is bonded to the anode electrode 1 by conductive glue or vacuum adsorption, the pre-etched surface is in contact with the electrolyte 5, the graphite threaded rod 7 and the tetrafluoroethylene cover plate 3 are fixed and adjusted by threads between the anode electrode 1 (graphite electrode) and the cathode electrode 2 (graphite electrode), the graphite threaded rod 7 is tightened with the graphite electrodes 1 and 2 for conduction, and the wire 8 is connected to the graphite threaded rod 7 by a conductive clamp for conduction.
[0036] The power supply is powered on, the power supply voltage is 0-50V, the current is 0-500mA, and the hydroxide (OH) is generated by electrolysis of water. - ) gather at the anode, and hydroxide (OH - ) and holes (h + ) forms free radicals ( . OH), the free radical is unstable and easily diffuses to the interface between the anode SiC and the electrolyte, oxidizing SiC to SiO x and CO x , and then the oxidation product SiO x and CO x Dissolved in HF electrolyte. The process can be expressed as:
[0037] 4OH - -4e - →2H 2 O+O 2 ;
[0038] OH - +h + → . OH;
[0039] SiC+4 . OH+O 2 →SiO 2 +CO 2 +2H 2 O;
[0040] SiO 2 +6HF→2H + +SiF 6 2- +2H 2 O.
[0041] In the present invention, the specific steps of electrochemical etching + silicon carbide single crystal growth are as follows:
[0042] Step 1: Expose the growth surface of the SiC substrate to be pretreated and cover the other side of the substrate.
[0043] Step 2: The shielded surface of the substrate is connected to a graphite electrode as an anode, and a graphite electrode or a platinum electrode is selected as a cathode;
[0044] Step 3: The anode and cathode are placed symmetrically, the silicon carbide substrate is placed in an electrolyte with a concentration of 0-60wt%, a power supply is connected, and the growth surface of the substrate is electrochemically etched for 0-5h;
[0045] The electrolyte temperature is controlled at 0-50°C, and auxiliary conditions can be added, such as ultraviolet light irradiation, ultrasonic vibration, etc. The electrolyte type can be neutral (such as NaCl solution), alkaline (such as KOH solution), acidic (such as HF solution). In the present invention, HF solution is preferably selected as the electrolyte.
[0046] Step 4: Soak the electrochemically etched substrate in an electrolyte for 0-12 hours, then soak it in deionized water for several times with ultrasonic vibrations for 0-10 hours, and finally dry it with an inert gas such as Ar or He for later use.
[0047] Step 5: Place the pretreated SiC substrate and high-purity SiC powder in the corresponding crystal growth crucible, tighten the crucible, and set a reasonable crystal growth thermal field (the substrate bonding method is not limited, for example: adhesive bonding, mechanical fixation, chemical fixation, etc., the crystal growth crucible type is not limited, for example: graphite crucible, tantalum carbide crucible, graphite crucible coated with tantalum carbide coating, etc., and the thermal field structure is not limited).
[0048] Step 6: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0049] Step 7: Under vacuum conditions, set the temperature rising program, after heating to 1100-1450°C for 2-6 hours, open the argon gas inlet line (gas flow rate is controlled at 0-5L / min), 0.5-3 hours, increase the pressure to 200-900mbar, under the condition of flowing argon constant pressure, 2-6 hours, increase the temperature to 2000-2300°C, and then under the condition of constant temperature flowing argon, reduce the pressure to 0.1-50mbar within 0.5-50 hours. Under the growth conditions of temperature: 2000-2300°C, pressure: 0.1-50mbar, the crystal grows for 3-15 days.
[0050] Step 8: Before increasing the pressure and lowering the temperature, keep the argon gas inlet open (gas flow rate controlled at 0-5L / min), increase the pressure to 200-900mbar for 0.5-3 hours, and lower the temperature to 700-1400℃ for 10-20 hours, then cool naturally, and the entire crystal growth is completed.
[0051] In the process of SiC epitaxial growth, a substrate with a eutectic orientation is generally used as a seed crystal, and HCl etching is used before epitaxial growth. The purpose of this is to make steps appear on the surface and avoid two-dimensional nucleation on the smooth substrate surface to cause dislocation, thereby improving the epitaxial quality. However, we use electrochemical etching pretreatment to perform controllable electrochemical etching pretreatment before epitaxial growth, which can replace HCl etching, thereby avoiding the introduction of corrosive gases and reducing the requirements for equipment. While being safe, reliable and pollution-free, it can control the depth, size and distribution of the etching pits, thereby better forming a step flow, so that the crystal grows in a step flow manner from the early stage of growth, achieving the purpose of improving the epitaxial quality, and has a more controllable advantage than HCl etching.
[0052] In the present invention, the specific steps of electrochemical etching + SiC epitaxial growth are as follows:
[0053] Step 1: Expose the growth surface of the SiC substrate to be pretreated and cover the other side of the substrate.
[0054] Step 2: The shielded surface of the substrate is connected to a graphite electrode as an anode, and a graphite electrode or a platinum electrode is selected as a cathode;
[0055] Step 3: The anode and cathode are placed symmetrically, the silicon carbide substrate is placed in an electrolyte with a concentration of 0-60wt%, a power supply is connected, and the growth surface of the substrate is electrochemically etched for 0-5h;
[0056] The electrolyte temperature is controlled at 0-50°C, and auxiliary conditions can be added, such as ultraviolet light irradiation, ultrasonic vibration, etc. The electrolyte type can be neutral (such as NaCl solution), alkaline (such as KOH solution), acid (such as HF solution). In the present invention, HF solution is preferably selected as the electrolyte.
[0057] Step 4: Soak the electrochemically etched substrate in an electrolyte for 0-12 hours, then soak it in deionized water for several times with ultrasonic vibrations for 0-10 hours, and finally dry it with an inert gas such as Ar or He for later use.
[0058] Step 5: Fix the pretreated substrate in a CVD epitaxial furnace and heat it to 1500-1700°C. After reaching the reaction temperature, introduce the purified and dried gas raw materials (preferably silane and propane, with a gas flow rate controlled at 0-1 L / min), and introduce high-purity H 2Used as carrier gas (gas flow rate controlled at 50-150 L / min), high purity N 2 (Gas flow rate is controlled at 0-1L / min) used as N-type doping gas or trimethylaluminum as P-type dopant, flowing gas mode, control the growth pressure at 200-500mbar, under the growth conditions of temperature: 1500-1700℃, pressure: 200-500mbar, epitaxial growth for 0 to 10 hours.
[0059] The present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.
[0060] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0061] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.
[0062] Example 1: Electrochemical Etching + PVT Method SiC Single Crystal Growth
[0063] Step 1: The C surface of the SiC substrate is exposed as the growth surface, and the Si surface is connected to the graphite electrode using a conductive glue to ensure complete contact between the SiC substrate and the graphite electrode.
[0064] Step 2: The SiC substrate and graphite electrode are used as anodes and connected to the positive pole of the power supply. The graphite electrode of the same size and thickness is used as cathode and connected to the negative pole of the power supply. The distance between the two electrodes is 6cm. The output voltage of the power supply is 15V and the current is 50mA.
[0065] Step 3: electrochemically etch the SiC substrate with the exposed C surface in a 10 wt% HF electrolyte for 10 minutes, and the temperature of the electrolyte is controlled at 30°C.
[0066] Step 4: Soak the electrochemically etched substrate in an electrolyte for 12 hours, then ultrasonically soak it in deionized water for 2 hours, and finally blow dry it with Ar gas for later use.
[0067] Step 5: Place the pre-treated and bonded SiC substrate and high-purity SiC powder in a graphite crucible, tighten the crucible, and place it in a reasonable crystal growth thermal field. Vacuum the single crystal growth furnace to make the pressure in the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0068] Step 6: Under vacuum conditions, set the temperature rising program, raise the temperature to 1350°C in 3 hours, then open the argon inlet line (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, and under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour. Under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal is grown for 5 days.
[0069] Step 7: Before increasing the pressure and lowering the temperature, keep the Ar gas inlet open (gas flow rate is 1L / min), increase the pressure to 800mbar for 1 hour, and lower the temperature to 1100℃ for 15 hours, then cool naturally, and the entire crystal growth is completed.
[0070] Example 2: Electrochemical Etching + HTCVD SiC Single Crystal Growth
[0071] Step 1: The C surface of the SiC substrate is exposed as the growth surface, and the Si surface is connected to the graphite electrode using a conductive glue to ensure complete contact between the SiC substrate and the graphite electrode.
[0072] Step 2: The SiC substrate and graphite electrode are used as anodes and connected to the positive pole of the power supply. The graphite electrode of the same size and thickness is used as cathode and connected to the negative pole of the power supply. The distance between the two electrodes is 6cm. The output voltage of the power supply is 15V and the current is 50mA.
[0073] Step 3: electrochemically etch the SiC substrate with the exposed C surface in a 10 wt% HF electrolyte for 10 min, and the temperature of the electrolyte is controlled at 30°C.
[0074] Step 4: Soak the electrochemically etched substrate in an electrolyte for 12 hours, then ultrasonically soak it in deionized water for 2 hours, and finally blow dry it with Ar gas for later use.
[0075] Step 5: Fix the pre-treated substrate on the top of the graphite crucible, set the gas transmission hole at the bottom, set the corresponding thermal field, and coat the graphite parts with tantalum carbide coating. Vacuum and leak test the single crystal growth furnace to make the pressure in the furnace reach 10 -6 mbar, 12 hours, pressure fluctuation does not exceed the leakage rate of 5Pa, set the corresponding temperature and pressure control program.
[0076] Step 6: Under vacuum conditions, set the temperature program, and heat to 2300°C for 10 hours. After reaching the reaction temperature, use the bottom gas inlet method to introduce high-purity Ar as carrier gas (gas flow rate controlled at 5L / min), and introduce SiH 4 and C 3 H 8 (gas flow rate is controlled at 0.1 L / min) was used as the reaction gas, in the flowing gas mode, the growth pressure was controlled at 200 mbar, and the crystal was grown for 5 days under the growth conditions of temperature: 2300°C and pressure: 200 mbar.
[0077] Step 7: Before increasing the pressure and lowering the temperature, stop the introduction of the reaction gas, keep the Ar gas inlet open (gas flow rate controlled at 5L / min), increase the pressure to 800mbar for 1 hour, and cool down to 1100℃ in 15 hours, then cool down naturally, and the entire crystal growth is completed.
[0078] Example 3: Electrochemical Etching + SiC Epitaxial Growth
[0079] Step 1: The C surface of the SiC substrate is exposed as the growth surface, and the Si surface is connected to the graphite electrode using a conductive glue to ensure complete contact between the SiC substrate and the graphite electrode.
[0080] Step 2: The SiC substrate and graphite electrode are used as anodes and connected to the positive pole of the power supply. The graphite electrode of the same size and thickness is used as cathode and connected to the negative pole of the power supply. The distance between the two electrodes is 6cm. The output voltage of the power supply is 15V and the current is 50mA.
[0081] Step 3: electrochemically etch the SiC substrate with the exposed C surface in a 10 wt% HF electrolyte for 10 minutes, and the temperature of the electrolyte is controlled at 30°C.
[0082] Step 4: Soak the electrochemically etched substrate in an electrolyte for 12 hours, then ultrasonically soak it in deionized water for 2 hours, and finally blow dry it with Ar gas for later use.
[0083] Step 5: Fix the pre-treated and bonded substrate in a CVD epitaxial furnace and heat it to 1600°C. After reaching the reaction temperature, introduce high-purity H 2 As carrier gas (gas flow rate controlled at 50 L / min), purified and dried silane and propane were introduced as reaction gas (gas flow rate controlled at 0.1 L / min), and high-purity N 2 (the volume flow rate is controlled at 0.05L / min) is used as the doping gas, and in the flowing gas mode, the growth pressure is controlled at 300mbar. Under the conditions of temperature: 1600℃ and pressure: 300mbar, the epitaxial growth is carried out for 1 hour, and then the growth is terminated by cooling down.
[0084] The experimental test of the crystal quality obtained in Example 1 is based on the crystal growth in the same furnace, ensuring that the growth conditions and thermal field are the same, avoiding the errors caused by the poor repeatability of silicon carbide single crystal growth and the fluctuation of growth conditions. The seed crystal is divided into two regions, one half is formed into an etched area by electrochemical pretreatment, and the other half is not treated and is an unetched area. The results are shown in Figure 2 As shown by Figure 2 It can be seen that the half-width at half maximum of the etched area is much smaller than that of the unetched area. The smaller the half-width at half maximum (FWHM), the better the crystal quality, which shows that the method of the present invention has the effect of improving the crystal quality.
[0085] The experimental test of the quality of the SiC epitaxial growth obtained in Example 3 was carried out. The experimental results were obtained by epitaxial growth in the same furnace, ensuring that the growth conditions and thermal field were the same, avoiding the error caused by fluctuations in the growth conditions. The seed crystal was divided into two regions, one half was formed into an etched region by electrochemical pretreatment, and the other half was not treated and was an unetched region. The results are shown in Figure 3 As shown by Figure 3 It can be seen that the half-width at half maximum of the etched area is much smaller than that of the unetched area. The smaller the half-width at half maximum (FWHM), the better the crystal quality. This shows that chemical etching can improve the quality of epitaxy.
[0086] In summary, electrochemical etching pretreatment reduces the nucleation energy of SiC single crystal and epitaxial growth. Whether it is PVT, HTCVD, TSSG method SiC single crystal growth or SiC epitaxial growth, it is more conducive to step flow growth, avoiding the occurrence of two-dimensional nucleation, optimizing nucleation in the early growth stage, and improving the quality of SiC crystals and epitaxy.
[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for improving the quality of SiC single crystal and epitaxial growth, characterized in that: Before SiC crystal growth, the SiC substrate material is pre-treated by electrochemical etching to improve the surface quality of the substrate, avoid the probability of misalignment caused by two-dimensional nucleation on the substrate surface, optimize nucleation in the early stage of growth, and thus improve the quality of SiC single crystal and epitaxial growth.
2. A method for improving the quality of SiC single crystal and epitaxial growth according to claim 1, characterized in that: The specific steps of electrochemical etching pretreatment of the SiC substrate material are: (1) Exposing the growth surface of the SiC substrate to be pretreated and covering the other surface; (2) The shielded surface of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode; (3) The anode and cathode are placed symmetrically, the silicon carbide substrate is placed in the electrolyte, a power source is connected and energized, and the growth surface of the substrate is electrochemically etched; (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.
3. A method for improving the quality of SiC single crystal and epitaxial growth according to claim 2, characterized in that: In the step (2), the substrate masking surface is connected to the graphite electrode by bonding with conductive glue or by vacuum adsorption.
4. A method for improving the quality of SiC single crystal and epitaxial growth according to claim 2, characterized in that: In the step (3), the distance between the cathode and the anode is 1-20 cm, the power supply voltage is 0-50 V, and the current is 0-500 mA.
5. A method for improving the quality of SiC single crystal and epitaxial growth according to claim 2, characterized in that: In the step (3), the electrolyte is an HF solution with a concentration of 0-60wt%, a temperature of 0-50°C, and an electrochemical etching time of 0-5h.
6. A method for improving the quality of SiC single crystal and epitaxial growth according to claim 2, characterized in that: In the step (4), the sample is immersed in the electrolyte for 0-12 hours, and immersed in deionized water for 0-10 hours.
7. A method for improving the quality of SiC single crystal and epitaxial growth according to claim 2, characterized in that: In the step (4), the inert gas is Ar or He.
Citation Information
Patent Citations
Method for rapidly removing sediments on back surface of wafer in epitaxial process of silicon carbide
CN113802184A
SiC step flow low-speed growth method for growing monomer through chemical potential regulation and control under non-equilibrium condition
CN114032616A
Composite silicon carbide substrate and preparation method thereof
CN115101584A
Electrochemical etching device and etching method thereof
CN116288641A
Production process of epitaxial silicon carbide single crystal substrate
US20130217213A1