Cellulose nanofiber and preparation method thereof

By using sodium percarbonate to treat agricultural product processing waste in an alkaline environment, remove impurities and prepare cellulose nanofibers, the problem of green and efficient utilization of agricultural product processing waste is solved, and the efficient preparation and environmentally friendly production of cellulose nanofibers are achieved.

CN119021022APending Publication Date: 2024-11-26INST OF AGRO FOOD SCI & TECH CHINESE ACADEMY OF AGRI SCI
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410906974.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively solve the problem of green and efficient preparation of cellulose nanofibers for agricultural product processing waste, and traditional methods have problems with high energy consumption and use of harmful chemicals.

Method used

Hemicellulose and lignin were removed by one-step treatment of sodium percarbonate, and cellulose nanofibers were prepared by enzymatic decomposition with sodium percarbonate solution, hydrogen peroxide solution, shear and homogenization treatment, and cellulose nanofibers were prepared by using the non-toxicity of sodium percarbonate. The odorless and pollution-free properties achieve cellulose purification in an alkaline environment.

Benefits of technology

It has achieved green and efficient preparation of cellulose nanofibers, with high specific strength, thermal stability and biocompatibility, and is suitable for food packaging, medicine and cosmetics and other fields, with mild reaction conditions, simple operation, economical and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119021022A_ABST
    Figure CN119021022A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of agricultural product processing waste utilization, in particular to a cellulose nanofiber and a preparation method thereof. The preparation method comprises the following steps: by taking an enzymolysis product of agricultural product processing waste as a raw material, treating by adopting a sodium percarbonate solution to obtain cellulose I, and treating the cellulose I by adopting a hydrogen peroxide solution to obtain cellulose II; and then shearing and homogenizing to obtain the cellulose nanofiber. According to the method, hemicellulose and lignin are removed through one-step treatment of sodium percarbonate, and green and efficient preparation of the cellulose nanofibers is achieved. The preparation method provided by the invention is simple in process, low in cost and easy for industrial production, and has huge popularization and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of utilization of agricultural product processing waste, and in particular to a cellulose nanofiber and a preparation method thereof. Background Art

[0002] Agricultural products such as potatoes, corn, wheat, and rice play an important role in ensuring national food security. During the processing of potatoes, corn, wheat, and rice, a large amount of waste such as potato peels, potato residues, potato vines, corn stalks, wheat stalks, and rice husks will be generated. The above wastes are rich in useful components such as cellulose and are ideal raw materials for preparing cellulose nanofibers. However, the above wastes are often directly discarded or a small part is used as feed, which greatly restricts the healthy and sustainable development of the agricultural product processing industry.

[0003] Cellulose nanofibers have become the research focus of advanced materials science due to their excellent physical and chemical properties such as high specific strength, high specific modulus, good thermal stability and biocompatibility. The application range of cellulose nanofibers covers composite materials, paper reinforcement, food packaging, medicine and cosmetics, making them an ideal choice to replace traditional petroleum-based plastics. However, the physical or chemical methods traditionally used to prepare cellulose nanofibers often involve high energy consumption and the use of hazardous chemicals. Therefore, the development of an environmentally friendly and cost-effective production method has become an urgent need to achieve sustainable production of cellulose nanofibers.

[0004] In recent years, domestic and foreign scholars and enterprise technicians have carried out a lot of research and development work on how to make high-value use of agricultural product processing waste: A Chinese patent with publication number CN115029808A discloses a cellulose nanomaterial and a continuous preparation method thereof. The method comprises the following steps: subjecting pulverized agricultural waste to ultrasonic-assisted ethanol solvent extraction to obtain polyphenols and residual peel residue; pre-treating and organic acid hydrolyzing the residual peel residue to obtain cellulose nanocrystals and residual peel residue; and subjecting the residual peel residue to high-pressure homogenization to obtain cellulose nanofibers, thereby realizing the recycling of raw materials.

[0005] A Chinese patent with publication number CN115028746A discloses a method for fully utilizing potato peels and potato residues and its products. Purple sweet potato peels and residues are used as raw materials and are processed by ultrasound-assisted ethanol solvent extraction to obtain anthocyanins and purple sweet potato peels and residues; the purple sweet potato peels and residues are pretreated and subjected to ultrasound-assisted organic acid hydrolysis to prepare cellulose nanocrystals, thereby realizing high-value utilization of the purple sweet potato peels and residues.

[0006] However, the current utilization of agricultural product processing waste mainly focuses on how to achieve full utilization of useful components, while the problem of green and efficient preparation of cellulose nanofibers has not been effectively solved. Summary of the invention

[0007] The present invention utilizes the cellulose-rich property of agricultural product processing waste, uses sodium percarbonate to remove hemicellulose and lignin in one step, and realizes the green and efficient preparation of cellulose nanofibers. Based on this, the following technical solution is proposed.

[0008] The present invention provides a method for preparing cellulose nanofibers, comprising: The enzymatic hydrolysis product of agricultural product processing waste is used as raw material, and cellulose I is obtained by treating it with sodium percarbonate solution, and cellulose I is treated with hydrogen peroxide solution to obtain cellulose II; then the cellulose nanofiber is obtained by shearing and homogenizing.

[0009] In the present invention, sodium percarbonate (2Na2CO3·3H2O2) as a strong oxidant has the advantages of being non-toxic, odorless and non-polluting. It can not only remove reducing substances such as lignin in addition to cellulose in agricultural product processing waste through redox reaction, but also remove hemicellulose therein through the alkaline environment provided by sodium carbonate. In summary, sodium percarbonate can more efficiently remove lignin and other impurities through oxidation under alkaline conditions.

[0010] In some embodiments, the mass ratio of the raw material to the sodium percarbonate solution is 1:(20-80), preferably 1:(20-60), and more preferably 1:(30-50); the concentration of the sodium percarbonate solution is 20-40 g / L.

[0011] In some embodiments, the temperature of the sodium percarbonate solution treatment is 100°C to 140°C, preferably 110°C to 130°C.

[0012] In some embodiments, the sodium percarbonate solution treatment time is 2 to 6 hours, preferably 3 to 5 hours.

[0013] In some embodiments, the concentration of the hydrogen peroxide solution is 100-200 g / L, preferably 150-200 g / L; And / or, the temperature of the hydrogen peroxide solution treatment is 80°C to 100°C; And / or, the treatment time of the hydrogen peroxide solution is 1 to 2 hours.

[0014] In some embodiments, the shearing speed is 8000-12000 r / min, preferably 10000-12000 r / min; and / or the shearing time is 0.5-2 min.

[0015] In some embodiments, the homogenization pressure is 30-50 MPa (preferably 40-50 MPa), and the number of cycles is 3-9 times (preferably 4-9 times).

[0016] When the homogenization pressure is within the above range, it is beneficial to better refine and disperse the cellulose, and ultimately obtain cellulose nanofibers with better performance.

[0017] In some embodiments, the enzyme used to prepare the enzymatic hydrolysate is a thermostable alpha-amylase; And / or, the agricultural product processing waste includes at least one of potato peels, potato residues, potato vines, corn stalks, wheat stalks, and rice husks.

[0018] In some embodiments, the tuber includes but is not limited to sweet potato, potato, cassava.

[0019] In some embodiments, the preparation method comprises the following steps: The enzymatic hydrolysis product of agricultural product processing waste is used as a raw material, treated with a sodium percarbonate solution to obtain a cellulose suspension I, the cellulose suspension I is centrifuged to obtain a precipitate, the precipitate is mixed with water and then subjected to a divergent ultrasonic treatment, and then treated with a hydrogen peroxide solution to obtain a cellulose suspension II, the cellulose suspension II is centrifuged to obtain a precipitate, the precipitate is mixed with water, and then subjected to shearing and homogenization treatment to obtain the cellulose nanofibers.

[0020] The use of divergent ultrasonic treatment can promote better suspension and dispersion of cellulose molecules, thereby enhancing the oxidation ability of hydrogen peroxide on lignin and further improving the purity and bleaching effect of cellulose.

[0021] In some embodiments, the cellulose nanofibers are obtained by freeze-drying after homogenization.

[0022] Preferably, the centrifugal rotation speed is 7000~9000 r / min (preferably 7500~9000 r / min).

[0023] Preferably, the centrifugation time is 5 to 20 min (preferably 15 to 20 min).

[0024] Preferably, the mass ratio of the precipitate to water is 1:20-80 (preferably 1:30-50).

[0025] Preferably, the power of the divergent ultrasonic treatment is 20-60 W / L (preferably 50-60 W / L).

[0026] Preferably, the cellulose suspension II is centrifuged to obtain a precipitate, the precipitate is mixed with water to prepare a suspension with a cellulose concentration of 0.05% to 0.5% (preferably 0.2% to 0.5%), stirred at 200 to 400 r / min for 4 to 8 h, and then sheared and homogenized to obtain the cellulose nanofibers.

[0027] In some embodiments, the method for preparing the raw material comprises: The agricultural product processing waste is dried and then crushed, and mixed with water to obtain a suspension, and then the suspension is mixed with a heat-resistant alpha amylase and enzymolyzed to obtain the enzymolysis product.

[0028] Preferably, the crushed agricultural product processing waste is mixed with water at a mass ratio of 1:10-30 (preferably 1:15-25) to prepare a suspension.

[0029] Preferably, the amount of the thermostable α-amylase used is 5% to 15% (preferably 8% to 10%) of the volume of the suspension.

[0030] Preferably, the enzymatic hydrolysis temperature is 90°C to 100°C, and the enzymatic hydrolysis time is 1 to 2 h.

[0031] Preferably, after the enzymolysis, the enzymolysis product is obtained by centrifugation and drying.

[0032] Preferably, after the enzymatic hydrolysis, the mixture is centrifuged at 7000-10000 r / min for 10-20 min and dried at 45° C.-85° C. to obtain the enzymatic hydrolysis product.

[0033] Furthermore, the present invention provides cellulose nanofibers (CNFs) prepared by any one of the above embodiments.

[0034] Preferably, the cellulose nanofibers have a diameter of 0.5-50 nm (preferably 2-15 nm) and a length of 500-2000 nm (preferably 1000-2000 nm).

[0035] The beneficial effects of the present invention are at least: 1) The method adopted by the present invention has the advantage of a wide range of applications, and can prepare cellulose nanofibers using various types of waste such as agricultural and forestry processing waste as raw materials.

[0036] 2) The sodium percarbonate used in the present invention achieves the purification of cellulose under mild conditions. Specifically, sodium percarbonate decomposes in water to generate hydrogen peroxide and sodium carbonate. Hydrogen peroxide, as a mild oxidant, can effectively remove impurities in cellulose in a moderately alkaline environment (pH 8-10) provided by sodium carbonate. Compared with strong alkaline chemicals (such as sodium hydroxide), sodium percarbonate causes less damage to cellulose itself, which helps to maintain the mechanical strength and chemical stability of cellulose.

[0037] 3) The sodium percarbonate used in the present invention has the advantages of being non-toxic, odorless and non-polluting, and compared with toxic or corrosive chemicals, it helps to reduce environmental pollution in the production process of cellulose nanofibers.

[0038] 4) The cellulose nanofibers in the present invention have a diameter of 0.5-50 nm and a length of 500-2000 nm, exhibit a high specific surface area and a network structure, and have excellent dispersion stability, thermal stability, mechanical strength and biocompatibility, and are widely used in food packaging, medicine, cosmetics and other fields.

[0039] 5) The method adopted by the present invention has mild reaction conditions, simple operation, economy and environmental protection, and is easy to promote on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a process flow chart of an embodiment of the present invention.

[0041] Figure 2 This is a transmission electron microscope image of the cellulose nanofibers prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] The percentage sign "%" involved in the present invention, unless otherwise specified, refers to mass percentage; however, the percentage of a solution, unless otherwise specified, refers to the number of grams of solute contained in 100 mL of solution.

[0044] If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the instruments used, they are all conventional products that can be purchased through regular channels.

[0045] In the following examples of the present invention, the centrifuge used is the GL-21M centrifuge of Shanghai Luxiangyi Centrifuge Instrument Co., Ltd.; the multifunctional reactor used is the MC500 multifunctional reactor of Beijing Century Senlang Experimental Instrument Co., Ltd.; the magnetic stirrer used is the HJ-6 magnetic stirrer of Changzhou Zhongbei Instrument Co., Ltd.; the ultrasonic equipment used is the sh-kudos ultrasonic cleaner of Shanghai Kedao Ultrasonic Instrument Co., Ltd.; the high shear emulsifier used is the I25 high shear emulsifier of IKN Co., Ltd.; the high pressure homogenizer used is the D-3L high pressure homogenizer of PhD Technology Co., Ltd. in the United States. The cellulose kit used is the Beijing Box Biotech cellulose content detection kit.

[0046] The process flow chart of the following embodiments of the present invention is as follows Figure 1 shown.

[0047] Example 1

[0048] This embodiment provides a cellulose nanofiber, and the preparation method thereof comprises the following steps: 1) The crushed sweet potato residue was suspended in water at a mass ratio of 1:20, and 8% by volume of thermostable α-amylase was added. The mixture was reacted in a 95 ℃ water bath for 1.5 h, then centrifuged at 7500 r / min for 15 min, and dried at 75 ℃ for 6 h. 2) The dried residue was mixed with 30 g / L sodium percarbonate solution at a mass ratio of 1:40 in a multifunctional reactor and treated at 120 °C for 4 h to obtain a cellulose suspension I; 3) The cellulose suspension I was centrifuged at 7500 r / min for 15 min to obtain a precipitate, which was mixed with water at a mass ratio of 1:40 and treated with a divergent ultrasonic wave at 50 W / L for 10 min. Then 150 g / L hydrogen peroxide was added and treated at 90 °C for 1.5 h to obtain a cellulose suspension II; 4) The cellulose suspension II was centrifuged at 7500 r / min for 15 min to obtain a precipitate; the precipitate was mixed with water to obtain a suspension with a cellulose concentration of 0.2%, and stirred at 300 r / min for 6 h. Then, the suspension was sheared at 10000 r / min for 1 min, and subjected to 4 high-pressure homogenization cycles at 40 MPa, and cellulose nanofibers were obtained after freeze drying.

[0049] Example 2

[0050] This embodiment provides a cellulose nanofiber, and the preparation method thereof is different from that of embodiment 1 in that: 2) The dried residue was mixed with 30 g / L sodium percarbonate solution in a multifunctional reactor at a mass ratio of 1:20 and treated at 100 °C for 2 h to obtain cellulose suspension I.

[0051] Example 3

[0052] This embodiment provides a cellulose nanofiber, and the preparation method thereof is different from that of embodiment 1 in that: 2) The dried residue was mixed with 30 g / L sodium percarbonate solution in a multifunctional reactor at a mass ratio of 1:60 and treated at 140 °C for 6 h to obtain a cellulose suspension I.

[0053] Comparative Example 1

[0054] This comparative example provides a cellulose nanofiber, and the preparation method thereof is different from that of Example 1 only in that: 2) The dried residue was mixed with 70 g / L potassium hydroxide solution in a multifunctional reactor at a mass ratio of 1:40 and treated at 120 °C for 4 h to obtain a cellulose suspension I.

[0055] Comparative Example 2

[0056] This comparative example provides a cellulose nanofiber, and the preparation method thereof is different from that of Example 1 only in that: 2) The dried residue was mixed with 70 g / L sodium hydroxide solution in a multifunctional reactor at a mass ratio of 1:40 and treated at 120 °C for 4 h to obtain a cellulose suspension I.

[0057] Comparative Example 3

[0058] This comparative example provides a cellulose nanofiber, and the preparation method thereof is different from that of Example 1 only in that: 2) The dried residue was mixed with 200 g / L sodium carbonate solution at a mass ratio of 1:40 in a multifunctional reactor and treated at 120 °C for 4 h to obtain a cellulose suspension I.

[0059] Test example

[0060] The cellulose yield, purity, and microscopic morphology and Zeta potential of the cellulose nanofibers in the examples and comparative examples were analyzed: 1. Cellulose yield

[0061] The final dried sample weight was designated as M2 and the dry weight of the sweet potato residue after initial drying was determined as M1. The yield was calculated as follows: Yield (%) = M2 / M1×100.

[0062] 2. Cellulose purity

[0063] The cellulose test kit was used for the assay. The assay method is as follows: 3 g of sample was mixed with 80% ethanol and treated in a water bath at 90 °C for 20 min, then centrifuged and the supernatant was discarded to obtain crude cell wall. The crude cell wall was soaked in reagent 1 for 15 h, centrifuged and dried and weighed to obtain dry cell wall material. About 5 mg of dry cell wall material was mixed with distilled water, added with concentrated sulfuric acid and treated in an ice water bath, centrifuged and the supernatant was diluted for determination. The determination steps include preparing the working solution (reagent 2 plus reagent 3), adding the sample, distilled water, working solution and concentrated sulfuric acid in sequence according to the instructions of the kit, mixing and treating in a water bath at 95 °C for 10 min, cooling to room temperature, and measuring the absorbance value at a wavelength of 620 nm with a spectrophotometer, and calculating the cellulose content according to the regression equation and formula measured under standard conditions.

[0064] 3. Microscopic morphology of cellulose nanofibers

[0065] A 0.1% suspension of cellulose nanofibers was prepared and coated on a copper grid and then dried at room temperature. Cellulose nanofibers were imaged using a transmission electron microscope with manual emission at 120 kV.

[0066] 4. Zeta potential of cellulose nanofibers

[0067] The cellulose nanofiber suspension was diluted to 1 mg / mL and dispersed under ultrasonic treatment for 5 min, and then the Zeta potential was measured using deionized water as a dispersant. The experimental conditions were set as follows: temperature 25 °C, scattering angle 173, and equilibrium time 3 min.

[0068] The experimental results of cellulose yield and purity are shown in Table 1.

[0069] Table 1

[0070] As can be seen from Table 1, the cellulose yield and purity in the samples of Examples 1 to 3 are both high, while the cellulose yield and purity in the samples of Comparative Examples 1 to 3 are significantly lower than those in the Examples. Among them, the cellulose yield obtained in Example 1 is the highest, which is 7.87±0.08%; the cellulose yield obtained in Comparative Example 3 is the lowest, which is 4.12±0.04%. At the same time, the cellulose purity obtained in Example 1 is the highest, which is 93.29±0.18%; the cellulose purity obtained in Comparative Example 3 is the lowest, which is 79.23±0.36%. Therefore, it can be seen that the cellulose prepared by the method of the present invention has a higher yield and purity.

[0071] The experimental results of the Zeta potential of cellulose nanofibers are shown in Table 2.

[0072] Table 2

[0073] It can be seen from Table 2 that the cellulose nanofiber suspension prepared in Example 1 has the highest Zeta potential, with an absolute value of 40.30±0.88 mV, while the cellulose nanofiber suspension prepared in Comparative Example 3 has the lowest Zeta potential, with an absolute value of 34.20±1.41 mV. Therefore, it can be seen that the cellulose nanofiber suspension prepared by the method of the present invention has higher stability.

[0074] In addition, if Figure 2 As shown, the cellulose nanofibers prepared in Example 1 present an entangled network structure with a diameter of 2-15 nm and a length of 1000-2000 nm.

[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing cellulose nanofibers, characterized in that: include: The enzymatic hydrolysis product of agricultural product processing waste is used as raw material, and cellulose I is obtained by treating it with sodium percarbonate solution, and cellulose I is treated with hydrogen peroxide solution to obtain cellulose II; then the cellulose nanofiber is obtained by shearing and homogenizing.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the raw material to the sodium percarbonate solution is 1:(20-80), preferably 1:(20-60), and more preferably 1:(30-50); the concentration of the sodium percarbonate solution is 20-40 g / L.

3. The preparation method according to claim 1, characterized in that: The temperature of the sodium percarbonate solution treatment is 100°C to 140°C, preferably 110°C to 130°C.

4. The preparation method according to claim 1, characterized in that: The treatment time of the sodium percarbonate solution is 2 to 6 hours, preferably 3 to 5 hours.

5. The preparation method according to claim 1, characterized in that: The concentration of the hydrogen peroxide solution is 100-200 g / L, preferably 150-200 g / L; And / or, the temperature of the hydrogen peroxide solution treatment is 80°C to 100°C; And / or, the treatment time of the hydrogen peroxide solution is 1 to 2 hours.

6. The preparation method according to claim 1, characterized in that: The shearing speed is 8000-12000 r / min, preferably 10000-12000 r / min; and / or the shearing time is 0.5-2 min.

7. The preparation method according to claim 1, characterized in that: The homogenization pressure is 30-50 MPa, and the number of cycles is 3-9 times.

8. The preparation method according to claim 1, characterized in that: The enzyme used to prepare the enzymatic hydrolyzate is a thermostable α-amylase; And / or, the agricultural product processing waste includes at least one of potato peels, potato residues, potato vines, corn stalks, wheat stalks, and rice husks.

9. The preparation method according to any one of claims 1 to 8, characterized in that The following steps are involved: The enzymatic hydrolysis product of agricultural product processing waste is used as a raw material, treated with a sodium percarbonate solution to obtain a cellulose suspension I, the cellulose suspension I is centrifuged to obtain a precipitate, the precipitate is mixed with water and then subjected to a divergent ultrasonic treatment, and then treated with a hydrogen peroxide solution to obtain a cellulose suspension II, the cellulose suspension II is centrifuged to obtain a precipitate, the precipitate is mixed with water, and then subjected to shearing and homogenization treatment to obtain the cellulose nanofibers.

10. Cellulose nanofibers obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for bleaching tossa

    CN101148820A

  • Dietary fiber and method of preparing dispersible tablet

    CN101406294A

  • Method for synchronously producing biological butanol and nano cellulose from sweet sorghum

    CN104651416A

  • Method for preprocessing lignocellulose biomasses by virtue of carbonate and hydrogen peroxide

    CN105154493A

  • Lignocellulose pretreatment method for increasing enzyme hydrolysis rate by oxidation removal of lignin

    CN107164424A