Construction method of fabricated building material with good waterproof performance
Patent Information
- Application Number
- CN202411113507.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
Under the influence of temperature changes and environmental factors, existing polymer waterproofing materials have reduced waterproofing functions, affecting building quality and service life.
Using a new composite waterproofing agent, the waterproofing and shrinkage resistance of concrete is enhanced by the polymerization and coating reaction of acrylylated diphenylsulfone and ethylene slag powder, combined with organic and inorganic materials, and is used for prefabricated building materials. In construction method.
It significantly improves the waterproof performance of building materials, enhances its durability and hollow resistance, and ensures the firmness and durability of the building.
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to a construction method of assembled building materials with good waterproof performance. Background Art
[0002] Prefabricated building materials refer to special materials that are industrially produced and used in prefabricated buildings, and are of excellent quality, energy-saving, environmentally friendly, and have good functions. They include concrete components, steel structure components and wooden structure components produced using modern industrial production technology, integrated cabinets, sanitary ware, doors and windows, curtain walls, integrated decoration materials, smart homes, and other building materials products suitable for prefabricated buildings and their decoration.
[0003] Building waterproofing is the measure taken from the building materials and structure to prevent water from penetrating certain parts of the building. Waterproofing is mostly used on roofs, underground buildings, underground parts of buildings, interior rooms and water storage structures that need waterproofing. According to the different measures and means taken, it is divided into two categories: material waterproofing and structural waterproofing. Material waterproofing relies on building materials to block the passage of water to achieve the purpose of waterproofing or increase the ability to resist leakage, such as waterproofing with coiled materials, waterproofing with coatings, rigid waterproofing of concrete and cement mortar, and waterproofing with clay and lime soil. Structural waterproofing takes appropriate structural forms to block the passage of water to achieve the purpose of waterproofing, such as waterstops and cavity structures.
[0004] Among the various existing waterproof materials, polymer waterproof membrane is the most commonly used material. This material is easy and quick to construct, does not require maintenance in the later stage, has good weather resistance, and is widely used. However, this organic waterproof material hardens, decomposes or other factors due to temperature changes in the placement environment, resulting in reduced waterproof function, which directly affects the quality and service life of the building to a large extent. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a construction method of assembled building materials with good waterproof performance.
[0006] The purpose of the present invention is achieved by adopting the following technical solutions:
[0007] A construction method of an assembled building material with good waterproof performance comprises the following steps:
[0008] (1) Mixing the raw materials in a mixer according to the composition of the prefabricated building materials, and mixing them evenly to obtain concrete slurry; pouring the concrete slurry into a pre-prepared mold, prefabricating and molding after curing, and demolding to obtain a prefabricated component;
[0009] (2) Make corresponding marks on the construction site according to the design drawings, use the positioning device to accurately embed the bolts, and then install the steel structure frame at the location of the embedded bolts and complete the fixation;
[0010] (3) Use a crane to lift the assembled components and connect them to the steel structure frame through the reserved holes in sequence to achieve splicing or installation;
[0011] (4) The same concrete slurry prepared in step (1) is filled into the gaps where the prefabricated components are installed or spliced, as well as the connection gaps between the prefabricated components and the steel structure skeleton. After the curing is completed, the construction is completed.
[0012] Preferably, the components of the prefabricated building material, calculated by weight, include:
[0013] 100 parts of cement, 152-189 parts of coarse aggregate, 121-168 parts of fine aggregate, 8-15 parts of fly ash, 6-12 parts of waterproofing agent, 3-6 parts of expansion agent, 5-10 parts of water reducing agent and 75-95 parts of deionized water.
[0014] Preferably, the cement is silicate cement, and the type is PO 42.5.
[0015] Preferably, the coarse aggregate is rock or sand particles with a particle size range of 4.75-9 mm.
[0016] Preferably, the fine aggregate is rock or sand particles with a particle size ranging from 0.15 to 4.75 mm.
[0017] Preferably, the fly ash is primary fly ash, and the residue passing through a 45 μm square hole sieve is not more than 12%.
[0018] Preferably, the expansion agent is one or more combinations of calcium sulfoaluminate, calcium oxide, aluminum oxide, and aluminum hydroxide.
[0019] Preferably, the water reducer is a polycarboxylic acid high performance water reducer, and the models include one of SP-409, HPEG-2400, TH-928, and SSF-4000.
[0020] Preferably, the preparation method of the waterproofing agent comprises:
[0021] S1. Weigh 4,4'-dihydroxydiphenyl sulfone and dichloromethane, add a small amount of polymerization inhibitor and acid binding agent, and stir in an ice-water bath until uniform to obtain a mixed solution A; add acryloyl chloride dropwise to the mixed solution A, and after the addition is completed, gradually heat it to 30-35°C, keep it warm and stir for 5-10 hours, and after the reaction is completed, filter out the precipitate, wash and dry the filtrate, and then remove the solvent under reduced pressure to obtain a reactant B;
[0022] S2, weighing ultrafine slag powder and deionized water, adding vinyl silane coupling agent dropwise, stirring well, stirring at 50-60° C. for 8-12 hours, then filtering and collecting solids, washing with water and drying to obtain vinyl slag powder;
[0023] S3. Weigh reactant B and solvent ethylene glycol dimethyl ether, mix them, add vinyl slag powder, mix them evenly by ultrasonication, then introduce nitrogen as protective gas, raise the temperature to 50-60°C, add azo initiator, keep warm and stir to react for 20-30h, after the reaction is completed, remove the solvent under pressure, wash with alcohol three times to obtain a waterproofing agent.
[0024] Preferably, during the preparation of the mixed solution A of S1, the mass volume ratio of 4,4'-dihydroxydiphenyl sulfone to dichloromethane is (2.2-2.8) g: (40-60) mL.
[0025] Preferably, in the process of preparing the reactant B in S1, the mass ratio of acryloyl chloride to 4,4'-dihydroxydiphenyl sulfone in the mixed solution A is 0.82-0.96:1.
[0026] Preferably, in S1, the polymerization inhibitor is hydroquinone or p-tert-butylcatechol, and the mass ratio of the polymerization inhibitor to 4,4'-dihydroxydiphenyl sulfone is 0.02-0.08:1.
[0027] Preferably, in S1, the acid binding agent is triethylamine, and the mass ratio of the acid binding agent to 4,4'-dihydroxydiphenyl sulfone is 1.2-1.5:1.
[0028] Preferably, in S2, the vinyl silane coupling agent is vinyl tri(β-methoxyethoxy)silane or vinyl triisopropoxysilane.
[0029] Preferably, in S2, the ultrafine slag powder is S95 grade slag powder; the mass volume ratio of the ultrafine slag powder, vinyl silane coupling agent and deionized water is 1g:(0.2-0.6)g:(10-20)mL.
[0030] Preferably, in S3, the azo initiator is azobisisobutyronitrile or azobisisoheptylnitrile, and the amount of the azo initiator added is 1%-3% of the mass of the reactant B.
[0031] Preferably, in S3, the mass volume ratio of vinylated slag powder, reactant B and solvent ethylene glycol dimethyl ether is 1 g: (0.2-0.6) g: (30-50) mL.
[0032] The beneficial effects of the present invention are:
[0033] 1. The present invention prepares a construction method for assembled building materials with good waterproof performance. During the construction process, the prefabricated assembled components and the subsequent repair and filling are all the same building materials. This has the advantage that the assembled components are more tightly bonded, making the building more solid. In addition, the present invention has also made certain improvements to the composition of the building materials, using a new type of waterproofing agent to enhance the waterproofness of the building materials, while also improving the shrinkage and hollowing phenomenon of the building materials, so that the durability of the building materials is enhanced.
[0034] 2. Most of the existing building material waterproofing agents are inorganic mineral powders or silicone surfactants, which have certain anti-seepage and waterproofing effects, but are prone to reduce the strength and durability of concrete. The present invention prepares a novel composite waterproofing agent combining inorganic and organic, by using bisphenol S (4,4'-dihydroxydiphenyl sulfone) as a raw material, first subjecting it to acryloylation treatment to obtain an acryloyl diphenyl sulfone compound, then mixing it with vinyl slag powder as a monomer, and then initiating a polymerization reaction to obtain a polymer-coated waterproofing agent.
[0035] 3. The waterproofing agent prepared by the present invention combines the advantages of organic materials and inorganic materials, which not only effectively enhances the waterproof performance of concrete building materials, but also enhances its shrinkage resistance and anti-airing performance. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0037] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0038] The present invention will be further described below in conjunction with the following examples.
[0039] Example 1
[0040] A construction method of an assembled building material with good waterproof performance comprises the following steps:
[0041] (1) Mixing the raw materials in a mixer according to the composition of the prefabricated building materials, stirring and mixing them evenly to obtain concrete slurry; pouring the concrete slurry into a pre-prepared mold, curing for 7 days under the conditions of a temperature of 20±3° C. and a relative humidity of 90% or more, prefabricating and molding, and demolding to obtain a prefabricated component;
[0042] (2) Make corresponding marks on the construction site according to the design drawings, use the positioning device to accurately embed the bolts, and then install the steel structure frame at the location of the embedded bolts and complete the fixation;
[0043] (3) Use a crane to lift the assembled components and connect them to the steel structure frame through the reserved holes in sequence to achieve splicing or installation;
[0044] (4) The same concrete slurry prepared in step (1) is filled into the gaps where the prefabricated components are installed or spliced, as well as the connection gaps between the prefabricated components and the steel structure skeleton. After the curing is completed, the construction is completed.
[0045] The components of the above-mentioned prefabricated building materials are calculated by weight and include:
[0046] 100 parts of cement, 171 parts of coarse aggregate, 146 parts of fine aggregate, 12 parts of fly ash, 9 parts of waterproofing agent, 4 parts of expansion agent, 8 parts of water reducing agent and 85 parts of deionized water.
[0047] Among them, cement is silicate cement, model PO 42.5; coarse aggregate is rock or sand and gravel particles with a particle size range of 4.75-9mm; fine aggregate is rock or sand and gravel particles with a particle size range of 0.15-4.75mm; fly ash is first-class fly ash, and the sieve residue passing through a 45μm square hole sieve is not more than 12%; the expansion agent is calcium sulfoaluminate; and the water reducer is polycarboxylic acid high-performance water reducer SP-409.
[0048] Wherein, the preparation method of the waterproofing agent comprises:
[0049] S1. Weigh 4,4'-dihydroxydiphenyl sulfone and dichloromethane, mix them, the mass volume ratio of 4,4'-dihydroxydiphenyl sulfone to dichloromethane is 2.5g:50mL, then add acid binding agent triethylamine and polymerization inhibitor p-tert-butylcatechol, the mass ratio of acid binding agent to 4,4'-dihydroxydiphenyl sulfone is 1.3:1, the mass ratio of polymerization inhibitor to 4,4'-dihydroxydiphenyl sulfone is 0.05:1, stir in an ice water bath until uniform, and obtain a mixed solution A;
[0050] Add acryloyl chloride dropwise to the mixed solution A, the mass ratio of acryloyl chloride to 4,4'-dihydroxydiphenyl sulfone is 0.89:1, the dropping speed is 50 drops / minute, after the dropping is completed, gradually heat to 35°C, keep warm and stir at a speed of 300r / min for 8h, after the reaction is completed, filter out the precipitate, and then wash the filtrate with saturated sodium bicarbonate solution and saturated brine in sequence, the washing is carried out in an extraction manner, after the washing is completed, first dehydrate and dry with anhydrous sodium sulfate, and then remove the solvent under reduced pressure to obtain reactant B;
[0051] S2, weigh S95 grade ultrafine slag powder (manufacturer: Hebei Kaicong Building Materials Technology Co., Ltd.) and mix with deionized water, add vinyl tri(β-methoxyethoxy) silane dropwise, the mass volume ratio of ultrafine slag powder, vinyl tri(β-methoxyethoxy) silane and deionized water is 1g:0.4g:15mL, stir well, stir at 55°C for 10h, then filter and collect the solid, wash with water and dry to obtain vinyl slag powder;
[0052] S3, weigh reactant B and solvent ethylene glycol dimethyl ether, mix them, then add vinyl slag powder, the mass volume ratio of vinyl slag powder, reactant B and solvent ethylene glycol dimethyl ether is 1g:0.4g:40mL, ultrasonically mix them evenly, then introduce nitrogen as protective gas, heat to 55°C, add azobisisobutyronitrile, the addition amount is 2% of the mass of reactant B, keep warm and stir to react for 25h, after the reaction is completed, pressurize to remove the solvent, wash three times with alcohol, and obtain a waterproofing agent.
[0053] Example 2
[0054] A construction method of an assembled building material with good waterproof performance, which is different from Example 1 in that the composition of the assembled building material is slightly different.
[0055] Among them, the components of prefabricated building materials are calculated by weight and include:
[0056] 100 parts of cement, 152 parts of coarse aggregate, 121 parts of fine aggregate, 8 parts of fly ash, 6 parts of waterproofing agent, 3 parts of expansive agent, 5 parts of water reducing agent and 75 parts of deionized water.
[0057] Wherein, the cement is silicate cement, model PO 42.5; the coarse aggregate is rock or sand and gravel particles with a particle size range of 4.75-9 mm; the fine aggregate is rock or sand and gravel particles with a particle size range of 0.15-4.75 mm; the fly ash is first-class fly ash, and the sieve residue passing through a 45 μm square hole sieve is not more than 12%; the expansion agent is calcium oxide; and the water reducing agent is polycarboxylic acid high-performance water reducing agent HPEG-2400. The preparation method of the waterproofing agent is the same as that of Example 1.
[0058] Example 3
[0059] A construction method of an assembled building material with good waterproof performance, which is different from Example 1 in that the composition of the assembled building material is slightly different.
[0060] Among them, the components of prefabricated building materials are calculated by weight and include:
[0061] 100 parts of cement, 189 parts of coarse aggregate, 168 parts of fine aggregate, 15 parts of fly ash, 12 parts of waterproofing agent, 6 parts of expansive agent, 10 parts of water reducing agent and 95 parts of deionized water.
[0062] Wherein, the cement is silicate cement, model PO 42.5; the coarse aggregate is rock or sand and gravel particles with a particle size range of 4.75-9 mm; the fine aggregate is rock or sand and gravel particles with a particle size range of 0.15-4.75 mm; the fly ash is first-class fly ash, and the sieve residue passing through a 45 μm square hole sieve is not more than 12%; the expansion agent is aluminum hydroxide; and the water reducer is polycarboxylic acid high-performance water reducer TH-928. The preparation method of the waterproofing agent is the same as that of Example 1.
[0063] Example 4
[0064] A prefabricated building material with good waterproof performance, which is different from Example 1 in that the preparation method of the waterproofing agent used in the prefabricated building material is different.
[0065] The preparation method of the waterproofing agent comprises:
[0066] S1, weigh 4,4'-dihydroxydiphenyl sulfone and dichloromethane, the mass volume ratio of 4,4'-dihydroxydiphenyl sulfone to dichloromethane is 2.2g:40mL, then add acid binding agent triethylamine and polymerization inhibitor hydroquinone, the mass ratio of acid binding agent to 4,4'-dihydroxydiphenyl sulfone is 1.2:1, the mass ratio of polymerization inhibitor to 4,4'-dihydroxydiphenyl sulfone is 0.02:1, and stir in an ice water bath until uniform, to obtain a mixed solution A;
[0067] Add acryloyl chloride dropwise to the mixed solution A, the mass ratio of acryloyl chloride to 4,4'-dihydroxydiphenyl sulfone is 0.82:1, the dropping speed is 40 drops / minute, after the dropping is completed, gradually heat to 30°C, keep warm and stir at a speed of 200r / min for 5h, after the reaction is completed, filter out the precipitate, and then wash the filtrate with saturated sodium bicarbonate solution and saturated brine in sequence, the washing is carried out in an extraction manner, after the washing is completed, first dehydrate and dry with anhydrous sodium sulfate, and then remove the solvent under reduced pressure to obtain reactant B;
[0068] S2, weighing S95 grade ultrafine slag powder and deionized water, adding vinyl triisopropoxysilane dropwise, the mass volume ratio of ultrafine slag powder, vinyl silane coupling agent and deionized water is 1g:0.2g:10mL, stirring well, stirring at 50°C for 8h, then filtering and collecting the solid, washing with water and drying to obtain vinyl slag powder;
[0069] S3, weigh reactant B and solvent ethylene glycol dimethyl ether and mix, then add vinyl slag powder, the mass volume ratio of vinyl slag powder, reactant B and solvent ethylene glycol dimethyl ether is 1g:0.2g:30mL, ultrasonic mixing is uniform, then nitrogen is introduced as protective gas, the temperature is raised to 50 ℃, azobisisoheptanonitrile is added, the addition amount is 1% of the mass of reactant B, and the reaction is stirred and kept warm for 20h. After the reaction is completed, the solvent is removed under pressure, and the mixture is washed with alcohol three times to obtain a waterproofing agent.
[0070] Example 5
[0071] A prefabricated building material with good waterproof performance, which is different from Example 1 in that the preparation method of the waterproofing agent used in the prefabricated building material is different.
[0072] The preparation method of the waterproofing agent comprises:
[0073] S1. Weigh 4,4'-dihydroxydiphenyl sulfone and dichloromethane, mix them, the mass volume ratio of 4,4'-dihydroxydiphenyl sulfone to dichloromethane is 2.8g:60mL, then add acid binding agent triethylamine and inhibited tert-butyl catechol, the mass ratio of acid binding agent to 4,4'-dihydroxydiphenyl sulfone is 1.5:1, the mass ratio of inhibitor to 4,4'-dihydroxydiphenyl sulfone is 0.08:1, stir in an ice water bath until uniform, and obtain a mixed solution A;
[0074] Add acryloyl chloride dropwise to the mixed solution A, the mass ratio of acryloyl chloride to 4,4'-dihydroxydiphenyl sulfone is 0.96:1, the dropping speed is 60 drops / minute, after the dropping is completed, gradually heat to 35°C, keep warm and stir at a speed of 400r / min for 10h, after the reaction is completed, filter out the precipitate, and then wash the filtrate with saturated sodium bicarbonate solution and saturated brine in sequence, the washing is carried out in an extraction manner, after the washing is completed, dehydrate and dry with anhydrous sodium sulfate, and then remove the solvent under reduced pressure to obtain reactant B;
[0075] S2, weighing S95 grade ultrafine slag powder and deionized water, adding vinyl tri(β-methoxyethoxy) silane dropwise, the mass volume ratio of ultrafine slag powder, vinyl silane coupling agent and deionized water is 1g:0.6g:20mL, stirring well, stirring at 60°C for 12h, then filtering and collecting the solid, washing with water and drying to obtain vinyl slag powder;
[0076] S3, weigh reactant B and solvent ethylene glycol dimethyl ether, mix them, then add vinyl slag powder, the mass volume ratio of vinyl slag powder, reactant B and solvent ethylene glycol dimethyl ether is 1g:0.6g:50mL, ultrasonically mix them evenly, then introduce nitrogen as protective gas, heat to 60°C, add azobisisobutyronitrile, the addition amount is 3% of the mass of reactant B, keep warm and stir to react for 30h, after the reaction is completed, pressurize to remove the solvent, wash with alcohol three times, and obtain a waterproofing agent.
[0077] Comparative Example 1
[0078] A prefabricated building material with good waterproof performance, which is different from Example 1 in that the waterproofing agent used in the prefabricated building material is different. The waterproofing agent used in this comparative example is S95 grade ultrafine slag powder.
[0079] Comparative Example 2
[0080] A prefabricated building material with good waterproof performance, which is different from Example 1 in that the waterproofing agent used in the prefabricated building material is different. The waterproofing agent used in this comparative example is a mixture of 4,4'-dihydroxydiphenyl sulfone and S95 grade superfine slag powder, and the mass ratio of 4,4'-dihydroxydiphenyl sulfone to S95 grade superfine slag powder is 0.6:1.
[0081] Comparative Example 3
[0082] A prefabricated building material with good waterproof performance, which is different from Example 1 in that the waterproofing agent used in the prefabricated building material is different. The waterproofing agent used in this comparative example is a mixture of reactant B (prepared in the same way as S1 in Example 1) and S95 grade ultrafine slag powder, and the mass ratio of reactant B to S95 grade ultrafine slag powder is 0.6:1.
[0083] The building materials prepared in Example 1 and Comparative Examples 1-3 were prefabricated and cured for 28 days at a temperature of 20±3°C and a relative humidity of 90% or more. The tensile strength, flexural strength and shrinkage were tested according to the method of GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete"; the waterproofness was expressed as the impermeability grade, and the detection method was referred to GB 50164-2011; the hollowing rate was the percentage of the area where hollowing occurred under the set conditions (45°C, 75% RH) for 90 days to the total area.
[0084] Table 1 Performance of different prefabricated building materials
[0085] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength(MPa) 49.2 41.5 42.8 45.3 Flexural strength(MPa) 7.24 6.12 6.37 6.78 Shrinkage rate (%) 0.031 0.075 0.056 0.042 Impermeability grade >P12 P10 P10 P12 Hollow rate (%) <2% 4%~5% 2%~3% <2%
[0086] It can be seen from Table 1 that the prefabricated building material prepared in Example 1 of the present invention not only has better waterproofness, but also has a certain degree of improvement in strength, shrinkage resistance and air-drum prevention, indicating that the prefabricated building material prepared in Example 1 of the present invention can simultaneously have the advantages of waterproofness, high strength, shrinkage resistance and air-drum prevention.
[0087] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0088] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A construction method for assembled building materials with good waterproof performance, characterized in that: The following steps are involved: (1) Mixing the raw materials in a mixer according to the composition of the prefabricated building materials, and mixing them evenly to obtain concrete slurry; pouring the concrete slurry into a pre-prepared mold, prefabricating and molding after curing, and demolding to obtain a prefabricated component; (2) Make corresponding marks on the construction site according to the design drawings, use the positioning device to accurately embed the bolts, and then install the steel structure frame at the location of the embedded bolts and complete the fixation; (3) Use a crane to lift the assembled components and connect them to the steel structure frame through the reserved holes in sequence to achieve splicing or installation; (4) The same concrete slurry prepared in step (1) is filled into the gaps where the prefabricated components are installed or spliced, as well as the connection gaps between the prefabricated components and the steel structure skeleton. After the curing is completed, the construction is completed.
2. The construction method of a prefabricated building material with good waterproof performance according to claim 1, characterized in that: The components of the prefabricated building materials are calculated by weight and include: 100 parts of cement, 152-189 parts of coarse aggregate, 121-168 parts of fine aggregate, 8-15 parts of fly ash, 6-12 parts of waterproofing agent, 3-6 parts of expansion agent, 5-10 parts of water reducing agent and 75-95 parts of deionized water.
3. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The cement is silicate cement, and the type is PO 42.
5.
4. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The coarse aggregate is rock or sand and gravel particles with a particle size range of 4.75-9 mm.
5. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The fine aggregate is rock or sand and gravel particles with a particle size range of 0.15-4.75 mm.
6. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The fly ash is first-grade fly ash, and the residue passing through a 45 μm square hole sieve is not more than 12%.
7. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The expansion agent is one or more combinations of calcium sulfoaluminate, calcium oxide, aluminum oxide, and aluminum hydroxide.
8. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The water reducer is a polycarboxylic acid high-performance water reducer, and the models include one of SP-409, HPEG-2400, TH-928, and SSF-4000.
9. The construction method of a prefabricated building material with good waterproof performance according to claim 2, characterized in that: The preparation method of the waterproofing agent comprises: S1. Weigh 4,4'-dihydroxydiphenyl sulfone and dichloromethane, add a small amount of polymerization inhibitor and acid binding agent, and stir in an ice-water bath until uniform to obtain a mixed solution A; add acryloyl chloride dropwise to the mixed solution A, and after the addition is completed, gradually heat it to 30-35°C, keep it warm and stir for 5-10 hours, and after the reaction is completed, filter out the precipitate, wash and dry the filtrate, and then remove the solvent under reduced pressure to obtain a reactant B; S2, weighing ultrafine slag powder and deionized water, adding vinyl silane coupling agent dropwise, stirring well, stirring at 50-60° C. for 8-12 hours, then filtering and collecting solids, washing with water and drying to obtain vinyl slag powder; S3. Weigh reactant B and solvent ethylene glycol dimethyl ether, mix them, add vinyl slag powder, mix them evenly by ultrasonication, then introduce nitrogen as protective gas, raise the temperature to 50-60°C, add azo initiator, keep warm and stir to react for 20-30h, after the reaction is completed, remove the solvent under pressure, wash with alcohol three times to obtain a waterproofing agent.
10. The construction method of a prefabricated building material with good waterproof performance according to claim 9, characterized in that: During the preparation of the mixed solution A of S1, the mass volume ratio of 4,4'-dihydroxydiphenyl sulfone and dichloromethane is (2.2-2.8) g: (40-60) mL; during the preparation of the reactant B of S1, the mass ratio of acryloyl chloride to 4,4'-dihydroxydiphenyl sulfone in the mixed solution A is 0.82-0.96: 1; in S2, the mass volume ratio of ultrafine slag powder, vinyl silane coupling agent and deionized water is 1 g: (0.2-0.6) g: (10-20) mL; in S3, the mass volume ratio of vinylated slag powder, reactant B and solvent ethylene glycol dimethyl ether is 1 g: (0.2-0.6) g: (30-50) mL.