Low-temperature drying method for high-strength and high-modulus polyethylene fiber product
Through the low-temperature drying method, combined with dynamic air pressure regulation, microwave infrared drying and waste heat recovery, the problems of long drying time and thermal damage in traditional high-temperature drying methods are solved, and efficient and low-energy-consuming fiber drying is achieved, protecting the mechanical properties of the fiber.
Patent Information
- Application Number
- CN202411509422.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional high-temperature drying methods lead to long drying time, high energy consumption, and it is difficult to ensure that the internal and external drying of the fibers are easily caused by thermal damage, affecting the mechanical properties, and unable to meet the needs of industrial production.
Low-temperature drying methods are adopted, including pretreatment, dynamic air pressure regulation and air pressure pulse, microwave and infrared drying, combined with waste heat recovery, gradually reduce the air pressure and temperature of the cavity to ensure that the internal and external fibers are dried simultaneously, and reduce thermal damage.
It significantly shortens the drying time, reduces the risk of thermal damage, improves drying efficiency and energy utilization, and ensures the protection and production efficiency of the mechanical properties of the fiber.
Smart Images

Figure CN119022585A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene fiber products, in particular to a low-temperature drying method for high-strength and high-modulus polyethylene fiber products. Background Art
[0002] High-strength and high-modulus polyethylene fiber has become a key material in many high-tech fields due to its excellent mechanical properties. This fiber has extremely high tensile strength and modulus, can withstand great external forces without breaking or deforming, and is particularly suitable for use in harsh environments. In addition, the fiber has excellent wear resistance and is not easy to wear after long-term use, which extends its service life in complex environments. More importantly, high-strength and high-modulus polyethylene fiber has extremely strong chemical corrosion resistance and can maintain the stability of its structure and performance in corrosive environments such as oceans and chemicals. Therefore, it is widely used in fields that require high strength, durability and corrosion resistance, such as aerospace, military protection and marine engineering. For example, in the aerospace field, this fiber is used to manufacture high-performance lightweight composite materials, which can reduce the weight of aircraft and improve fuel efficiency; in military protection, bulletproof vests and protective equipment made of polyethylene fibers can provide excellent protection; in marine engineering, polyethylene fibers are used in high-strength and corrosion-resistant products such as cables and fishing nets to ensure that they can be used for a long time in harsh marine environments without failure.
[0003] However, in the preparation process of high-strength and high-modulus polyethylene fibers, humidity control becomes a crucial step. Since the fiber absorbs a lot of water during the production process, if it is not effectively dried, the moisture in the fiber will cause the product performance to deteriorate, and even cause quality problems in subsequent processing. In order to obtain a final product with excellent performance, the drying step is indispensable. However, traditional drying methods mainly rely on high temperature or room temperature drying in a natural environment. Although these methods are simple, they have several significant problems. First, the drying process takes a long time, and the migration and evaporation of water are slow. Especially in mass production, the long drying cycle greatly reduces the production efficiency. Secondly, high-temperature drying will bring certain risks, especially for heat-sensitive materials such as high-strength and high-modulus polyethylene fibers, high temperature may cause irreversible damage to them, resulting in a decrease in the mechanical properties of the fiber. Excessive temperature may cause changes in the surface or internal structure of the fiber, such as the generation of microcracks or the breakage of molecular chains, which will significantly reduce the mechanical properties of the fiber such as tensile strength and modulus, thereby affecting its performance in the final application.
[0004] Among the existing drying technologies, common drying methods still have many defects. First, the conventional drying time is too long, especially for high-strength and high-modulus polyethylene fibers, the evaporation rate of water is slow. This slow drying usually relies only on a single air pressure or temperature control, which is difficult to effectively promote the migration of water, resulting in low drying efficiency and unable to meet the needs of large-scale industrial production. Secondly, high-temperature drying may cause changes in the internal structure of the fiber. Especially for materials with poor thermal stability, high temperature can easily cause irreversible damage, such as cracks inside the fiber, brittle surface or molecular chain breakage. This thermal damage not only affects the appearance quality of the fiber, but also leads to a significant decrease in its mechanical properties, which in turn affects subsequent use. Furthermore, traditional drying equipment has high energy consumption, and the equipment lacks an effective energy recovery mechanism, resulting in a large amount of energy waste and increased production costs. In modern industry, improving energy efficiency has become a key consideration. How to reduce energy consumption while improving drying efficiency is another major challenge facing companies. Finally, the traditional drying method has poor uniformity, and it is difficult to achieve synchronous drying of the inside and outside of the fiber. It is often the case that the fiber surface is over-dry while the inside is not completely dry, which not only affects the appearance of the fiber, but may also affect the performance of subsequent processing and use.
[0005] Therefore, how to effectively dry the fiber in a low temperature environment, reduce the drying time and ensure the mechanical properties of the fiber has become the focus and difficulty of current fiber drying technology research. Developing a drying method that can be both efficient and protective, which can accelerate the migration of moisture and prevent the fiber from being damaged by heat during the drying process, has become the main goal of technicians. Summary of the invention
[0006] The present invention mainly solves the technical problems existing in the above-mentioned prior art and provides a low-temperature drying method for high-strength and high-modulus polyethylene fiber products.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme, which is a low-temperature drying method for high-strength and high-modulus polyethylene fiber products, comprising the following steps: Step 1: Pre-treat the high-strength and high-modulus polyethylene fiber product, start the vacuum pump, extract the air in the cavity, make the vacuum degree reach the range of 200Pa to 500Pa, start the heater, raise the cavity temperature to 30°C to 40°C, perform preliminary drying, maintain for 10 to 15 minutes, observe that there is no obvious moisture on the fiber surface, and then proceed to the next step; Step 2: Set the initial air pressure in the pretreatment chamber to atmospheric pressure, and gradually reduce the chamber pressure to 100Pa by adjusting the vacuum pump for hot air drying. During the drying period, every 20 minutes, use the vacuum pump to reduce the air pressure to 50Pa and maintain it for 10 minutes, then restore it to 100Pa, and at the same time combine air pressure pulse adjustment to dry for 4 to 8 hours; Step 3: Combine microwave and infrared drying to further strengthen the high-strength and high-modulus polyethylene fiber products at low temperature; Step 4: Recover the waste heat after low-temperature drying is completed; Step 5: Slowly cool the high-strength high-modulus polyethylene fiber product to room temperature and then take it out; Step 6: Quality inspection and storage of high-strength and high-modulus polyethylene fiber products.
[0008] A further improvement of the technical solution of the present invention is that dynamic air pressure regulation and dynamic air pressure pulse regulation are used in step 2, wherein during dynamic air pressure regulation, the hot air circulation system is started to set the temperature of the pretreatment cavity where the fibers are placed at 40°C to 50°C, and the airflow is kept stable.
[0009] A further improvement of the technical solution of the present invention is that in step 2, the air pressure pulse is adjusted to quickly restore the air pressure to standard atmospheric pressure every 30 minutes, maintain it for 5 minutes, and then quickly reduce it to 50Pa, and this operation is repeated multiple times.
[0010] A further improvement of the technical solution of the present invention is that in step 3, the dried fiber is placed in a microwave and infrared environment, the power of the microwave drying device is set to 150W to 300W, the microwave frequency is controlled at 2.45GHz, and the infrared drying device is started at the same time, and the infrared wavelength is set to 2μm to 10μm. In this step, the temperature is controlled at 40°C to 50°C and maintained for 2 to 3 hours, and the evaporation of water is monitored according to the degree of dryness of the fiber.
[0011] A further improvement of the technical solution of the present invention is that in step 4, the waste heat around the fiber, the excess heat generated by the hot air system and the microwave infrared heating system are transported to the pretreatment cavity through a recovery pipeline for reheating through a waste heat recovery system.
[0012] A further improvement of the technical solution of the present invention is that in step 5, after drying is completed, the heating system is turned off, the cooling device is started, the temperature in the cavity is controlled to gradually decrease, and the cooling rate is set to 5°C to 10°C / hour.
[0013] A further improvement of the technical solution of the present invention is that in step 6, a humidity detector is used to detect the moisture content of the fiber to ensure that it is within the specified standard range. If the humidity exceeds the standard or the drying is uneven, the fiber is re-entered into the dynamic air pressure control or microwave infrared drying process for supplementary drying. After confirming the drying quality, the fiber is stored in a moisture-proof environment to ensure its stability during subsequent use.
[0014] A further improvement of the technical solution of the present invention is that, in the pretreatment of step 1, the high-strength and high-modulus polyethylene fiber product is evenly spread on the shelf in the pretreatment cavity. Beneficial Effects
[0015] The present invention provides a low-temperature drying method for high-strength and high-modulus polyethylene fiber products. It has the following beneficial effects: (1) The low-temperature drying method for high-strength and high-modulus polyethylene fiber products accelerates the migration of moisture inside the fiber and reduces the drying time by combining dynamic air pressure regulation with air pressure pulses.
[0016] (2) The low-temperature drying method for high-strength and high-modulus polyethylene fiber products reduces the risk of thermal damage and cracks during the low-temperature drying and slow cooling process, thereby protecting the mechanical properties of the fiber.
[0017] (3) The low-temperature drying method for high-strength and high-modulus polyethylene fiber products and the waste heat recovery system improve energy utilization and reduce overall energy consumption.
[0018] (4) The low-temperature drying method for high-strength and high-modulus polyethylene fiber products combines microwave and infrared drying to ensure that the inside and outside of the fiber are dried synchronously to avoid the phenomenon of over-drying the surface or not drying the inside. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the implementation of the present invention or the technical solution in the prior art, the following is a brief introduction to the drawings required for the implementation or the prior art description. Obviously, the drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0020] Figure 1 It is a flow chart of the present invention; Figure 2 This is the overall layout diagram of the drying equipment of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Low temperature drying method for high strength and high modulus polyethylene fiber products, such as Figure 1-Figure 2 As shown, the following steps are included: Step 1: Preprocessing; The purpose of this step is to preliminarily remove the free moisture on the surface of the high-strength high-modulus polyethylene fiber in preparation for subsequent drying.
[0023] During treatment, first place the fiber product in the pretreatment chamber, control the ambient temperature at 30°C to 40°C, then set the vacuum degree to 200Pa to 500Pa, maintain it for 10 to 15 minutes, and finally adjust the ambient pressure to standard atmospheric pressure conditions.
[0024] The specific processing flow is to spread the fiber evenly on the shelves in the drying room to ensure that the airflow can fully contact the fiber surface, turn on the vacuum pump to extract the air in the cavity to make the vacuum degree reach the range of 200Pa to 500Pa, start the heater, raise the cavity temperature to 30°C to 40°C, perform preliminary drying, maintain for 10 to 15 minutes, and observe that there is no obvious moisture on the fiber surface before proceeding to the next step.
[0025] Step 2: Low-temperature drying combining dynamic air pressure regulation and air pressure pulse technology; The purpose of this step is to accelerate the diffusion of moisture from inside the fiber to the outside, shorten the drying time, and protect the fiber structure at the same time.
[0026] When drying, first set the temperature range to 40°C to 50°C, and then adjust the air pressure change curve as needed, such as gradually reducing it from standard atmospheric pressure to 50Pa to 100Pa, maintaining it for a certain period of time, then restoring the atmospheric pressure and repeating the air pressure change process. The drying time is 4 to 8 hours, which can be adjusted appropriately according to the fiber thickness and moisture content.
[0027] The specific drying process is to set the temperature in the cavity at 40°C to 50°C, start the hot air circulation system, maintain stable airflow, and then perform dynamic air pressure control. The initial air pressure is set to atmospheric pressure, and the cavity air pressure is gradually reduced to 100Pa by adjusting the vacuum pump. Maintain this condition for 2 hours to accelerate the evaporation of surface and internal moisture. During the drying period, every 20 minutes, the air pressure is reduced to 50Pa using the air pressure control system and maintained for 10 minutes before returning to 100Pa.
[0028] Afterwards, on the basis of dynamic air pressure control, an air pressure pulse operation was added to quickly restore the air pressure to the standard atmospheric pressure every 30 minutes, maintain it for 5 minutes, and then quickly reduce it to 50Pa again to promote the diffusion and evaporation of moisture inside the fiber. This operation was repeated 4 times, and the time was adjusted according to the fiber thickness and drying requirements.
[0029] Continue to maintain constant temperature drying for 4 to 8 hours. The specific time is adjusted according to the actual moisture content and thickness of the fiber.
[0030] Step 3: Low temperature drying intensification combining microwave and infrared drying; The purpose of this step is to accelerate the evaporation of water and ensure uniform drying by combining internal heating with an external low temperature environment.
[0031] During drying, the microwave power needs to be adjusted to 150W to 300W, the infrared wavelength needs to be set to 2μm to 10μm, and the drying temperature needs to be maintained at 40°C to 50°C.
[0032] The specific drying process is as follows: after completing the air pressure pulse regulation, start the microwave drying device, set the power to 150W to 300W, adjust the power according to the thickness and moisture content of the fiber, control the microwave frequency at 2.45GHz, and start the infrared drying device at the same time, set the infrared wavelength to 2μm to 10μm to ensure uniform heating of the inside and the surface. At this stage, the temperature is controlled at 40°C to 50°C, combined with the low-temperature drying process, and maintained for 2 to 3 hours, and the evaporation of water is monitored according to the degree of dryness of the fiber.
[0033] During the microwave and infrared drying process, the power and wavelength are adjusted through an automatic feedback system to ensure synchronous evaporation of moisture inside and outside the fiber, preventing over-drying of the fiber surface.
[0034] Step 4: Waste heat recovery and energy saving optimization; The purpose of this step is to reduce energy consumption and improve the overall drying efficiency of the equipment.
[0035] The specific operation process is to turn on the waste heat recovery system during the entire drying process, and use the waste heat around the fibers to reheat the air entering the pretreatment chamber.
[0036] The excess heat generated by the hot air system and microwave infrared heating system is transported to the pretreatment chamber through a recovery pipeline to increase the pretreatment temperature of the next batch of fibers and reduce heating energy consumption.
[0037] Monitor the operating status of the recovery system in real time to ensure that the waste heat recovery rate remains above 70% and save energy.
[0038] Step 5: Cool slowly; The purpose of this step is to protect the fiber structure and prevent cracks or internal stress caused by sudden cooling.
[0039] When cooling, maintain a cooling rate of 5°C to 10°C / hour.
[0040] The specific operation process is that after drying is completed, the heating system is turned off, the cooling device is started, the temperature in the cavity is controlled to gradually decrease, and the cooling rate is set to 5°C to 10°C / hour to avoid fiber shrinkage or surface cracks due to sudden temperature drop.
[0041] When the cavity temperature drops to room temperature, the cavity can be opened to take out the dried fiber.
[0042] Step 6: Quality inspection and storage; The purpose of this step is to ensure that the fibers are dried evenly and avoid over-drying or uneven moisture content.
[0043] The specific operation process is to use a humidity detector to detect the moisture content of the fiber to ensure that it is within the specified standard range. If the humidity exceeds the standard or the drying is uneven, re-enter the dynamic air pressure control or microwave infrared drying process for additional drying. After confirming the drying quality, the fiber is stored in a moisture-proof environment to ensure its stability during subsequent use.
[0044] Embodiment, comparative example and control example design:
[0045] Example 1: Low-temperature drying using dynamic air pressure control and air pressure pulse technology combined with microwave / infrared drying. Dynamic air pressure and air pressure pulse combined with microwave / infrared drying technology can shorten the drying time, ensure drying uniformity, and protect the strength of the fiber.
[0046] Set the temperature to 40°C to 50°C in steps 2 and 3, The air pressure is set to fluctuate from 50Pa to 100Pa. The microwave power was set to 200W. The infrared wavelength is set to 5μm, The drying time was set to 6 hours.
[0047] The implementation result of Example 1 is that the moisture is evenly removed and the fiber strength remains unchanged.
[0048] Comparative Example 1: Low-temperature drying with only dynamic air pressure regulation, without air pressure pulses, was used to verify the role of air pressure pulse technology in accelerating moisture diffusion.
[0049] condition: In step 3, set the temperature to 40°C to 50°C. The air pressure is set to 100Pa constant. The microwave power was set to 200W. The infrared wavelength is set to 5μm, The drying time was set to 8 hours.
[0050] Results of Comparative Example 1: Compared with Example 1, the drying time was prolonged, the water diffusion was slow, and some parts were not completely dried.
[0051] Control Example 1: Use traditional constant temperature drying without combining dynamic air pressure control and air pressure pulse to verify the effect of dynamic air pressure control technology and air pressure pulse on improving drying efficiency.
[0052] The drying condition was set to a constant 50 °C, no air pressure regulation, and a drying time of 10 h.
[0053] Results of Control Example 1: The drying time was significantly prolonged, the outside of the fiber was too dry, and the internal moisture was not completely evaporated, resulting in a decrease in fiber strength.
[0054] Embodiment 2: Combine low-temperature drying with waste heat recovery system to improve energy efficiency and reduce energy consumption through waste heat recovery system.
[0055] The implementation conditions of Example 2 are as follows: the temperature is set to 40°C to 50°C, The air pressure is set to 50Pa to 100Pa. The microwave power was set to 200W. The infrared wavelength is set to 5μm, The drying time was set to 6 hours.
[0056] Results of Example 2: Compared with Example 1, the drying efficiency is similar, but the energy consumption is reduced and the energy utilization rate is improved.
[0057] Comparative Example 2: Low-temperature drying without using a waste heat recovery system to verify the impact of the waste heat recovery system on energy saving.
[0058] The implementation conditions of Comparative Example 2 are as follows: the temperature is set to 40°C to 50°C, and there is no waste heat recovery. The air pressure is set to 50Pa to 100Pa. The microwave power was set to 200W. The infrared wavelength is set to 5μm, The drying time was set to 6 hours.
[0059] Comparative Example 2 Results: The drying time was the same as in Example 2, but the energy consumption was higher.
[0060] Control Example 2: Without using a low-temperature drying system, the temperature is increased only by heating to verify the effect of low-temperature drying on fiber protection.
[0061] The implementation conditions of Control Example 2 are as follows: the temperature is set at 60°C, there is no microwave / infrared heating, no air pressure control, and no waste heat recovery.
[0062] Drying time: 5 hours Results of Control Example 2: Fiber strength decreased significantly, drying was uneven, and cracks appeared in some fibers.
[0063] By comparison: Compared with Comparative Example 1 and Control Example 1, Example 1 verifies the advantages of air pressure pulse and microwave / infrared drying in shortening drying time and improving drying uniformity.
[0064] The comparison between Example 2 and Comparative Example 2 demonstrates the significant impact of the waste heat recovery system on energy saving.
[0065] Control Examples 1 and 2 respectively verify that the traditional drying method has the disadvantages of long drying time and severe fiber damage.
[0066] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A low temperature drying method for high strength and high modulus polyethylene fiber products, comprising the following steps: Step 1: Pre-treat the high-strength and high-modulus polyethylene fiber product, start the vacuum pump, extract the air in the cavity, make the vacuum degree reach the range of 200Pa to 500Pa, start the heater, raise the cavity temperature to 30°C to 40°C, perform preliminary drying, maintain for 10 to 15 minutes, observe that there is no obvious moisture on the fiber surface, and then proceed to the next step; Step 2: Set the initial air pressure in the pretreatment chamber to atmospheric pressure, and gradually reduce the chamber pressure to 100Pa by adjusting the vacuum pump for hot air drying. During the drying period, every 20 minutes, use the vacuum pump to reduce the air pressure to 50Pa and maintain it for 10 minutes, then restore it to 100Pa, and at the same time combine air pressure pulse adjustment to dry for 4 to 8 hours; Step 3: Combine microwave and infrared drying to further strengthen the high-strength and high-modulus polyethylene fiber products at low temperature; Step 4: Recover the waste heat after low-temperature drying is completed; Step 5: Slowly cool the high-strength high-modulus polyethylene fiber product to room temperature and then take it out; Step 6: Quality inspection and storage of high-strength and high-modulus polyethylene fiber products.
2. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In step 2, dynamic air pressure regulation and dynamic air pressure pulse regulation are used, wherein during dynamic air pressure regulation, the hot air circulation system is started to set the temperature of the pretreatment cavity where the fibers are placed at 40°C to 50°C, and the airflow is kept stable.
3. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In step 2, the air pressure pulse is adjusted to quickly restore the air pressure to standard atmospheric pressure every 30 minutes, maintain it for 5 minutes, and then quickly reduce it to 50 Pa. This operation is repeated multiple times.
4. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In the step 3, the dried fiber is placed in a microwave and infrared environment, the power of the microwave drying device is set to 150W to 300W, the microwave frequency is controlled at 2.45GHz, and the infrared drying device is started at the same time, and the infrared wavelength is set to 2μm to 10μm. In this step, the temperature is controlled at 40°C to 50°C and maintained for 2 to 3 hours, and the water evaporation is monitored according to the degree of dryness of the fiber.
5. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In step 4, the waste heat around the fiber, the excess heat generated by the hot air system and the microwave infrared heating system are transported to the pretreatment cavity through a recovery pipeline for reheating by means of a waste heat recovery system.
6. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In step 5, after drying is completed, the heating system is turned off, the cooling device is started, and the temperature in the cavity is controlled to gradually decrease, and the cooling rate is set to 5°C to 10°C / hour.
7. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In step 6, a humidity detector is used to detect the moisture content of the fiber to ensure that it is within the specified standard range. If the humidity exceeds the standard or the drying is uneven, the fiber is re-entered into the dynamic air pressure control or microwave infrared drying process for additional drying. After confirming the drying quality, the fiber is stored in a moisture-proof environment.
8. The low temperature drying method for high strength and high modulus polyethylene fiber products according to claim 1, characterized in that: In the pretreatment of step 1, the high-strength and high-modulus polyethylene fiber product is evenly spread on the shelf in the pretreatment chamber.
Citation Information
Patent Citations
Vacuum microwave drying system based on temperature controlling
CN104792120A
Vacuum drying process and equipment of lithium ion battery raw material
CN107024080A
Micro-negative-pressure low-temperature drying device and drying process thereof
CN107289742A
Vacuum pulse system of wolfberry low-temperature drying machine
CN118318949A
Microwave infrared drying device for grinding fibers
CN218065580U