Method for testing adhesion rate of pressure-sensitive adhesive
By placing pressure-sensitive adhesive on the film and applying gravity, the ratio of the unbounced sample was calculated, and the problem of large initial adhesive force testing error in the film material in the prior art was solved, and the accurate evaluation of the adhesion rate of pressure-sensitive adhesive and the film were achieved. Effective screening of initial viscosity.
Patent Information
- Application Number
- CN202311152037.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2023-09-07
- Publication Date
- 2024-11-26
AI Technical Summary
The existing initial viscosity testing methods are difficult to accurately test film materials such as polyimide films, PET films, etc., especially the initial viscosity testing error of pressure-sensitive adhesives is large, and it is impossible to effectively overcome the film stiffness to stick. The damage is connected.
A pressure-sensitive adhesive rate test method is used to calculate the ratio of the number of samples that have not been opened to evaluate the adhesion rate by placing pressure-sensitive adhesive on the film and applying gravity. The ratio of the number of samples that have not been opened is used to evaluate the adhesion rate. High-temperature vulcanized silicone rubber raw rubber is used to The mixture of MQ silicone resin acts as a pressure sensitive adhesive and ensures the accuracy of the adhesion position through a laser positioning device.
Accurate testing of the initial viscosity of the film is achieved, with good repeatability and easy operation, and is especially suitable for films with smaller viscosity. It can effectively screen samples with higher viscosity and reduce test errors.
Smart Images

Figure CN119023569A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of initial adhesion testing of a pressure-sensitive adhesive, in particular to a method for testing the adhesion rate of a pressure-sensitive adhesive. Background Art
[0002] In the application of adhesive sealing materials, the necessary initial adhesion is required to achieve adhesion to the substrate at room temperature. However, for some film materials such as polyimide film, PET film, polytetrafluoroethylene film, etc., the initial adhesion is quite different from that of metal materials. The commonly used initial adhesion test method is difficult to conduct targeted evaluation of such film materials. The rolling ball method (GB / T 4852-2002) is the most widely used test method. By rolling a steel ball over the sticky surface placed on an inclined plate, the initial adhesion is evaluated based on the maximum size of the steel ball that can be adhered. The equipment of this method is extremely simple, but it cannot conduct targeted testing of film materials such as polyimide film, PET film, etc. The ring method initial adhesion test (GB / T 31125-2014) is to bend the adhesive tape sample into a ring-shaped tape ring with the adhesive surface facing outward, fix it on the tensile machine and make it contact with the surface of the substrate test plate, and form adhesion by the gravity of the rubber ring itself. Then, the rubber ring is peeled off the test plate to test its maximum force. This method can be used for targeted testing of different substrates, but the test error of this method is large, especially for sealing materials with small initial adhesion values, it is difficult to evaluate the accurate value of its initial adhesion. In addition, for some pressure-sensitive adhesives, the viscosity itself is strong, but a certain amount of pressure is required to make them adhere, and their own gravity is not enough to provide enough pressure. The touch adhesion test method (ASTM D-2979) is a test method that simulates finger contact. The probe on the test machine presses the adhesive surface of the pressure-sensitive tape and then pulls it apart to test the maximum separation force required. This method can quantify the viscosity felt by the finger touching the pressure-sensitive tape, but it is also unable to conduct targeted testing of film materials. At the same time, for small initial adhesion values, the test error is large.
[0003] Therefore, it is necessary to design a method for testing the initial adhesion of a pressure-sensitive adhesive to a film. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the initial adhesion test method of the prior art and provide a method for testing the adhesion of a pressure-sensitive adhesive. When a film with a certain stiffness is bonded to a bend using a pressure-sensitive adhesive, it is necessary to overcome the force generated by the stiffness that damages the bonding. The method of the present invention can be used to test the adhesion rate of the pressure-sensitive adhesive, thereby qualitatively determining whether the initial adhesion of the pressure-sensitive adhesive to the film meets the standard.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for testing the adhesion rate of a pressure-sensitive adhesive, the method comprising:
[0007] Take n films, place pressure-sensitive adhesive on the upper part of each film, and bond the lower part of each film to the upper part of each film through the pressure-sensitive adhesive. Apply gravity to the bonded films to obtain n samples. Calculate the ratio of the number of samples that did not bounce off to the total number n, which is the adhesion rate.
[0008] According to an embodiment of the present invention, the flexural modulus of the film is above 2.00 GPa, preferably 2-7 GPa.
[0009] According to an embodiment of the present invention, the film is selected from at least one of polyamide-imide film (bending modulus is 4-7 GPa), polybutylene terephthalate film (bending modulus is 2-4 GPa), polycarbonate film (bending modulus is 2.2-2.5 GPa), polyetheretherketone film (bending modulus is 3.7-4 GPa), polyetherimide film (bending modulus is 3-3.4 GPa), polybutylene terephthalate film (bending modulus is 2.8-3.5 GPa), polyimide film (bending modulus is 2.48-4.1 GPa), polymethyl methacrylate film (bending modulus is 2.5-3.5 GPa), and polystyrene film (bending modulus is 3-3.5 GPa). The bending modulus data of the film are shown in Table 1 below.
[0010] Table 1. Flexural modulus of film materials suitable for the present invention
[0011]
[0012]
[0013] According to an embodiment of the present invention, the shape of the film is rectangular or square, and the size of the film is 2cm×2cm~10×10cm, exemplarily 2.5cm×6cm. The wider the width of the film, the greater the spring force generated by the stiffness, and the higher the viscosity requirement for the pressure-sensitive adhesive.
[0014] According to an embodiment of the present invention, the step of bonding the lower portion of the film to the upper portion of the film via the pressure-sensitive adhesive may be folding the film in half.
[0015] According to an embodiment of the present invention, the pressure-sensitive adhesive is selected from a mixture of high-temperature vulcanized silicone rubber raw rubber and MQ silicone resin, and the mass ratio of the high-temperature vulcanized silicone rubber raw rubber to the MQ silicone resin is 5:0.5-10, and exemplarily is 5:0.5, 5:1, 5:2, 5:3, 5:4, 5:5, 5:6, 5:7, 5:8, 5:9, 5:10.
[0016] According to an embodiment of the present invention, the pressure-sensitive adhesive is placed 1-4 cm away from the top of the film, preferably 1 cm away from the top of the film. In the present invention, the closer the pressure-sensitive adhesive is placed to the center of the film, the greater the rebound force generated by the stiffness, and the higher the viscosity requirement of the pressure-sensitive adhesive.
[0017] According to an embodiment of the present invention, the weight of the pressure-sensitive adhesive is 0.005-0.1 g, exemplarily 0.01 g. The less the weight of the pressure-sensitive adhesive, the more difficult it is to bond, and the higher the viscosity requirement of the pressure-sensitive adhesive.
[0018] According to an embodiment of the present invention, the gravity applied to the bonded film is 0.5-1.5 kg, exemplarily 0.5 kg, 0.6 kg, 0.7 kg, 0.8 kg, 0.9 kg, 1 kg, 1.1 kg, 1.1 kg, 1.2 kg, 1.3 kg, 1.4 kg, and 1.5 kg.
[0019] According to an embodiment of the invention, the time for applying gravity is 1-20 s, preferably 2-10 s, exemplarily 2 s, 3 s, 4 s, 5 s, 6 s, 7 s, 8 s, 9 s, 10 s.
[0020] According to an embodiment of the invention, the method comprises counting the number of samples that did not pop open within 1-20 minutes, preferably within 1-10 minutes, exemplarily within 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, and 10 minutes.
[0021] According to an embodiment of the invention, n is 10 or more, preferably 10-30.
[0022] As an exemplary embodiment of the present invention, the test method of the pressure-sensitive adhesive adhesion rate is as follows:
[0023] Take more than 10 square films, place pressure-sensitive adhesive on the upper part of each film, fold them in half, press them with a 1kg weight for 5s, and then release them. Observe the number of samples that have not bounced after 1min and 5min, and calculate the percentage of this number to the total number, which is the adhesion rate.
[0024] In the present invention, the percentages of the number of samples that did not bounce off after 1 minute and after 5 minutes are counted. The former is a targeted test of the initial adhesion, and the latter can be used as a reference for the adhesive performance.
[0025] According to the implementation scheme of the invention, when the ratio of the number of samples that did not pop open to the total amount n is not less than 90%, the initial adhesion of the pressure-sensitive adhesive to the film is qualified.
[0026] According to the implementation scheme of this method, the pressure-sensitive adhesive is placed through a pressure-sensitive adhesive placement plate; the placement plate includes a placement template and a laser positioning device;
[0027] The placement template is used for placing the film;
[0028] The placement template is located directly below the laser light source of the laser positioning device.
[0029] In the present invention, the position where the pressure-sensitive adhesive is placed has a great influence on the adhesion rate. The pressure-sensitive adhesive placement plate can ensure that the adhesive sample is placed in the same position, so that the adhesion rate test result is reliable and repeatable.
[0030] Beneficial effects of the present invention:
[0031] The test method of the present invention can test the initial adhesion performance of the pressure-sensitive adhesive to the film based on the film itself, has good repeatability and is easy to operate. In particular, for films with low initial adhesion, the difference in adhesion rates can be compared to screen samples with higher initial adhesion. In addition, the device is easy to manufacture, does not require the addition of precision components such as sensors, and has low requirements on the use environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a diagram of the placement of the pressure-sensitive adhesive of the present invention and a schematic diagram of the bending of the film.
[0033] Figure 2 It is a film and pressure sensitive adhesive template.
[0034] Figure 3 It is a diagram of a laser-assisted pressure-sensitive adhesive placement device;
[0035] Figure 3 In the figure, 1 is a laser light source. DETAILED DESCRIPTION
[0036] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0037] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0038] Example 1
[0039] Add 50g of high temperature vulcanized silicone rubber (sample 1) to a two-roll mixer, and then add 10g, 25g, and 50g of MQ silicone resin respectively. Mix well and take out, and name them as sample 2, sample 3, and sample 4 respectively. Take 0.01g of each group of samples (sample 1, sample 2, sample 3, and sample 4) and place them on a 6cm×2.5cm polyimide film (bending modulus of 3.1GPa). Use a template and laser to assist in positioning 1cm away from the upper edge. After placement, press with a 1kg weight for 5s and then release. The placement position and state of the pressure-sensitive adhesive after bending are shown in Figure 1. Figure 1 As shown. In this way, 10 samples were prepared for each group of samples, and the number of samples that bounced off after 1 minute and 5 minutes was observed. The results are shown in Table 1. With the increase in the amount of MQ silicone resin added, the 1-minute adhesion rate increased significantly. The adhesion rates of samples 3 and 4 were both above 90%. The two pressure-sensitive adhesive samples had good initial adhesion to the polyimide film. However, the adhesion rate of most pressure-sensitive adhesive samples after 5 minutes was not high because the sample cohesion was insufficient. The cohesion of the pressure-sensitive adhesive should be improved to improve its bonding performance.
[0040] The pressure-sensitive adhesive is placed through a pressure-sensitive adhesive placement plate; the placement plate includes a placement template ( Figure 2 ) and laser positioning device ( Figure 3 );
[0041] The placement template is used for placing the film;
[0042] The placement template is located directly below the laser light source 1 of the laser positioning device. The position of the pressure-sensitive adhesive on the film is determined by the laser light source 1 of the laser positioning device, and the pressure-sensitive adhesive is manually placed there.
[0043] Evaluation criteria for initial adhesion:
[0044] If the adhesion rate is 0-59%, the initial adhesion is poor;
[0045] If the adhesion rate is 60-89%, the initial adhesion is good;
[0046] If the adhesion rate is not less than 90%, the initial adhesion is excellent.
[0047] Table 1 Test results of adhesion rate of pressure sensitive adhesive to silicone rubber
[0048]
[0049] In Table 1, Sample 1 is used as a comparative sample.
[0050] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for testing the adhesion rate of a pressure-sensitive adhesive, characterized in that: The method is: Take n films, place pressure-sensitive adhesive on the upper part of each film, and bond the lower part of each film to the upper part of each film through the pressure-sensitive adhesive. Apply gravity to the bonded films to obtain n samples. Calculate the ratio of the number of samples that did not bounce off to the total number n, which is the adhesion rate.
2. The method according to claim 1, characterized in that The bending modulus of the film is greater than 2.00 GPa; The film is selected from at least one of polyamideimide film, polybutylene terephthalate film, polycarbonate film, polyetheretherketone film, polyetherimide film, polybutylene terephthalate film, polyimide film, polymethyl methacrylate film and polystyrene film.
3. The method according to claim 1, characterized in that: The shape of the film is rectangular or square, and the size of the film is 2cm×2cm to 10×10cm; The step of bonding the lower portion of the film to the upper portion of the film via the pressure-sensitive adhesive may be folding the film in half.
4. The method according to claim 1, characterized in that: The pressure-sensitive adhesive is selected from a mixture of high-temperature vulcanized silicone rubber and MQ silicone resin, and the mass ratio of the high-temperature vulcanized silicone rubber to the MQ silicone resin is 5:0.5-10.
5. The method according to claim 1, characterized in that The pressure-sensitive adhesive is placed 1-4 cm away from the top of the film; The weight of the pressure-sensitive adhesive is 0.005-0.1 g.
6. The method according to claim 1, characterized in that The gravity applied to the bonded film is 0.5-1.5kg; The gravity is applied for 1-20 seconds.
7. The method according to claim 1, characterized in that The method comprises: counting the number of samples that did not pop open within 1-20 minutes.
8. The method according to claim 1, characterized in that n is 10 or more.
9. The method according to claim 1, characterized in that: When the ratio of the number of samples that did not bounce off to the total amount n is not less than 90%, the initial adhesion of the pressure-sensitive adhesive to the film is qualified.
10. The method according to claim 1, characterized in that The pressure-sensitive adhesive is placed on a pressure-sensitive adhesive placement plate; the placement plate includes a placement template and a laser positioning device; The placement template is used for placing the film; The placement template is located directly below the laser light source of the laser positioning device.