Nanoimprint photoresist and preparation method thereof
Patent Information
- Application Number
- CN202411021684.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-26
AI Technical Summary
[0003]本申请提供了一种纳米压印光刻胶及其制备方法,旨在解决现有的光刻胶的抗蚀刻性能和刻蚀选择比较低,从而影响了光学性能的问题
[0008] This application provides a nanoimprint photoresist and a preparation method thereof, which utilizes a cage polysilsesquioxane oligomer and a monofunctional functional monomer with an alicyclic structure to react, so that the prepared nanoimprint photoresist The imprinting photoresist has a POSS structure and an alicyclic structure, which enhances the oxygen plasma etching resistance of the nanoimprinting photoresist. The CP dry etching process has a high etching selectivity ratio, and can also make the prepared nanoimprint photoresist have low surface energy, high Young's modulus and high hardness. During the imprinting process Has good release, fidelity and resolution.
Smart Images

Figure CN119024644A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of nanoimprint technology, and in particular to a nanoimprint photoresist and a preparation method thereof. Background Art
[0002] Nano-imprinting (NIL) is a process of transferring the microstructure of a master onto a wafer. For ultraviolet nano-imprinting, the performance of the photoresist has a great influence on the performance parameters such as the replication accuracy of the imprinted pattern, the pattern defect rate, and the etching selectivity when the pattern is transferred to the substrate. Especially after photocuring, it is necessary to use a plasma etching process to remove the excess photoresist, so the photocured photoresist also needs to meet the requirements of being able to resist oxygen plasma etching. However, at present, nano-imprint photoresist has low adhesion to the substrate, and when there is less residual adhesive for imprinting, the structure is prone to fall off, and there is photoresist residue on the template after imprinting; the adhesion to the template adhesive is large, and the high fidelity and resolution of the imprinted pattern are affected; the etching resistance and selectivity of the photoresist are relatively low, thereby affecting the optical performance. Summary of the invention
[0003] The present application provides a nanoimprint photoresist and a preparation method thereof, aiming to solve the problem that the etching resistance and etching selectivity of the existing photoresist are relatively low, thereby affecting the optical performance.
[0004] In a first aspect, the present application provides a nanoimprint photoresist, which includes: a cage-type polysilsesquioxane oligomer, a monofunctional monomer, an organic silane, an auxiliary agent, a photoinitiator and an organic solvent.
[0005] In a second aspect, the present application provides a method for preparing a nanoimprint photoresist, the preparation method comprising:
[0006] Provide cage-type polysilsesquioxane oligomers, monofunctional monomers, organosilanes, additives, photoinitiators and organic solvents;
[0007] The nanoimprint photoresist is prepared by using the cage-type polysilsesquioxane oligomer, monofunctional monomer, organic silane, auxiliary agent, photoinitiator and organic solvent.
[0008] The present application provides a nanoimprint photoresist and a preparation method thereof, which utilizes a cage-type polysilsesquioxane oligomer and a monofunctional monomer with an alicyclic structure to react, so that the prepared nanoimprint photoresist has a POSS structure and an alicyclic structure, thereby enhancing the oxygen plasma etching resistance of the nanoimprint photoresist, having a higher etching selectivity in an ICP dry etching process, and enabling the prepared nanoimprint photoresist to have low surface energy, high Young's modulus and high hardness, and having good demolding effect, fidelity and resolution in the imprint process. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0010] Figure 1 This is a schematic diagram of the chemical reaction of a fluorine-modified caged silsesquioxane oligomer provided in an embodiment of the present application;
[0011] Figure 2 It is a schematic flow chart of an embodiment of a method for preparing a nanoimprint photoresist provided in an embodiment of the present application;
[0012] Figure 3 It is a schematic flow chart of another embodiment of a method for preparing a nanoimprint photoresist provided in an embodiment of the present application;
[0013] Figure 4 It is a flow chart of another embodiment of a method for preparing a nanoimprint photoresist provided in an embodiment of the present application. DETAILED DESCRIPTION
[0014] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0015] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0016] It should also be understood that the terms used in this application specification are only for the purpose of describing specific embodiments and are not intended to limit the application. As used in this application specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0017] It should be further understood that the term “and / or” used in the specification and appended claims refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0018] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0019] For UV nanoimprinting technology, the main components and application performance of the photoresist that matches it are mostly vague, which brings difficulties to users and is expensive. Most of these photoresists still have a problem, that is, the cleaning of the template. Due to the micro-nano structure on the surface of the template, the photoresist after imprinting is easy to remain on the template due to the wedging effect between the micro-nano structure of the template and the template, or due to the high van der Waals force generated by the huge surface area of the template, thereby contaminating the template. Therefore, after a period of imprinting, the template needs to be cleaned before it can be used again. However, once the existing photoresist remains on the template, these residues are difficult to be thoroughly cleaned by chemical methods, and the residues will accumulate more and more as the number of imprinting increases, eventually making the expensive template unusable due to excessive residues. There are eight performance requirements that UV nanoimprint photoresist must meet during the imprint and etching processes, namely, low viscosity of the photoresist, low surface roughness of the photoresist on the substrate, low UV exposure during photoresist curing, greater adhesion of the photoresist to the substrate than to the template, high fidelity and high resolution of the imprinted pattern, no photoresist residue on the template after imprinting, excellent etching resistance of the photoresist, and one-time rapid cleaning of unqualified patterns.
[0020] Therefore, the key to UV nanoimprinting is photoresist, whose performance has a great influence on the replication accuracy of the imprinted pattern, the defect rate of the pattern, and the etching selectivity when the pattern is transferred to the substrate. At present, UV nanoimprinting photoresist has low adhesion on the substrate, and when there is less residual glue in the imprinting, the structure is prone to fall off, and there is photoresist residue on the template after imprinting; the adhesion with the soft template glue is large, resulting in the high fidelity and resolution of the imprinted pattern being affected; the etching resistance and etching selectivity are relatively low. Therefore, the photoresist for UV nanoimprinting should have the properties of being able to undergo photocuring cross-linking reaction under UV light irradiation, and low viscosity, easy flow, good wetting of the mold, etc. The photoresist can quickly fill the gap between the mold and the substrate under the action of capillary absorption. At the same time, the photoresist should have the property of low surface energy, mainly that the photoresist should not adhere to the mold surface after UV exposure and curing, so as not to affect the quality of pattern transfer. Another requirement is that the cured photoresist can resist oxygen plasma etching. After light curing, the excess photoresist must be removed by plasma etching. In summary, it is of great significance to develop a photoresist suitable for ultraviolet nanoimprinting, which can achieve rapid imprinting and etching, and can quickly and thoroughly clean the template once it is contaminated.
[0021] The embodiment of the present application provides a nanoimprint photoresist, which includes a cage-type polysilsesquioxane oligomer, a monofunctional monomer with an alicyclic structure, an organic silane, an auxiliary agent, a photoinitiator and an organic solvent.
[0022] Wherein, cage type polysilsesquioxane oligomer can be the oligomer of cage type polysilsesquioxane (poly l yhedra lo ligomer ic sil sesquioxane, POSS). POSS structure is the inorganic kernel that is composed of the silicon oxygen skeleton that Si-O is connected alternately, and its shape is like a "cage", and its three-dimensional size is between 1-3nm, and wherein the distance between Si atoms is 0.5nm, and the distance between R groups is 1.5nm, and belongs to nano compound. Monofunctional functional monomer can be the monofunctional functional monomer that comprises alicyclic structure, and the monofunctional functional monomer with alicyclic structure is a class of monofunctional functional monomer that organic chemistry classification obtains by the different arrangement of carbon skeleton. Its molecule contains the carbocyclic ring that is connected by 3 or more carbon atoms, and between two adjacent carbon atoms in the ring can be single bond, double bond or triple bond, and the number of rings can be one or more. The difference of the structure of the ring and the number makes the monofunctional functional monomer with alicyclic structure have different chemical properties. The carbon atoms on the ring can also be connected to chemical functional groups, such as amino, carboxyl, hydroxyl, carbon-carbon double bond, carbon-carbon triple bond, etc. Different functional groups have different chemical properties. Such monofunctional monomers include alicyclic hydrocarbons and their derivatives.
[0023] Exemplarily, the monofunctional monomer may be a monofunctional monomer with an alicyclic structure, and the alicyclic structure may be introduced on the side chain in the reaction with the cage-type polysilsesquioxane oligomer. Since ICP dry etching uses plasma etching, specifically using some neutral gases such as CF4, etc., by introducing it into the gas discharge region, free radical active substances are generated by ionization or decomposition, and these free radicals are highly active and are easy to contact with the material on the etching surface to chemically react and cause the material to peel off. The electronic structure of the compound with an alicyclic structure is very stable, the electron cloud density is very small, and the plasma resistance is relatively large. The active free radicals generated by ionization are difficult to capture the electrons therein and cause structural damage. On the contrary, the silicon base is a highly active single substance, which is easily attacked by free radicals in the plasma atmosphere and chemically reacts. The generated product is SiF4, which is a gas and leaves the silicon base surface, resulting in a sharp decrease in the surface product concentration and accelerating the reaction, and finally forming a higher etching selectivity ratio for the nanoimprint photoresist.
[0024] Exemplary, organosilane can be ultraviolet (UV) reactive organosilane, which can promote the adhesion of nanoimprint photoresist to substrate, avoid the film from detaching from the substrate during the imprint process, and avoid the migration of free coupling agent due to the reaction. The auxiliary agent plays the role of wetting and leveling, so that the photoresist can wet the substrate well when spin-coated on the wafer surface, thereby obtaining a film with uniform thickness and smooth surface. Photoinitiator is mainly used to adjust the curing rate and curing degree of the system. Solvent is mainly used to adjust the viscosity and volatilization rate of the system, which is convenient for controlling the thickness and surface flatness of the film during the spin-coating process.
[0025] The embodiment of the present application provides a nanoimprint photoresist, which utilizes a cage-type polysilsesquioxane oligomer and a monofunctional functional monomer to react, so that the prepared nanoimprint photoresist has a POSS structure and an alicyclic structure, thereby enhancing the oxygen plasma etching resistance of the nanoimprint photoresist, having a higher etching selectivity in an inductively coupled plasma (ICP) dry etching process, and can also make the prepared nanoimprint photoresist have low surface energy, high Young's modulus and high hardness, and have good demolding effect, fidelity and resolution in the imprint process. At the same time, the viscosity of the nanoimprint photoresist is 3.5-15mPa.s, the fluidity is good, the wetting and leveling effect on the substrate is good, a film layer with uniform thickness can be obtained, and the stability is good.
[0026] In some embodiments, the nanoimprint photoresist further comprises a multifunctional acrylate monomer and / or a multifunctional vinyl ether monomer. Since the nanoimprint photoresist contains a multifunctional acrylate monomer and / or a multifunctional vinyl ether monomer, the compatibility between the components in the system can be enhanced, and a photoresist with good stability can be obtained.
[0027] For example, the multifunctional acrylate monomer may be a difunctional acrylate monomer, and the multifunctional vinyl ether monomer may be a difunctional vinyl ether monomer, which can enhance the compatibility of the system and also adjust the film-forming property of the system and the adhesion to the substrate.
[0028] In some embodiments, by weight percentage, the content of cage-type polysilsesquioxane oligomer is 15%-30%, for example: 15%, 20%, 25%, 30%, etc.; the content of monofunctional functional monomer is 5%-10%, the content of multifunctional monofunctional functional monomer and / or multifunctional vinyl ether monomer is 5%-10%, for example: 5%, 7%, 8%, 10%, etc.; the content of organosilane is 1%-5%, for example: 1%, 2%, 3%, 5%, etc.; the content of auxiliary agent is 1%-3%, for example: 1%, 2%, 3%, etc.; the content of photoinitiator is 1%-3%, for example: 1%, 2%, 3%, etc.; the content of organic solvent is 50%-70%, for example: 50%, 55%, 60%, 70%, etc.
[0029] It should be noted that if the nanoimprint photoresist does not include multifunctional acrylate monomers and / or multifunctional vinyl ether monomers, the content of these materials can be replaced by organic solvents.
[0030] Since nanoimprint photoresist is mainly based on cage-type polysilsesquioxane oligomers, its proportion is relatively high; monofunctional functional monomers are used to provide alicyclic structures, so their proportion is relatively low; multifunctional monofunctional functional monomers and / or multifunctional vinyl ether monomers are used to enhance the compatibility of the system, and can also adjust the film-forming properties of the system and adhesion to the substrate, so their proportion is relatively low. Organosilanes, additives and photoinitiators mainly play an auxiliary role, so they can be added in appropriate amounts. Organic solvents are mainly used to adjust the viscosity and volatilization rate of the system, so their proportion is relatively high.
[0031] Exemplarily, cage-type polysilsesquioxane oligomers may account for 25% of the nanoimprint photoresist, monofunctional functional monomers may account for 8% of the nanoimprint photoresist, multifunctional monofunctional functional monomers and / or multifunctional vinyl ether monomers may account for 7% of the nanoimprint photoresist, organosilane may account for 3% of the nanoimprint photoresist, additives may account for 1% of the nanoimprint photoresist, photoinitiators may account for 1% of the nanoimprint photoresist, and organic solvents may account for 55% of the nanoimprint photoresist.
[0032] In some embodiments, the cage polysilsesquioxane oligomer can be selected from any one or more of fluorine-modified cage polysilsesquioxane oligomers, cage polysilsesquioxane oligomers having epoxy groups on the side chains, cage polysilsesquioxane oligomers having acryloxypropyl groups on the side chains, and cage polysilsesquioxane oligomers having methacryloxypropyl groups on the side chains.
[0033] like Figure 1 As shown, illustratively, the cage-type polysilsesquioxane oligomer can be reacted with a silane coupling agent including an acid bond structure and a silane coupling agent including a fluorine-based structure to prepare a fluorine-modified cage-type silsesquioxane oligomer (MA-F-POSS). The nanoimprint photoresist provided by the present application introduces a fluorine-modified cage-type silsesquioxane oligomer, so that the photoresist has low surface energy, high Young's modulus and high hardness, and has good demolding effect, fidelity and resolution during the imprint process.
[0034] It should be noted that the cage-type polysilsesquioxane oligomer can be any oligomer that can provide a POSS structure. Preferably, the best effect is achieved when a fluorine-modified cage-type silsesquioxane oligomer is selected, which can make the nanoimprint photoresist have low surface energy, high Young's modulus and high hardness, and have good demolding effect, fidelity and resolution during the imprint process.
[0035] In some embodiments, the monofunctional functional monomer can be selected from any one or more of isobornyl methacrylate, 2-methyl-2-adamantyl methacrylate, 3-hydroxy-1-adamantyl methacrylate, 2,6-sultone-5-norbornyl methacrylate, (1'-methylcyclopentyl-1-cyclopentyl) methacrylate, α-(γ-butyrolactone) methacrylate, 3-oxo-4,10-dioxa-tricyclo[5.2.1.02,6]dec-8-yl methacrylate, 3-hydroxy-1-adamantyl methacrylate, (2,2-dimethyl-1,3-dioxolane-4-methyl) methacrylate, [bis(2,2-dimethyl-1,3-dioxolane)-4-methyl] methacrylate, norbornene, norbornene-maleic anhydride, norbornene-sulfur dioxide, and vinyl ether-maleic anhydride ester.
[0036] Illustratively, the monofunctional monomers provided above all include an alicyclic structure, which can react with cage-like silsesquioxane oligomers to make the nanoimprint photoresist have both a POSS structure and an alicyclic structure, thereby enhancing the resistance to oxygen plasma etching and having a higher etching selectivity during ICP dry etching.
[0037] In some embodiments, the multifunctional vinyl ether monomer includes: one or more of hydroxybutyl vinyl ether, triethylene glycol divinyl ether, 1,4-cyclohexyl dimethanol divinyl ether, and butyl vinyl ether; the multifunctional acrylate monomer includes: one or more of 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, 4(ethoxylated)pentaerythritol tetraacrylate, and pentaerythritol tetraacrylate.
[0038] Illustratively, the multifunctional vinyl ether monomer and / or multifunctional acrylate monomer provided above can enhance the compatibility of the components in the nanoimprint photoresist, and can also adjust the film-forming property of the system and the adhesion to the substrate.
[0039] In some embodiments, the organosilane can be selected from any one or more of γ-(methacryloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltriethoxysilane, γ-(methacryloxy)propyltriethoxysilane, methacryloxymethyltriethoxysilane, 3-methacryloxypropyltri(methoxyethoxy)silane, methacryloxypropyltri(dimethylsiloxy)silane, γ-(acryloxy)propyltrimethoxysilane, γ-(acryloxy)propyltriethoxysilane, allyltri(trimethylsiloxy)silane, 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, and N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane.
[0040] Illustratively, the organosilanes provided above can promote adhesion to the substrate, prevent the film from detaching from the substrate during the imprinting process, and prevent the migration of free coupling agents.
[0041] In some embodiments, the additive can be any one or more of BYK333, BYK3550, BYK302, BYK3500, BYK3530, BYK3570, Deqian 407, Deqian 410, Deqian 411, Deqian 432, Deqian 435, and Deqian 455.
[0042] Exemplarily, the auxiliary agents provided above can all play a role in wetting and leveling, so that the photoresist can well wet the substrate when spin-coated on the wafer surface, thereby obtaining a film layer with uniform thickness and smooth surface.
[0043] In some embodiments, the photoinitiator can be any one or more of photoinitiator 1173, photoinitiator 1176, photoinitiator 184, TPO, TPO-L, photoinitiator 127, photoinitiator 369, I TX, BDK, photoinitiator 819, photoinitiator 754, photoinitiator 380, BMF, ANTHRACURE UVS-1331, ANTHRACURE UVS-1101, Easep i 6992, Easep i 1176, and Easep i 250.
[0044] Exemplarily, the photoinitiators provided above can all play the role of adjusting the curing rate and curing degree of the nanoimprint photoresist.
[0045] In some embodiments, the organic solvent can be selected from any one or more of propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, ethyl acetate, N,N-dimethylformamide, methyl ethyl ketone, dimethyl sulfoxide, and butyl acetate.
[0046] Illustratively, the organic solvents provided above can adjust the viscosity and volatilization rate of the nanoimprint photoresist, thereby facilitating the control of the thickness and surface flatness of the film layer during the spin coating process.
[0047] It should be noted that the above-mentioned multiple different types of cage-type polysilsesquioxane oligomers, monofunctional functional monomers, multifunctional acrylate monomers and / or multifunctional vinyl ether monomers, organosilanes, additives, photoinitiators and organic solvents generally have different molecular weights, functional groups or hardness, but all belong to the same category of substances.
[0048] See also Figure 2 , Figure 2 It is a flow chart of an embodiment of a method for preparing a nanoimprint photoresist provided in an embodiment of the present application, wherein the preparation method comprises: step S101 and step S102.
[0049] Step S101: providing a cage-type polysilsesquioxane oligomer, a monofunctional monomer, an organic silane, an auxiliary agent, a photoinitiator and an organic solvent, wherein the monofunctional monomer has an alicyclic structure.
[0050] It should be noted that the specific examples of the cage-type polysilsesquioxane oligomer, the monofunctional monomer, the organosilane, the auxiliary agent, the photoinitiator and the organic solvent can refer to the above examples, and will not be repeated here.
[0051] Step S102: preparing a nanoimprint photoresist by using a cage-type polysilsesquioxane oligomer, a monofunctional monomer, an organic silane, an auxiliary agent, a photoinitiator and an organic solvent.
[0052] The embodiment of the present application provides a method for preparing a nanoimprint photoresist, which utilizes a cage-type polysilsesquioxane oligomer and a monofunctional functional monomer to react, so that the prepared nanoimprint photoresist has a POSS structure and an alicyclic structure, thereby enhancing the oxygen plasma etching resistance of the nanoimprint photoresist, having a higher etching selectivity in the ICP dry etching process, and also enabling the prepared nanoimprint photoresist to have low surface energy, high Young's modulus and high hardness, and having good demolding effect, fidelity and resolution in the imprinting process. At the same time, the viscosity of the nanoimprint photoresist is 3.5-15mPa.s, the fluidity is good, the wetting and leveling effect on the substrate is good, a film layer with uniform thickness can be obtained, and the stability is good.
[0053] In some embodiments, in step S101, adding the organosilane, the auxiliary agent, and the photoinitiator into the first container, continuing the second stirring to mix evenly, standing and filtering to obtain the filtered nanoimprint photoresist, can include: sub-steps S201 and S202, such as Figure 3 shown.
[0054] Sub-step S201: adding cage-type polysilsesquioxane oligomer, monofunctional monomer and organic solvent into a first container, and stirring and mixing them uniformly based on a first stirring parameter.
[0055] Sub-step S202: adding the organosilane, the auxiliary agent and the photoinitiator into the first container, stirring and mixing them evenly based on the second stirring parameter, letting them stand and filtering to obtain a filtered nanoimprint photoresist.
[0056] Exemplarily, the first stirring parameter includes a first stirring temperature, a first stirring speed and a first stirring time, the first stirring temperature is 23°, the first stirring temperature can be 21°-25°, preferably, the first stirring temperature can be 23°, the first stirring temperature is the temperature in the container during stirring, the first stirring speed is 600r / min, and the first stirring time is 30 minutes. When stirring and mixing evenly, an organic solvent, a fluorine-modified caged silsesquioxane oligomer, a monofunctional acrylate and a multifunctional acrylate can be added to the container, and slowly stirred at a speed of 600r / min for 30 minutes to completely dissolve the system to obtain a uniform solution, and the liquid temperature in the container is maintained between 21°-25° during the process.
[0057] Exemplarily, the second stirring parameter includes a second stirring temperature, a second stirring speed, and a second stirring time. The second stirring temperature is 23°, and the second stirring temperature can be 21°-25°. Preferably, the second stirring temperature can be 23°, the second stirring temperature is the temperature in the container during stirring, the second stirring speed is 1000r / min, and the second stirring time is 30 minutes. When stirring and mixing evenly, adjust the speed to 1000r / min, then slowly add the organosilane, auxiliary agent and photoinitiator, and continue stirring for 30 minutes, and maintain the liquid temperature in the container between 21°-25° during the process. After stirring, let it stand for 30 minutes, and then filter under pressure with a 0.22μm organic filter to obtain a colorless and transparent nanoimprint photoresist.
[0058] It should be noted that, during the process of stirring and mixing, an inert gas such as nitrogen may be introduced into the container to reduce the oxygen concentration in the container, and the specific selection may be made according to actual conditions.
[0059] In some embodiments, in step S101, providing a cage-type polysilsesquioxane oligomer may include: sub-step S301 and sub-step S303, such as Figure 4 shown.
[0060] Sub-step S301: adding a first silane coupling agent, a second silane coupling agent, a first alkaline catalyst and a first solvent into a second container and stirring and mixing them uniformly, wherein the first silane coupling agent has an acid bond structure and the second silane coupling agent has a fluorine-based structure.
[0061] Sub-step S302: performing rotary evaporation, washing and drying treatment on the mixed liquid in the second container to obtain a silsesquioxane product.
[0062] Sub-step S303: performing condensation treatment on the silsesquioxane product to obtain a fluorine-modified cage-like silsesquioxane oligomer.
[0063] Among them, the first silane coupling agent has an acid bond structure, the second silane coupling agent has a fluorine-based structure, the first alkaline catalyst is 25% tetramethylammonium hydroxide, ammonia water or sodium hydroxide, which is used to catalyze the reaction, and the first solvent can be isopropanol, n-propanol, dimethyl carbonate or propylene glycol methyl ether.
[0064] Exemplarily, the first silane coupling agent can be γ-methacryloxypropyltrimethoxysilane (KH570) or other silane coupling agents with an acid bond structure; the second silane coupling agent can be dodecafluoroheptylpropyltrimethoxysilane (G502), heptadecafluorooctyltrimethoxysilane, nonafluorohexyltrimethoxysilane, trifluoropropyltrimethylsiloxane or other silane coupling agents with a fluorine-based structure.
[0065] In some embodiments, by weight percentage, the content of the first silane coupling agent is 5%-15%, for example: 5%, 10%, 12%, 15%, etc.; the content of the second silane coupling agent is 15%-20%, for example: 15%, 17%, 18%, 20%, etc.; the content of the first alkaline catalyst is 5-10%, for example: 5%, 7%, 8%, 10%, etc.; the content of the first solvent is 60-75%, for example: 60%, 67%, 70%, 75%, etc.
[0066] For example, the content of the first silane coupling agent may be 15%, the content of the second silane coupling agent may be 15%, the content of the first alkaline catalyst may be 5%, and the content of the first solvent may be 65%.
[0067] In some embodiments, the first alkaline catalyst and the first solvent are added to the second container and stirred and mixed evenly; the first silane coupling agent and the first solvent are added to the third container and stirred and mixed evenly; the second silane coupling agent and the first solvent are added to the fourth container and stirred and mixed evenly; the mixed solution of the third container and the mixed solution of the fourth container are added dropwise alternately to the second container and stirred and mixed evenly. Since the polarity difference between the first silane coupling agent and the second silane coupling agent is large, the compatibility when mixed together is not very good, and the density difference is large, there is stratification, so by adding separately, the first silane coupling agent and the second silane coupling agent can better react evenly with the system.
[0068] Exemplarily, 120g of isopropanol solvent and 9.4g of alkaline catalyst (tetramethylammonium hydroxide with a concentration of 25%) can be added to a single-mouth round-bottom flask, and a magnet can be added for magnetic stirring. In addition, 20ml of the first solvent isopropanol and 15g of KH570 are taken in a dropping funnel, and 28.9g of G502 is taken in another dropping funnel. While stirring, the liquids in the two dropping funnels are slowly added dropwise to the flask, and the addition is controlled to be completed in about half an hour. After the solution in the dropping funnel is added dropwise, magnetic stirring is performed at a temperature of 25°C and the reaction is performed for 2-3 hours. After the reaction is completed, the mixed solution is subjected to a rotary evaporation operation to evaporate the solvent isopropanol to obtain a light yellow oily liquid with a certain viscosity. Then, about 200ml of toluene is added to dissolve the rotary evaporation product, and the product is washed with saturated brine to remove the alkaline catalyst until pH = 7 (generally 3-5 times). The product is then dried over anhydrous magnesium sulfate, filtered, and the solvent toluene is removed by rotary evaporation to obtain a colorless viscous product, which is a silsesquioxane product.
[0069] In some embodiments, the silsesquioxane product, the second alkaline catalyst and the second solvent are added to a fifth container and stirred and mixed uniformly; the mixed solution in the fifth container is distilled and refluxed, and then subjected to rotary evaporation, washing and drying to obtain a fluorine-modified caged silsesquioxane oligomer. Thus, the fluorine-modified caged silsesquioxane oligomer can be obtained by condensing the silsesquioxane product.
[0070] The second alkaline catalyst may be tetramethylammonium hydroxide, ammonia water or sodium hydroxide with a concentration of 10%, which is used to catalyze the reaction, and the second solvent may be a solvent such as toluene that can be used for distillation and reflux.
[0071] Exemplarily, 100 ml of toluene, 3 g of alkaline catalyst (10% tetramethylammonium hydroxide), and silsesquioxane product can be added to a single-mouth round-bottom flask, and then a magnet is added for magnetic stirring. Using a water-separating distiller, the system is heated to remove water from the system. Then the temperature is heated to 120°C, and the toluene is recondensed at the reflux temperature. After about 3 hours of toluene reflux, the reaction is basically completed. Then, saturated salt water is used to wash to remove alkalinity, and anhydrous magnesium sulfate is used for dehydration. After filtering and rotary evaporation, a colorless, viscous oily liquid is obtained, which is an oligomeric silsesquioxane with a photosensitive side chain, that is, a fluorine-modified caged silsesquioxane oligomer. Among them, the photosensitive side chain is a segment with a UV-curable carbon-carbon double bond.
[0072] The following is a specific example to illustrate the preparation method of the fluorine-modified caged silsesquioxane oligomer provided in the examples of the present application.
[0073] Embodiment a:
[0074] In a single-mouth round-bottomed flask, 20g of isopropanol and 5g of an alkaline catalyst (tetramethylammonium hydroxide with a concentration of 25%) are added, and a magnet is added for magnetic stirring. In addition, 40g of isopropanol and 15g of KH570 are put into a dropping funnel, and 20g of G502 is put into another dropping funnel. While stirring, the liquids in the two dropping funnels are slowly added dropwise to the reactor, and the dropwise addition is completed in about half an hour. After the solution in the dropping funnel is added dropwise, at 25°C, magnetic stirring is used for reaction for 2-3 hours, and then rotary evaporation, washing and drying are carried out to obtain a silsesquioxane product, and finally the silsesquioxane product is subjected to condensation treatment to obtain a fluorine-modified cage-like silsesquioxane oligomer, and the fluorine-modified cage-like silsesquioxane oligomer prepared by the above-mentioned mass ratio composition raw materials reacts quickly and has high hardness.
[0075] Embodiment b:
[0076] In a single-mouth round-bottomed flask, 37.5g of n-propyl alcohol and 5g of an alkaline catalyst (tetramethylammonium hydroxide with a concentration of 25%) were added, and a magnet was added for magnetic stirring. In addition, 37.5g of n-propyl alcohol and 5g of KH570 were taken in a dropping funnel, and 15g of heptadecafluoroquinoline trimethoxysilane was taken in another dropping funnel. While stirring, the liquids in the two dropping funnels were slowly added dropwise to the reactor, and the dropwise addition was completed in about half an hour. After the solution in the dropping funnel was added dropwise, at 25°C, magnetic stirring was used, and the reaction was performed for 2-3 hours, followed by rotary evaporation, washing and drying to obtain a silsesquioxane product, and finally the silsesquioxane product was subjected to condensation treatment to obtain a fluorine-modified cage-like silsesquioxane oligomer, which was softer and had a slightly slower reaction speed than the fluorine-modified cage-like silsesquioxane oligomer prepared by the above-mentioned mass ratio composition raw materials.
[0077] Embodiment c:
[0078] In a single-mouth round-bottom flask, 35g of propylene glycol methyl ether and 10g of an alkaline catalyst (sodium hydroxide with a concentration of 25%) were added, and a magnet was added for magnetic stirring. In addition, 30g of propylene glycol methyl ether and 8g of KH570 were taken in a dropping funnel, and 17g of nonafluorohexyl trimethoxysilane was taken in another dropping funnel. While stirring, the liquids in the two dropping funnels were slowly added dropwise to the reactor, and the addition was completed in about half an hour. After the solution in the dropping funnel was added dropwise, at 25°C, magnetic stirring was used, and the reaction lasted for 2-3 hours, and then rotary distillation, washing and drying were performed to obtain a silsesquioxane product, and finally the silsesquioxane product was subjected to condensation treatment to obtain a fluorine-modified cage-like silsesquioxane oligomer, and the fluorine-modified cage-like silsesquioxane oligomer prepared by the above-mentioned mass ratio composition raw materials reacted quickly and had a higher hardness.
[0079] Embodiment d:
[0080] 40g of dimethyl carbonate and 7g of alkaline catalyst (sodium hydroxide with a concentration of 25%) were added to a single-mouth round-bottom flask, and a magnet was added for magnetic stirring. In addition, 31g of dimethyl carbonate and 6g of KH570 were placed in a dropping funnel, and 16g of nonafluorohexyltrimethoxysilane was placed in another dropping funnel. While stirring, the liquids in the two dropping funnels were slowly added dropwise to the reactor, and the addition was completed in about half an hour. After the solution in the dropping funnel was added dropwise, the reaction was carried out at 25°C with magnetic stirring for 2-3 hours, and then rotary evaporation, washing and drying were performed to obtain a silsesquioxane product, and finally the silsesquioxane product was subjected to condensation treatment to obtain a fluorine-modified caged silsesquioxane oligomer. The fluorine-modified caged silsesquioxane oligomer prepared by the above-mentioned mass ratio composition raw materials reacts faster and has a higher hardness.
[0081] The preparation method and performance of the nanoimprint photoresist provided in the embodiments of the present application are described below through specific examples.
[0082] Embodiment 1:
[0083] (1) Add 65 g of propylene glycol methyl ether acetate, 22 g of homemade fluorine-modified caged silsesquioxane oligomer, 3 g of 2-methyl-2-methylacrylate adamantyl ester, 2 g of 2,6-sultone-5-methacrylate norbornane ester, and 5 g of 1,6-hexanediol diacrylate into a container, and slowly stir at a speed of 600 r / min for 30 minutes to completely dissolve the system to obtain a uniform solution. During the process, the liquid temperature in the container is maintained at 23°C.
[0084] (2) Adjust the rotation speed to 1000 r / min, then slowly add 1 g of γ-(methacryloyloxy)propyltrimethoxysilane, 1 g of BYK333 and 1 g of photoinitiator 1176, and continue stirring for 30 minutes. During the process, maintain the liquid temperature in the container at 23°C.
[0085] (3) After stirring, the mixture was allowed to stand for 30 minutes, and then filtered under pressure using a 0.22 μm organic filter to obtain a colorless and transparent nanoimprint photoresist.
[0086] Therefore, in Example 1, the amount of cage-type polysilsesquioxane oligomer accounts for 22%, the amount of monofunctional monomer accounts for 5%, the amount of multifunctional monofunctional monomer accounts for 5%, the amount of organosilane accounts for 1%, the amount of auxiliary agent accounts for 1%, the amount of photoinitiator accounts for 1%, and the amount of organic solvent accounts for 65%.
[0087] Embodiment 2:
[0088] (1) Add 50 g of dipropylene glycol methyl ether acetate, 19 g of homemade fluorine-modified caged silsesquioxane oligomer, 6 g of isobornyl methacrylate, 4 g of 3-hydroxy-1-adamantyl methacrylate, and 10 g of triethylene glycol divinyl ether into a container, and slowly stir at 600 r / min for 30 minutes to completely dissolve the system to obtain a uniform solution. During the process, the liquid temperature in the container is maintained at 23°C.
[0089] (2) Adjust the rotation speed to 1000 r / min, then slowly add 5 g of vinyl trimethoxysilane, 3 g of BYK3550 and 3 g of photoinitiator 184, and continue stirring for 30 minutes. During the process, maintain the liquid temperature in the container at 23°C.
[0090] (3) After stirring, the mixture was allowed to stand for 30 minutes, and then filtered under pressure using a 0.22 μm organic filter to obtain a colorless and transparent nanoimprint photoresist.
[0091] Therefore, in Example 2, the usage of cage-type polysilsesquioxane oligomer accounts for 19%, the usage of monofunctional monomer accounts for 10%, the usage of multifunctional monofunctional monomer accounts for 10%, the usage of organosilane accounts for 5%, the usage of auxiliary agent accounts for 3%, the usage of photoinitiator accounts for 3%, and the usage of organic solvent accounts for 50%.
[0092] Embodiment 3:
[0093] (1) Add 70 g of dipropylene glycol methyl ether acetate, 15 g of a caged silsesquioxane oligomer having an epoxy group on the side chain, 2 g of 2,6-sultone-5-methylpropenoic acid norbornane ester, 3 g of 3-hydroxy-1-methylpropenoic acid adamantane ester, and 5 g of pentaerythritol triacrylate into a container, and slowly stir at a speed of 600 r / min for 30 minutes to completely dissolve the system to obtain a uniform solution. During the process, the liquid temperature in the container is maintained at 23°C.
[0094] (2) Adjust the rotation speed to 1000 r / min, then slowly add 3 g of methacryloxypropyl tri(dimethylsiloxy)silane, 1 g of BYK3570 and 1 g of TPO, and continue stirring for 30 minutes. During the process, maintain the liquid temperature in the container at 23°C.
[0095] (3) After stirring, the mixture was allowed to stand for 30 minutes, and then filtered under pressure using a 0.22 μm organic filter to obtain a colorless and transparent nanoimprint photoresist.
[0096] Therefore, in Example 3, the amount of cage-type polysilsesquioxane oligomer accounts for 15%, the amount of monofunctional monomer accounts for 5%, the amount of multifunctional monofunctional monomer accounts for 5%, the amount of organosilane accounts for 3%, the amount of auxiliary agent accounts for 1%, the amount of photoinitiator accounts for 1%, and the amount of organic solvent accounts for 70%.
[0097] Embodiment 4:
[0098] (1) Add 60 g of dipropylene glycol methyl ether acetate, 20 g of a caged silsesquioxane oligomer having a methacryloyloxypropyl group on the side chain, 4 g of vinyl ether-maleic anhydride ester, 4 g of 3-hydroxy-1-methacrylate adamantyl ester, and 7 g of pentaerythritol tetraacrylate into a container, and slowly stir at a speed of 600 r / min for 30 minutes to completely dissolve the system to obtain a uniform solution. During the process, the liquid temperature in the container is maintained at 23°C.
[0099] (2) Adjust the rotation speed to 1000 r / min, then slowly add 1 g of γ-(acryloyloxy)propyltrimethoxysilane, 2 g of Deqian 455 and 2 g of photoinitiator 754, and continue stirring for 30 minutes. During the process, maintain the liquid temperature in the container at 23°C.
[0100] (3) After stirring, the mixture was allowed to stand for 30 minutes, and then filtered under pressure using a 0.22 μm organic filter to obtain a colorless and transparent nanoimprint photoresist.
[0101] Therefore, in Example 4, the amount of cage-type polysilsesquioxane oligomer accounts for 20%, the amount of monofunctional monomer accounts for 8%, the amount of multifunctional monofunctional monomer accounts for 7%, the amount of organosilane accounts for 1%, the amount of auxiliary agent accounts for 2%, the amount of photoinitiator accounts for 2%, and the amount of organic solvent accounts for 60%.
[0102] The nanoimprint photoresist provided in the above embodiment was used for performance testing, and the performance test experimental data are shown in Table 1. The related art provides the specification value of the nanoimprint photoresist, which is used to compare with the nanoimprint template glue provided in the above embodiment to confirm whether the nanoimprint template glue provided in the above embodiment meets the specification value.
[0103] Table 1
[0104]
[0105]
[0106] As can be seen from Table 1, the appearance of the nanoimprint template glue provided in the embodiment of the present application meets the standard value of colorless transparent liquid; the viscosity meets the standard value of 3.5-15mPa.s; the hardness after curing meets the standard value of 60-75D; the surface water drop angle meets the standard value greater than or equal to 100°; the Young's modulus meets the standard value greater than or equal to 1GPa; taking the substrate as a silicon base as an example, the etching selectivity meets the standard value greater than or equal to 1. Taking the silicon base as an example, since the etching selectivity is greater than 1, it has a higher etching selectivity in the ICP dry etching process, so that after photocuring, the excess photoresist can be quickly and thoroughly removed by using a plasma etching process. At the same time, it can also make the prepared nanoimprint photoresist have low surface energy, high Young's modulus and high hardness, and have good demolding effect, fidelity and resolution during the imprinting process.
[0107] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A nanoimprint photoresist, characterized in that: The nanoimprint photoresist is prepared from the following raw materials: cage-type polysilsesquioxane oligomer, monofunctional monomer, organic silane, auxiliary agent, photoinitiator and organic solvent, wherein the monofunctional monomer has an alicyclic structure.
2. The nanoimprint photoresist according to claim 1, characterized in that: The nanoimprint photoresist further comprises a multifunctional acrylate monomer and / or a multifunctional vinyl ether monomer.
3. The nanoimprint photoresist according to claim 2, characterized in that: In weight percentage, the content of the cage-type polysilsesquioxane oligomer is 15%-30%, the content of the monofunctional functional monomer is 5%-10%, the content of the multifunctional monofunctional functional monomer and / or the multifunctional vinyl ether monomer is 5%-10%, the content of the organosilane is 1%-5%, the content of the auxiliary agent is 1%-3%, the content of the photoinitiator is 1%-3%, and the content of the organic solvent is 50%-70%.
4. The nanoimprint photoresist according to claim 1, characterized in that: The cage polysilsesquioxane oligomer is at least one of a fluorine-modified cage polysilsesquioxane oligomer, a cage polysilsesquioxane oligomer having an epoxy group on the side chain, a cage polysilsesquioxane structure oligomer having an acryloxypropyl group on the side chain, and a cage polysilsesquioxane oligomer having a methacryloxypropyl group on the side chain.
5. The nanoimprint photoresist according to claim 2, characterized in that: The monofunctional monomer is at least one of isobornyl methacrylate, 2-methyl-2-adamantyl methacrylate, 3-hydroxy-1-adamantyl methacrylate, 2,6-sultone-5-norbornyl methacrylate, (1'-methylcyclopentyl-1-cyclopentyl) methacrylate, α-(γ-butyrolactone) methacrylate, 3-oxo-4,10-dioxa-tricyclo[5.2.1.02,6]dec-8-yl methacrylate, 3-hydroxy-1-adamantyl methacrylate, (2,2-dimethyl-1,3-dioxolane-4-methyl) methacrylate, [bis(2,2-dimethyl-1,3-dioxolane)-4-methyl] methacrylate, norbornene, norbornene-maleic anhydride, norbornene-sulfur dioxide, and vinyl ether-maleic anhydride ester.
6. The nanoimprint photoresist according to claim 2, characterized in that: The multifunctional vinyl ether monomer is at least one of hydroxybutyl vinyl ether, triethylene glycol divinyl ether, 1,4-cyclohexyl dimethanol divinyl ether and butyl vinyl ether; The multifunctional acrylate monomer is at least one of 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, 4(ethoxylated)pentaerythritol tetraacrylate and pentaerythritol tetraacrylate.
7. The nanoimprint photoresist according to claim 1, characterized in that: The organosilane is at least one of γ-(methacryloxy)propyl trimethoxysilane, vinyl trimethoxysilane, vinyl tri(2-methoxyethoxy)silane, vinyl triethoxysilane, γ-(methacryloxy)propyl triethoxysilane, methacryloxymethyl triethoxysilane, 3-methacryloxypropyl tri(methoxyethoxy)silane, methacryloxypropyl tri(dimethylsiloxy)silane, γ-(acryloxy)propyl trimethoxysilane, γ-(acryloxy)propyl triethoxysilane, allyl tri(trimethylsiloxy)silane, 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, and N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyl triethoxysilane.
8. The nanoimprint photoresist according to claim 1, characterized in that: The auxiliary agent is at least one of BYK333, BYK3550, BYK302, BYK3500, BYK3530, BYK3570, Deqian 407, Deqian 410, Deqian 411, Deqian 432, Deqian 435, and Deqian 455.
9. The nanoimprint photoresist according to claim 1, characterized in that: The photoinitiator is at least one of photoinitiator 1173, photoinitiator 1176, photoinitiator 184, TPO, TPO-L, photoinitiator 127, photoinitiator 369, ITX, BDK, photoinitiator 819, photoinitiator 754, photoinitiator 380, BMF, ANTHRACURE UVS-1331, ANTHRACURE UVS-1101, Easepi 6992, Easepi 1176, and Easepi 250.
10. The nanoimprint photoresist according to claim 1, characterized in that: The organic solvent is at least one of propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, ethyl acetate, N,N-dimethylformamide, methyl ethyl ketone, dimethyl sulfoxide, and butyl acetate.
11. A method for preparing a nanoimprint photoresist, characterized in that: The method comprises: Providing a cage-type polysilsesquioxane oligomer, a monofunctional functional monomer, an organic silane, an auxiliary agent, a photoinitiator and an organic solvent, wherein the monofunctional functional monomer has an alicyclic structure; The nanoimprint photoresist is prepared by using the cage-type polysilsesquioxane oligomer, monofunctional monomer, organic silane, auxiliary agent, photoinitiator and organic solvent.
12. The preparation method according to claim 11, characterized in that: The method of preparing the nanoimprint photoresist by using the cage-type polysilsesquioxane oligomer, a monofunctional monomer, an organic silane, an auxiliary agent, a photoinitiator and an organic solvent comprises: Adding the cage-type polysilsesquioxane oligomer, the monofunctional monomer and the organic solvent into a first container, and stirring and mixing them uniformly based on a first stirring parameter; The organosilane, auxiliary agent and photoinitiator are added into the first container, and stirred and mixed evenly based on the second stirring parameter, and the mixture is allowed to stand and filtered to obtain a filtered nanoimprint photoresist.
13. The preparation method according to claim 12, characterized in that: The first stirring parameters include a first stirring temperature, a first stirring speed and a first stirring time, the first stirring temperature is 21°-25°, the first stirring speed is 600r / min, and the first stirring time is 30 minutes; the second stirring parameters include a second stirring temperature, a second stirring speed and a second stirring time, the second stirring temperature is 21°-25°, the second stirring speed is 1000r / min, and the second stirring time is 30 minutes.
Citation Information
Patent Citations
Silicon-containing (meth)acrylate light-cured stamping adhesive for ultraviolet nanometer-sized stamping and application thereof
CN101750895A
Sulfydryl-containing low polysiloxane compound, ultraviolet photoresist composition thereof, and impressing process
CN102174059A
Imprinting material
CN106575606A
Curable composition for nano-imprint, cured product using the same, and member for liquid crystal display device
JP2010013514A
Cited By
High-transparency rare earth nanoparticle / polyhedral oligomeric silsesquioxane composite photoresist as well as preparation method and application thereof
CN121806380A
Highly transparent rare earth nanoparticle / caged polysilsesquioxane composite photoresist, and preparation method and application thereof
CN121806380B
Method for regulating and controlling surface energy of silicon-based anti-reflection coating and hard mask material by using polyhedral oligomeric silsesquioxane
CN122239373A