Low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste curing and preparation method of low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material
By sintering the double-layer curing structure of the cement-phosphate glass mixed material of low temperature, the problems of high ion leaching rate and low mechanical strength are solved, and the stable curing and long-term preservation of high radioactive nuclear waste are achieved.
Patent Information
- Application Number
- CN202310598017.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
In the high radioactive environment, existing nuclear waste solidified materials have problems such as high ion leaching rate of nuclides, insufficient nuclide capacity and low mechanical strength, making it difficult to effectively cure high radioactive nuclear waste.
The low-temperature sintered magnesium potassium phosphate cement-phosphate glass mixture is used to adjust the component ratio and process flow, including the use of Na2B4O7·10H2O as a retarder, nano-level efficient modified oxides and decomposed carbonates and other components. A double-layer cured structure is formed to improve mechanical strength and chemical stability.
It achieves a low leaching rate of radioactive elements, improves the mechanical strength and chemical stability of glass, enhances the inclusiveness and curing effect of high radionuclides, and reduces energy consumption and costs.
Smart Images

Figure BDA0004247810410000061 
Figure BDA0004247810410000062
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-level radioactive nuclear waste treatment, and relates to a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification and a preparation method thereof, and is suitable for solidification treatment of high-level radioactive waste liquid in the nuclear industry and defense fields. Background Art
[0002] Nuclear energy is an efficient, clean and sustainable energy that can meet human needs. Today, nuclear energy is mainly used in the nuclear industry and the field of national defense and military. The military application of nuclear energy mainly refers to the development of nuclear weapons, which play an irreplaceable role in national defense and security. However, in the process of nuclear weapons production and use, a large amount of unavoidable dangerous products such as nuclear waste liquid will also be produced. Due to its long half-life period and high biological toxicity, it has become an important factor endangering environmental health and urgently needs to be treated and disposed of. In order to minimize the impact of nuclear waste liquid on the natural environment, the international community currently often uses the method of first evaporating the nuclear waste liquid into solid nuclear waste and then wrapping the nuclear waste with solidifying materials and burying it deep underground. This process has high requirements for nuclear waste solidifying materials.
[0003] Nuclear waste solidification materials must have the characteristics of good chemical stability, high mechanical strength and excellent thermal stability. As the solidification substrate of high-level radioactive nuclear waste that is widely studied and applied in the world, glass waste solidification body undergoes high-temperature melting and vitrification treatment. High-valent ions enter the glass grid to become network forming bodies, while low-valent alkali metal cations fill the network to become network compensating bodies, which prevent the migration of nuclides through huge viscosity and density. Compared with borosilicate glass, phosphate glass has greater tolerance for nuclear waste and strong chemical corrosion resistance, forming a glass with stable and excellent performance. However, at the same time, the active corrosion components (such as iron, sulfate, etc.) in high-level nuclear waste contain high concentrations of α-radioactive nuclides and ammonium nitrate, which will seriously affect the durability of phosphate glass. The crystalline substances precipitated in the glass are more soluble in water, causing the nuclear substances in the glass solidification to be easily leached. In addition, the mechanical strength of phosphate glass is not ideal. Once the glass solidification body is broken, the specific surface area of the solidification body increases, resulting in an increase in the leaching rate.
[0004] Potassium magnesium phosphate cement has the characteristics of fast setting and hardening, high early strength, and strong durability. It generates insoluble phosphate precipitates through chemical reactions between harmful metal ions and phosphate ions in the system. Phosphate precipitates can also be physically encapsulated in the cement matrix by magnesium phosphate cement, thereby achieving effective solidification of nuclides and heavy metal ions. In addition, the high-temperature sintering ceramicization phenomenon of magnesium phosphate cement is also conducive to the long-term disposal of the solidified body, so it is often used in the treatment of medium and low-level radioactive nuclear waste. However, traditional potassium magnesium phosphate cement materials have a relatively fast setting speed, a relatively large irregular pore structure, and a relatively large specific surface area, which can easily cause the migration of nuclides.
[0005] Therefore, the present invention aims to overcome the shortcomings of existing materials, combine the advantages of the performance of two solidifying materials, and prepare a solidifying material with stable performance, low nuclide ion leaching rate, high nuclide encapsulation capacity and high mechanical strength, so as to be suitable for the treatment of high-level radioactive nuclear waste. Summary of the invention
[0006] In order to overcome the problems of high nuclide ion leaching rate, insufficient nuclide packaging capacity, low mechanical strength, etc. in the application process of existing nuclear waste solidification materials, the present invention provides a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification.
[0007] The solution adopted by the present invention to solve the technical problem is: a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification, the mixed material includes 66 to 82 parts of potassium magnesium phosphate cement and 89 to 114 parts of phosphate glass by weight, which can be used to solidify 20 to 30 parts of nuclear waste liquid; the potassium magnesium phosphate cement includes 10 to 12 parts of KH 2 PO 4 , 6 to 10 parts of additives and 50 to 60 parts of MgO; the phosphate glass includes 35 to 40 parts by weight of NH 4 H 2 PO 4 , 26-34 parts of nano-scale high-efficiency modified oxides, 26-36 parts of decomposable carbonates and 2-4 parts of H 3 BO 3 .
[0008] The present invention uses phosphate glass, which has a lower melting temperature and is more tolerant to nuclear waste elements. 4 H 2 PO 4 P 2 O 5It is the main forming body of phosphate glass and exists in the glass in the form of a phosphorus-oxygen tetrahedron. There is a double-bonded covalent oxygen in the phosphorus-oxygen tetrahedron, which causes the phosphorus-oxygen tetrahedron to present a deformed vertex due to the asymmetry of the bond energy. This vertex is connected to the oxygen in other tetrahedrons to form a skeleton or sheet structure. The mass of magnesium-potassium phosphate cement powder is less than the mass of phosphate glass raw materials, which can ensure that the molten glass fully wraps the magnesium-potassium phosphate cement powder and can completely fill the pores in the sintered magnesium-potassium phosphate cement. From H 3 BO 3 B 2 O 3 The thermo-mechanical properties of the glass phase in phosphate glass can be improved, so that the flexural strength, fracture toughness and microhardness of the phosphate glass are increased.
[0009] Further, the admixture is Na 2 B 4 O 7 10H 2 O.
[0010] Na 2 B 4 O 7 10H 2 O acts as a retarder to prolong the setting and hardening time of magnesium potassium phosphate cement, ensure uniform mixing of nuclear waste liquid and various components of magnesium potassium phosphate cement, and improve the solidification effect of magnesium potassium phosphate cement.
[0011] Furthermore, the nano-scale high-efficiency modified oxide includes 12 to 15 parts of Al 2 O 3 , 6-8 parts SiO 2 , 6 to 8 parts Fe 2 O 3 , 2-3 parts ZrO 2 .
[0012] The Al 2 O 3 As a network former, it forms aluminum-oxygen tetrahedron with oxygen, repairing defects in the glass network, improving the stability of the glass, and also greatly improving the mechanical properties of phosphate glass.
[0013] The Fe 2 O 3 It plays a dual role in phosphate glass, acting as a modifier and a network former. The PO-Fe connection formed after the addition of iron oxide replaces the original POP connection, enhancing the strength and hardness of the glass network.
[0014] The ZrO 2The addition of will destroy the POP bonds and P=O in the network structure, and the formed PO-Zr will strengthen the network structure of the glass. The chemical stability of the glass will be enhanced because the network structure of the glass becomes dense, which will help reduce the leaching rate of nuclides in the solid body, enhance the compressive strength of the final product solid body, and help the long-term preservation of the solid body.
[0015] The SiO 2 As the "skeleton" of glass, it can increase the viscosity of molten glass and improve the chemical and thermal stability of the glass.
[0016] Furthermore, the decomposable carbonate includes 6 to 8 parts of Li 2 CO 3 ,12~16 copies of K 2 CO 3 , 8 to 12 parts Na 2 CO 3 .
[0017] Under high temperature environment, Li in this phosphate glass system 2 CO 3 , K 2 CO 3 and Na 2 CO 3 Decomposition to obtain alkali metal oxide Li 2 O, K 2 O and Na 2 O, these alkali metal oxides can "open" the skeleton structure of the glass during melting, thereby increasing the melting rate of the glass, reducing the viscosity of the glass during melting, making the properties of the glass more uniform, and helping the glass liquid to wrap the magnesium potassium phosphate cement powder.
[0018] Furthermore, the MgO is sieved through a 200-mesh sieve.
[0019] As the MgO mesh size increases, the hydration reaction rate of magnesium potassium phosphate cement accelerates, and the early strength shows a rapid growth trend. Considering the two indicators of initial setting time and early strength, 200 mesh is taken as the appropriate fineness.
[0020] The invention also discloses a method for preparing a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification, comprising the following steps:
[0021] 1) Take 10-12 portions of KH 2 PO 4 , 6 to 10 parts Na 2 B 4 O 7 10H 2 O, uniformly mixed to obtain a mixture A;
[0022] 2) taking 20 to 30 parts of the treated nuclear waste liquid, mixing the mixture A with the target nuclear waste liquid by ultrasonic vibration to obtain a mixed liquid, adding 50 to 60 parts of MgO to the mixed liquid and stirring at high speed to obtain a magnesium potassium phosphate cement slurry, then pouring the obtained slurry into a mold, placing it in a constant temperature and humidity chamber for curing, and then removing the mold, and continuing to cure to a specified age, the curing conditions are: temperature 25±2°C, humidity ≥95%, to obtain a magnesium potassium phosphate cement block, and grinding the magnesium potassium phosphate cement block through a 200 mesh sieve to obtain a powder B;
[0023] 3) Phosphate glass powder raw materials are weighed according to the mass ratio: 35-40 parts NH 4 H 2 PO 4 , 12 to 15 parts Al 2 O 3 , 6-8 parts SiO 2 , 2 to 4 parts H 3 BO 3 , 6 to 8 parts Li 2 CO 3 ,6~8 parts Fe 2 O 3 , 12 to 16 copies of K 2 CO 3 , 8 to 12 parts Na 2 CO 3 , 2-3 parts ZrO 2 , after mixing, raw material C is obtained;
[0024] 4) taking powder material B and glass powder raw material C and mixing them thoroughly to obtain mixed powder material D;
[0025] 5) placing the obtained mixed powder D in a muffle furnace and heating it to 750-850° C. for melting for 1 hour, and then cooling it to room temperature to obtain a glass embryo E of a magnesium potassium phosphate cement-phosphate glass mixed material;
[0026] 6) crushing the glass embryo E into glass blocks with a diameter of 5 mm, and passing through a glass bead electric heating rotary furnace at 550-650° C. to soften the surface and shrink the irregular edges and corners under the action of surface tension while rolling to form a spherical shape;
[0027] 7) Annealing at 400° C. for 24 hours to obtain the final product, a solidified body F.
[0028] The preparation method of a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification provided by the present invention solves the problems existing in the existing nuclear waste solidification materials well. The potassium magnesium phosphate cement has a fast hardening speed and has good tolerance to active corrosion components (such as iron, sulfate, etc.) in high-level nuclear waste liquid. In the process of mixing and melting the potassium magnesium phosphate cement with the glass powder raw material, the potassium magnesium phosphate cement has no obvious grain boundaries after high-temperature heating, and the grains are completely melted, showing a good ceramic structure. At the same time, the phosphate glass fills the pore structure in the potassium magnesium phosphate cement as a molten liquid. The phosphate glass covered on the surface of the potassium magnesium phosphate cement re-solidifies the nuclides migrating in the potassium magnesium phosphate cement, and the solidified body forms a more compact structure. The double-layer solidification structure reduces the leaching rate of radioactive elements. At the same time, the potassium magnesium phosphate cement as an internal filler of the phosphate glass improves the mechanical strength of the glass, which is conducive to the long-term preservation of the solidified body.
[0029] The beneficial effects of the present invention are as follows: (1) the double-layer solidification form is adopted, and the leaching rate of highly radioactive elements is low. (2) the glass melting temperature is low, the processing technology is simple, energy consumption is saved, and the cost is reduced; (3) magnesium potassium phosphate cement forms a dense ceramic structure after high-temperature sintering, which further improves the mechanical properties, water stability and chemical stability of the solidified body; (4) magnesium potassium phosphate cement powder is added into the glass as the introduced second phase filler to improve the mechanical strength of the glass and reduce the influence of environmental disturbance on the solidified body during long-term storage; (5) the tolerance to radioactive elements is enhanced, and the high concentration of α-radioactive nuclides and ammonium nitrate contained in the active corrosion components (such as iron, sulfate, etc.) in the highly radioactive nuclear waste liquid can also be effectively solidified; (6) phosphate can form insoluble compounds with some heavy metal ions and radioactive isotopes, thereby effectively removing radioactive substances from raw water. DETAILED DESCRIPTION
[0030] In order to more clearly explain the technical solutions of the present invention and the prior art, the implementation process of the present invention will be fully and exemplarily described below. It should be noted that based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention. A specific preparation method of a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification is as follows:
[0031] Example 1
[0032] A low-temperature sintered magnesium potassium phosphate cement-phosphate glass mixed material for nuclear waste solidification, comprising the following components by weight: 59 grams of MgO, 12 grams of KH 2 PO 4 , 10 g Na 2 B 4 O 710H 2 O, 28 g nuclear waste liquid, 35 g NH 4 H 2 PO 4 , 12 g Al 2 O 3 , 6 g SiO 2 , 3 g H 3 BO 3 , 6 grams 2 CO 3 , 7 g Fe 2 O 3 , 12g K 2 CO 3 , 8 grams Na 2 CO 3 , 2 grams ZrO 2 A method for preparing a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification comprises the following steps:
[0033] 1) Take 12 g KH 2 PO 4 , 10 g Na 2 B 4 O 7 10H 2 O, uniformly mixed to obtain a mixture A;
[0034] 2) 28 g of the treated nuclear waste liquid is taken, and the mixture A and the target nuclear waste liquid are mixed by ultrasonic vibration to obtain a mixed liquid, 59 g of MgO is added to the mixed liquid and stirred at high speed to obtain magnesium potassium phosphate cement slurry, and the obtained slurry is poured into a mold after ultrasonic vibration, and placed in a constant temperature and humidity chamber for curing for 1 day before demolding, and the mold is continued to be cured to a specified age, and the curing conditions are: temperature 25±2°C, humidity ≥95%, to obtain a magnesium potassium phosphate cement block, and the magnesium potassium phosphate cement block is crushed and ground through a 200 mesh sieve to obtain a powder B;
[0035] 3) Weigh 35 g of NH 4 H 2 PO 4 , 12 g Al 2 O 3 , 6 g SiO 2 , 3 g H 3 BO 3 , 6 grams 2 CO 3 , 7 g Fe 2 O 3 , 12g K 2 CO 3 , 8 grams Na 2 CO 3 , 2 grams ZrO2 , and obtained raw material C after mixing with a pulverizer;
[0036] 4) Fully mixing powder material B and glass powder raw material C to obtain mixed powder material D;
[0037] 5) placing the obtained mixed powder D into a muffle furnace and melting it at 750° C. for 1 hour, and then cooling it to room temperature to obtain a glass embryo E of magnesium potassium phosphate cement doped with nuclear waste;
[0038] 6) crushing the glass embryo E into glass blocks with a diameter of 5 mm, and passing through a glass bead electric heating rotary furnace at 550° C. to soften the surface and shrink the irregular edges and corners under the action of surface tension while rolling to form a spherical shape;
[0039] 7) Annealing at 400° C. for 24 hours to obtain the final product, a solidified body F.
[0040] Example 2
[0041] A low-temperature sintered magnesium potassium phosphate cement-phosphate glass mixed material for nuclear waste solidification, comprising the following components by weight: 50 grams of MgO, 10 grams of KH 2 PO 4 , 7 grams Na 2 B 4 O 7 10H 2 O, 21 g nuclear waste liquid, 40 g NH 4 H 2 PO 4 , 14 g Al 2 O 3 , 8 g SiO 2 , 4 g H 3 BO 3 , 8 grams 2 CO 3 , 8 g Fe 2 O 3 , 16g K 2 CO 3 , 12 g Na 2 CO 3 , 3 grams ZrO 2 A method for preparing a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification comprises the following steps:
[0042] 1) Take 10 g KH 2 PO 4 , 7 grams Na 2 B 4 O 7 10H 2 O, uniformly mixed to obtain a mixture A;
[0043] 2) 21 g of the treated nuclear waste liquid is taken, and the mixture A and the target nuclear waste liquid are mixed by ultrasonic vibration to obtain a mixed liquid, 50 g of MgO is added to the mixed liquid and stirred at high speed to obtain magnesium potassium phosphate cement slurry, and the obtained slurry is poured into a mold after ultrasonic vibration, and placed in a constant temperature and humidity chamber for curing for 1 day before demolding, and the mold is continued to be cured to a specified age, and the curing conditions are: temperature 25±2°C, humidity ≥95%, to obtain a magnesium potassium phosphate cement block, and the magnesium potassium phosphate cement block is crushed and ground through a 200 mesh sieve to obtain a powder B;
[0044] 3) Weigh 40 g of NH 4 H 2 PO 4 , 14 g Al 2 O 3 , 8 g SiO 2 , 4 g H 3 BO 3 , 8 grams 2 CO 3 , 8 g Fe 2 O 3 , 16g K 2 CO 3 , 12 g Na 2 CO 3 , 3 grams ZrO 2 , and obtained raw material C after mixing with a pulverizer;
[0045] 4) Fully mixing powder material B and glass powder raw material C to obtain mixed powder material D;
[0046] 5) placing the obtained mixed powder D into a muffle furnace and melting it at 800° C. for 1 hour, and then cooling it to room temperature to obtain a glass embryo E of magnesium potassium phosphate cement doped with nuclear waste;
[0047] 6) crushing the glass embryo E into glass blocks with a diameter of 5 mm, and passing through a glass bead electric heating rotary furnace at 600° C. to soften the surface and shrink the irregular edges and corners under the action of surface tension while rolling to form a spherical shape;
[0048] 7) Annealing at 400° C. for 24 hours to obtain the final product, a solidified body F.
[0049] Example 3
[0050] A low-temperature sintered magnesium potassium phosphate cement-phosphate glass mixed material for nuclear waste solidification, comprising the following components by weight: 56 grams of MgO, 10 grams of KH 2 PO 4 , 8 grams Na 2 B 4 O 710H 2 O, 25 g nuclear waste liquid, 40 g NH 4 H 2 PO 4 , 15 g Al 2 O 3 , 7 g SiO 2 , 2 g H 3 BO 3 , 7 grams 2 CO 3 , 8 g Fe 2 O 3 , 12g K 2 CO 3 , 8 grams Na 2 CO 3 , 2 grams ZrO 2 , a low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification, comprising the following steps:
[0051] 1) Take 10 g KH 2 PO 4 , 8 grams Na 2 B 4 O 7 10H 2 O, uniformly mixed to obtain a mixture A;
[0052] 2) 25 g of the treated nuclear waste liquid is taken, and the mixture A and the target nuclear waste liquid are mixed by ultrasonic vibration to obtain a mixed liquid, 56 g of MgO is added to the mixed liquid and stirred at high speed to obtain magnesium potassium phosphate cement slurry, and the obtained slurry is poured into a mold after ultrasonic vibration, and placed in a constant temperature and humidity chamber for curing for 1 day before demolding, and the mold is continued to be cured to a specified age, and the curing conditions are: temperature 25±2°C, humidity ≥95%, to obtain a magnesium potassium phosphate cement block, and the magnesium potassium phosphate cement block is crushed and ground through a 200 mesh sieve to obtain a powder B;
[0053] 3) Weigh 40 g of NH 4 H 2 PO 4 , 15 g Al 2 O 3 , 7 g SiO 2 , 2 g H 3 BO 3 , 7 grams 2 CO 3 , 8 g Fe 2 O 3 , 12g K 2 CO 3 , 8 grams Na 2 CO 3 , 2 grams ZrO 2, and obtained raw material C after mixing with a pulverizer;
[0054] 4) Fully mixing powder material B and glass powder raw material C to obtain mixed powder material D;
[0055] 5) placing the obtained mixed powder D into a muffle furnace and melting it at 850° C. for 1 hour, and then cooling it to room temperature to obtain a glass embryo E of magnesium potassium phosphate cement doped with nuclear waste;
[0056] 6) crushing the glass embryo E into glass blocks with a diameter of 5 mm, and passing through a glass bead electric heating rotary furnace at 650° C. to soften the surface and shrink the irregular edges and corners under the action of surface tension while rolling to form a spherical shape;
[0057] 7) Annealing at 400° C. for 24 hours to obtain the final product, a solidified body F.
[0058] Comparative Example 1
[0059] A magnesium potassium phosphate cement-based nuclear waste solidified body, comprising the following components by weight: 50 grams of MgO, 10 grams of KH 2 PO 4 , 7 grams Na 2 B 4 O 7 10H 2 O, 40 grams of nuclear waste liquid;
[0060] A magnesium potassium phosphate cement-based nuclear waste solidified body comprises the following steps:
[0061] 1) Take 10 g KH 2 PO 4 , 50 g MgO, 7 g Na 2 B 4 O 7 10H 2 O, uniformly mixed to obtain a mixture A;
[0062] 2) 21 g of the treated nuclear waste liquid was taken, and mixture A was mixed with the nuclear waste liquid to obtain a mixed liquid. After ultrasonic vibration, the mixed liquid was poured into a 10 mm×10 mm×10 mm mold to obtain a magnesium potassium phosphate cement solidified body.
[0063] Comparative Example 2
[0064] A phosphate glass-based nuclear waste solidified body, comprising the following components by weight: 40 g NH 4 H 2 PO 4 , 14 g Al 2 O 3 , 8 g SiO 2 , 4 g H 3 BO3 , 8 grams 2 CO 3 , 8 g Fe 2 O 3 , 16g K 2 CO 3 , 12 g Na 2 CO 3 , 2 grams ZrO 2 A method for preparing a phosphate glass-based nuclear waste liquid solidified body, comprising the following steps:
[0065] 1) Take 40 g NH 4 H 2 PO 4 , 14 g Al 2 O 3 , 8 g SiO 2 , 4 g H 3 BO 3 , 8 grams 2 CO 3 , 8 g Fe 2 O 3 , 16g K 2 CO 3 , 12 g Na 2 CO 3 , 3 grams ZrO 2 Mixing evenly to obtain mixture A;
[0066] 2) heating the mixture A to 800° C., melting for 1 hour to fully react, and stirring evenly to obtain a homogenized high-level radioactive nuclear waste glass liquid, and cooling to room temperature to obtain a phosphate glass embryo;
[0067] 3) crushing the glass embryo into glass blocks with a diameter of 5 mm, and passing through a glass bead electric heating rotary furnace at 600 degrees Celsius to soften the surface and shrink the irregular edges and corners under the action of surface tension while rolling to form a spherical shape;
[0068] 4) Annealing at 400°C for 24 hours to obtain the final product.
[0069] In order to verify the effect of the present invention on nuclear waste solidification, the following test was conducted.
[0070] (1) Anti-leaching performance
[0071] Experiments were conducted on Examples 1, 2, 3, 4 of the present invention and Comparative Examples 1 and 2 to test their anti-leaching performance. The standardized leaching rates were measured as follows.
[0072] Table 1: Standardized leaching rates
[0073]
[0074] It can be seen from Table 1 that, compared with Comparative Examples 1 and 2, the standardized leaching rate of Example 1 is smaller, indicating that its anti-leaching performance is more excellent and can fully meet the use requirements of high-level radioactive nuclear waste solidification.
[0075] (2) Mechanical strength
[0076] Experiments were conducted on Examples 1, 2, 3, 4 of the present invention and Comparative Examples 1 and 2 to test their mechanical strengths. The compressive strength results were as follows.
[0077] Table 2: Compressive strength
[0078]
[0079] It can be seen from Table 2 that, compared with Comparative Example 1 and Example 2, Example 1 has a higher compressive strength, indicating that the mechanical strength performance is more excellent and can fully meet the use requirements during the long-term storage of high-level radioactive nuclear waste solidification.
Claims
1. A low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material for nuclear waste solidification, characterized in that: The mixed material includes 66 to 82 parts of magnesium potassium phosphate cement and 89 to 114 parts of phosphate glass by weight, which can be used to solidify 20 to 30 parts of nuclear waste liquid; the magnesium potassium phosphate cement includes 10 to 12 parts of KH2PO4, 6 to 10 parts of admixtures and 50 to 60 parts of MgO by weight; the phosphate glass includes 35 to 40 parts of NH4H2PO4, 26 to 34 parts of nano-level high-efficiency modified oxides, 26 to 36 parts of decomposable carbonates and 2 to 4 parts of H3BO3 by weight.
2. The low-temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material according to claim 1, characterized in that: The additive is Na2B4O7·10H2O.
3. The low temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material according to claim 1, characterized in that: The nanometer-scale high-efficiency modified oxide comprises 12 to 15 parts of Al2O3, 6 to 8 parts of SiO2, 6 to 8 parts of Fe2O3, and 2 to 3 parts of ZrO2.
4. The low temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material according to claim 1, characterized in that: The decomposable carbonate includes 6 to 8 parts of Li2CO3, 12 to 16 parts of K2CO3, and 8 to 12 parts of Na2CO3.
5. The low temperature sintered potassium magnesium phosphate cement-phosphate glass mixed material according to claim 1, characterized in that: The MgO is sieved through a 200-mesh sieve.
6. A method for preparing a low-temperature sintered magnesium potassium phosphate cement-phosphate glass mixed material for nuclear waste solidification, characterized in that The following steps are involved: 1) Take 10-12 parts of KH2PO4 and 6-10 parts of Na2B4O7·10H2O, mix them evenly to obtain a mixture A; 2) Take 20-30 parts of the treated nuclear waste liquid, mix the mixture A with the target nuclear waste liquid by ultrasonic vibration to obtain a mixed liquid, add 50-60 parts of MgO to the mixed liquid and stir at high speed to obtain magnesium potassium phosphate cement slurry, then pour the obtained slurry into a mold, put it into a constant temperature and humidity chamber for curing, then remove the mold, and continue to cure to a specified age, the curing conditions are: temperature 25±2°C, humidity ≥95%, to obtain magnesium potassium phosphate cement blocks, The potassium magnesium phosphate cement block is crushed and ground through a 200-mesh sieve to obtain powder B; 3) The phosphate glass powder raw material is weighed according to the mass ratio: 35-40 parts of NH4H2PO4, 12-15 parts of Al2O3, 6-8 parts of SiO2, 2-4 parts of H3BO3, 6-8 parts of Li2CO3, 6-8 parts of Fe2O3, 12-16 parts of K2CO3, 8-12 parts of Na2CO3, 2-3 parts of ZrO2, and mixed to obtain raw material C; 4) taking powder material B and glass powder raw material C and mixing them thoroughly to obtain mixed powder material D; 5) placing the obtained mixed powder D in a muffle furnace and heating it to 750-850° C. for melting for 1 hour, and then cooling it to room temperature to obtain a glass embryo E of a magnesium potassium phosphate cement-phosphate glass mixed material; 6) crushing the glass embryo E into glass blocks with a diameter of 5 mm, and passing through a glass bead electric heating rotary furnace at 550-650° C. to soften the surface and shrink the irregular edges and corners under the action of surface tension while rolling to form a spherical shape; 7) Annealing at 400° C. for 24 hours to obtain the final product, a solidified body F.