Atomic beam collimator based on porous metal adsorption and preparation method thereof

By using atomic beam collimator of foam metal-graphene composite porous material, the problems of collimation and life of atomic beam collimation structures in the prior art in high-throughput applications are solved, achieving high efficiency and stability Atomic beam output.

CN119028624APending Publication Date: 2024-11-26CHINA STATE SHIPBUILDING CORP NO 707 RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411126950.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing atomic beam collimation structure is difficult to ensure high collimation and long life in high throughput applications, especially foam metal adsorbers with high specific surface area are prone to alloy blockage due to active metal atoms, which affects performance.

Method used

Using foam metal-graphene composite porous material as the adsorption layer of the atomic beam collimator, the physical and chemical properties of graphene avoids pore blockage, and combining stainless steel sleeves and capillary structures to form an efficient atomic beam collimator .

Benefits of technology

It significantly improves the adsorption efficiency and service life of the atomic adsorber, and is suitable for a variety of high-coordinate atomic beam application scenarios, ensuring the collimation and long-term stability of the atomic beam.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028624A_ABST
    Figure CN119028624A_ABST
Patent Text Reader

Abstract

The invention relates to an atomic beam collimator based on porous metal adsorption and a preparation method thereof. The atomic beam collimator comprises an atomic nozzle and a tubular adsorption assembly. The front end of the atomic nozzle is coaxially and fixedly connected with the rear end of the tubular adsorption assembly; the atomic nozzle comprises a clamping sleeve and a plurality of capillary tubes with the same length, a regular triangle inner hole is formed in the center of the clamping sleeve, and the capillary tubes with the same length are stacked and pressed in the regular triangle inner hole of the clamping sleeve in the mode that the two ends are aligned. The tubular adsorption assembly comprises a stainless steel sleeve located outside and an adsorption layer fixedly attached to the interior of the sleeve, the adsorption layer is made of a foam metal-graphene composite porous material, and the foam metal-graphene composite porous material is prepared by soaking foam metal in graphene water-phase dispersion liquid. The adopted foam metal has excellent chemical stability after being adsorbed by graphene, pore blockage caused by reaction of active atoms and metal is avoided, the adsorption efficiency of the atom adsorber can be remarkably improved, and the service life of the atom adsorber can be remarkably prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of atomic physics and relates to an atomic beam collimator based on porous metal adsorption and a preparation method thereof. Background Art

[0002] Atomic beams are widely used in the field of atomic physics. Precision measuring devices such as atomic clocks and atomic beam gyroscopes all rely on highly collimated atomic beams to achieve high-precision measurements. People usually choose microtubes with high aspect ratios as emission structures to reduce the divergence angle of atomic beams. However, due to the limitations of device size and processing accuracy, the size of the current emission microtubes is difficult to meet the needs of the devices. Therefore, it is necessary to introduce additional collimation structures to reduce the divergence angle of the atomic beam. The existing collimation structures include multi-segment cascade collimation ports and porous foam metal adsorbers. However, both face various problems when applied to high-flux atomic beam systems. The cascade collimation ports are small in size and it is difficult to ensure the atomic flux. When encountering a large number of active metal atoms, foam metals with high specific surface area easily form alloys, block the surface micropores, reduce the performance of the adsorber, and thus affect its life. Therefore, in the application scenarios of high-flux atomic beams, it is urgent to find an efficient and long-life atomic adsorber to ensure the emission of highly collimated atomic beams. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention proposes an atomic beam collimator based on porous metal adsorption and a preparation method thereof, which can significantly improve the adsorption efficiency and service life of the atomic adsorber and can be applicable to a variety of application scenarios requiring a highly collimated atomic beam.

[0004] One of the above objects of the present invention is achieved by the following technical solution:

[0005] An atomic beam collimator based on porous metal adsorption comprises an atomic nozzle and a tubular adsorption component; the front end of the atomic nozzle is coaxially fixedly connected with the rear end of the tubular adsorption component;

[0006] The atomic nozzle comprises a ferrule and a plurality of capillaries of equal length, wherein an equilateral triangular inner hole is arranged at the center of the ferrule, and the plurality of capillaries of equal length are stacked and pressed in the equilateral triangular inner hole of the ferrule in a manner of aligning both ends;

[0007] The tubular adsorption component includes a stainless steel sleeve located outside and an adsorption layer fixed to the inside of the sleeve. The adsorption layer adopts a foam metal-graphene composite porous material, and the foam metal-graphene composite porous material is prepared by immersing foam metal in a graphene aqueous phase dispersion.

[0008] Moreover, the ferrule adopts a two-part structure, including a ferrule main body part and a pressure block part, and a socket consistent with the shape of the pressure block is provided on the ferrule main body part; the pressure block is inserted into the socket and is bonded to the ferrule main body part on both sides by glue, and the two are spliced ​​to form a cylindrical ferrule with an equilateral triangle inner hole and a circular outer surface.

[0009] Moreover, the capillary is made of stainless steel, copper or glass, and has an inner diameter of 100-500 μm and a length of 10-50 mm.

[0010] Moreover, the front end of the ferrule is provided with an external thread, and the inner end of the stainless steel sleeve is provided with an internal thread, so that the front end of the atomic nozzle and the rear end of the tubular adsorption component form a threaded fit.

[0011] The second objective of the present invention is achieved by the following technical solutions:

[0012] A method for preparing an atomic beam collimator based on porous metal adsorption comprises the following steps:

[0013] Step 1, stacking a plurality of capillaries of equal length in a manner of aligning both ends, placing them in the inner hole of a ferrule and locking them to form an atomic nozzle;

[0014] Step 2: placing the cut foam metal sheet into a graphene dispersion solution for graphene adsorption;

[0015] Step 3, folding the graphene-adsorbed foam metal sheet into a cylindrical shape, and inserting and fixing it in a stainless steel sleeve to form a tubular adsorption component;

[0016] Step 4: coaxially and fixedly connect the rear end of the nozzle front end assembly with the front end of the atomic nozzle to obtain an atomic beam collimator based on porous metal adsorption.

[0017] Moreover, in step 1, before stacking, the capillaries are sequentially placed in water, acetone and isopropanol for cleaning for 15 minutes respectively, and then blown dry with nitrogen. After drying, the transmittance is checked under light, and capillaries with qualified transmittance are selected for stacking.

[0018] Moreover, in step 2, the size of the foam metal after cutting is (10-50mm)×(0.3-1.5mm), the thickness is 0.1-0.3mm, and the porosity can be 50-110PPI; the cut foam metal needs to be cleaned before being placed in the graphene dispersion solution, and the cleaning process is: cleaning with acetone, isopropanol, and deionized water for 15 minutes each.

[0019] Moreover, in step 2, the foam metal selected may be foam copper, foam nickel or foam titanium.

[0020] Moreover, in step 2, adsorption of graphene comprises the following steps:

[0021] 4) diluting the graphene aqueous dispersion with isopropanol, wherein the solid content of the graphene aqueous dispersion may be 5-10 mg / g, and the dilution ratio may be 10-50 mg / L;

[0022] 5) Immerse the cut and cleaned foam metal sheet in the graphene aqueous dispersion solution for 2-5 minutes, and then place the foam metal sheet in clean isopropanol for ultrasonic vibration for 5-10 minutes;

[0023] 6) Repeat the immersion and ultrasonic process 3-5 times to ensure the uniformity of graphene adsorption;

[0024] 7) After taking out the foam metal sheet, blow it dry with nitrogen, put it into an oven at 100-150° C. and bake it for 10-40 minutes to enhance the bonding force between graphene and the foam metal, and take it out after cooling.

[0025] The advantages and positive effects of the present invention are:

[0026] 1. After the foam metal used in the atomic beam collimator of the present invention is adsorbed by graphene, due to the stable physical and chemical properties of graphene, the graphene adsorbed on the metal surface avoids pore blockage caused by the direct reaction of active atoms and metal, which can significantly improve the adsorption efficiency and service life of the atomic adsorber.

[0027] 2. The foam metal-graphene composite porous material of the present invention is simple and quick to process, and the flake graphene can be quickly adsorbed on the porous metal surface. It has a wide range of applications and can be applied to a variety of application scenarios that require highly collimated atomic beams. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a schematic cross-sectional view of an atomic nozzle made by the present invention;

[0029] Figure 2 It is a schematic diagram of manufacturing an atomic nozzle according to the present invention;

[0030] Figure 3 This is a flow chart for preparing the foam metal-graphene composite porous material of the present invention;

[0031] Figure 4 It is a schematic diagram of the structure of the atomic beam collimator of the present invention;

[0032] Figure 5 It is a comparison chart of Doppler sensitive Raman spectra of atomic beam without adsorber and with adsorber;

[0033] Figure 6This is a diagram showing the Raman spectrum width variation of atoms when the atomic beam collimator of the present invention is used for a long time. DETAILED DESCRIPTION

[0034] The structure of the present invention is further described below with reference to the accompanying drawings and by way of examples. It should be noted that the present examples are descriptive rather than restrictive.

[0035] An atomic beam collimator based on porous metal adsorption, see Figure 1-Figure 6 , the invention point is: it includes an atomic nozzle and a tubular adsorption component (also called adsorber). The front end of the atomic nozzle is coaxially fixedly connected with the rear end of the tubular adsorption component. The atomic nozzle includes a ferrule and a plurality of capillaries of equal length, the center of the ferrule is provided with an equilateral triangular inner hole, and the plurality of capillaries of equal length are stacked and pressed in the equilateral triangular inner hole of the ferrule in a manner of being aligned at both ends; the tubular adsorption component includes a stainless steel sleeve located outside and an adsorption layer fixedly attached to the inside of the sleeve, the adsorption layer adopts a foam metal-graphene composite porous material, and the foam metal-graphene composite porous material is prepared by immersing foam metal in a graphene aqueous dispersion.

[0036] The method for preparing the atomic beam collimator based on porous metal adsorption of the present invention comprises the following steps.

[0037] Step 1, stacking a plurality of capillaries 1.2 of equal length in a manner of aligning both ends, and placing them in the inner hole of the ferrule 1.1 for locking, so as to form an atomic nozzle 1;

[0038] Step 2: placing the cut foam metal sheet into a graphene dispersion solution for graphene adsorption;

[0039] Step 3, folding the foam metal sheet after adsorbing graphene into a cylindrical shape, and inserting and fixing it in a stainless steel sleeve to form a tubular adsorption component 2;

[0040] Step 4: coaxially and fixedly connect the rear end of the nozzle front end assembly with the front end of the atomic nozzle to obtain an atomic beam collimator based on porous metal adsorption.

[0041] The method specifically comprises the following operations:

[0042] In the above step 1: the capillary can be made of stainless steel, copper or glass as required, with an inner diameter of 100-500μm and a length of 10-50mm. The ferrule is a cylindrical ferrule with an equilateral triangle inner hole and a circular outer surface, wherein the side length of the equilateral triangle can be 2-10mm. The ferrule adopts a two-part structure, including a ferrule main body part 1.1.2 and a pressing block part 1.1.1. A socket consistent with the shape of the pressing block is provided on the ferrule main body part, and the two are spliced ​​to form a cylindrical ferrule with an equilateral triangle inner hole and a circular outer surface.

[0043] Before stacking, the capillaries need to be cleaned in acetone, isopropanol and deionized water for 15 minutes respectively. Acetone and isopropanol are used to remove organic impurities such as oil, and deionized water is used to clean inorganic pollutants such as dust. Then, they are blown dry with nitrogen to ensure the dispersion of the capillaries and prevent them from sticking together. After drying, check their transmittance under light and select capillaries with qualified transmittance.

[0044] In order to facilitate the fixed connection between the atomic nozzle and the tubular adsorption component, an external thread is processed on the outer surface of the ferrule near the front end, and fixedly connected with the tubular adsorption component by threaded connection.

[0045] In the above step 2: the size of the cut metal foam is (10-50mm)×(0.3-1.5mm), the thickness is 0.1-0.3mm, and the porosity can be 50-110PPI. The cut metal foam needs to be cleaned, and the specific method is: clean it with acetone, isopropanol, and deionized water for 15 minutes each, acetone and isopropanol are used to remove organic impurities such as oil, and deionized water is used to clean inorganic pollutants such as dust. The selected metal foam can be copper foam, nickel foam or titanium foam.

[0046] In the above step 2, the graphene adsorption method is as follows:

[0047] 1. Dilute the graphene aqueous dispersion with isopropanol, wherein the solid content of the graphene aqueous dispersion can be 5-10 mg / g, and the dilution ratio can be 10-50 mg / L;

[0048] 2. Immerse the cut and cleaned foam metal sheet in the graphene aqueous dispersion solution for 2-5 minutes, and then put the foam metal sheet into clean isopropanol for ultrasonic vibration for 5-10 minutes;

[0049] 3. Repeat the above immersion and ultrasonic process 3-5 times to ensure the uniformity of graphene adsorption;

[0050] 4. Take out the foam metal sheet, blow it dry with nitrogen, put it into an oven at 100-150℃ and bake it for 10-40 minutes to enhance the bonding force between graphene and foam metal, and take it out after cooling.

[0051] The physical and chemical stability of the foam metal is improved after graphene adsorption. The graphene covered on the surface avoids pore clogging while retaining the adsorption capacity of the porous metal, thereby increasing its adsorption life for atoms.

[0052] In the above step 3, the specific assembly method of the tubular adsorption component is: bend the foam metal sheet into a cylindrical shape, insert it into the stainless steel sleeve, and fix it at the edge with silicone rubber, wherein a section is reserved at the rear end of the stainless steel sleeve, and an internal thread is processed on the inner hole wall of the section for fastening with the atomic nozzle through threads.

[0053] Example:

[0054] Preparation of atomic beam collimator based on foam copper-graphene adsorption material.

[0055] (1) Place a stainless steel microtube with a diameter of 200 μm and a length of 2 cm in water, acetone, and isopropanol in turn for cleaning for fifteen minutes. After drying with nitrogen, check its transmittance under light. Select unblocked capillaries and stack them in layers in the triangular inner hole of the ferrule. During the stacking process, the capillaries must be parallel to each other. The side length of the regular triangle inner hole is 2 mm. After pressing with a pressing plate, apply quick-drying 502 glue at the joint and lock the ferrule. The prepared atomic nozzle part is placed in a drying cabinet for storage.

[0056] (2) Cut the copper foam with a thickness of 0.15 mm and a porosity of 110 PPI into a 20 mm × 20 mm square, wash it in water, acetone and isopropanol in turn for 15 min, take it out and blow it dry with nitrogen; take out 0.5 g of graphene aqueous dispersion with a solid content of 10 mg / g, dilute it with 50 ml of isopropanol to form a graphene dispersion solution; soak the cleaned copper foam in the solution for 5 min, take it out and ultrasonicate it with 50 ml of isopropanol for 5 min, repeat the ultrasonication and soaking process 3 times, take out the copper foam and blow it dry with nitrogen.

[0057] (3) The treated foam copper sheet is rolled into a tube shape and inserted into a stainless steel cylinder with a diameter of 5 mm and a length of 2 cm. The fitting position is fixed with silicone rubber to complete the preparation of the tubular adsorption component.

[0058] (4) Connect the threads on the ferrule with the threads on the edge of the stainless steel cylinder, ensuring that the center of the launch nozzle and the adsorption tube are aligned.

[0059] The performance of the atomic beam was subsequently evaluated, and the Doppler-sensitive Raman spectra of the atomic beam before and after the adsorption tube collimator were added were as follows: Figure 5 As shown in the figure, the spectral width corresponds to the lateral divergence speed of the atoms. Compared with the atomic beam without the adsorption tube, the Raman spectrum width of the atomic number is significantly narrowed after the adsorption tube is added, indicating that the collimation of the atomic beam is significantly improved after the adsorption tube is added. At the same time, the adsorber also showed good stability. After working continuously for 240 hours, the Raman spectrum width of the atoms did not change significantly. Figure 6 , indicating that the atomic alignment can still be maintained after long-term operation.

[0060] Although the embodiments and drawings of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments and drawings.

Claims

1. An atomic beam collimator based on porous metal adsorption, characterized in that: It comprises an atomic nozzle and a tubular adsorption component; the front end of the atomic nozzle is coaxially fixedly connected with the rear end of the tubular adsorption component; The atomic nozzle comprises a ferrule and a plurality of capillaries of equal length, wherein an equilateral triangular inner hole is arranged at the center of the ferrule, and the plurality of capillaries of equal length are stacked and pressed in the equilateral triangular inner hole of the ferrule in a manner of aligning both ends; The tubular adsorption component includes a stainless steel sleeve located outside and an adsorption layer fixed to the inside of the sleeve. The adsorption layer adopts a foam metal-graphene composite porous material, and the foam metal-graphene composite porous material is prepared by immersing foam metal in a graphene aqueous phase dispersion.

2. The atomic beam collimator based on porous metal adsorption according to claim 1, characterized in that: The ferrule adopts a two-part structure, including a ferrule main body and a pressure block part. A socket consistent with the shape of the pressure block is provided on the ferrule main body; the pressure block is inserted into the socket and is bonded to the ferrule main body on both sides by glue. The two are spliced ​​to form a cylindrical ferrule with an equilateral triangle inner hole and a circular outer surface.

3. The atomic beam collimator based on porous metal adsorption according to claim 1, characterized in that: The capillary is made of stainless steel, copper or glass, with an inner diameter of 100-500 μm and a length of 10-50 mm.

4. The atomic beam collimator based on porous metal adsorption according to claim 1, characterized in that: The front end of the ferrule is provided with an external thread, and the inner end of the stainless steel sleeve is provided with an internal thread, so that the front end of the atomic nozzle and the rear end of the tubular adsorption component form a threaded fit.

5. A method for preparing an atomic beam collimator based on porous metal adsorption as claimed in any one of claims 1 to 4, characterized in that: The steps include: Step 1, stacking a plurality of capillaries of equal length in a manner of aligning both ends, placing them in the inner hole of a ferrule and locking them to form an atomic nozzle; Step 2: placing the cut foam metal sheet into a graphene dispersion solution for graphene adsorption; Step 3, folding the graphene-adsorbed foam metal sheet into a cylindrical shape, and inserting and fixing it in a stainless steel sleeve to form a tubular adsorption component; Step 4: coaxially and fixedly connect the rear end of the nozzle front end assembly with the front end of the atomic nozzle to obtain an atomic beam collimator based on porous metal adsorption.

6. The method for preparing an atomic beam collimator based on porous metal adsorption according to claim 5, characterized in that: In step 1, before stacking, the capillaries are sequentially placed in water, acetone and isopropanol for cleaning for 15 minutes respectively, and then blown dry with nitrogen. After drying, the transmittance is checked under light, and capillaries with qualified transmittance are selected for stacking.

7. The method for preparing an atomic beam collimator based on porous metal adsorption according to claim 5, characterized in that: In step 2, the size of the foam metal after cutting is (10-50mm)×(0.3-1.5mm), the thickness is 0.1-0.3mm, and the porosity can be 50-110PPI; the cut foam metal needs to be cleaned before being placed in the graphene dispersion solution, and the cleaning process is: cleaning with acetone, isopropanol, and deionized water for 15 minutes each.

8. The method for preparing an atomic beam collimator based on porous metal adsorption according to claim 5, characterized in that: In step 2, the foam metal selected is foam copper, foam nickel or foam titanium.

9. The method for preparing an atomic beam collimator based on porous metal adsorption according to claim 5, characterized in that: In step 2, adsorption of graphene comprises the following steps: 1) diluting the graphene aqueous dispersion with isopropanol, wherein the solid content of the graphene aqueous dispersion may be 5-10 mg / g, and the dilution ratio may be 10-50 mg / L; 2) Immerse the cut and cleaned foam metal sheet in the graphene aqueous dispersion solution for 2-5 minutes, and then place the foam metal sheet in clean isopropanol for ultrasonic vibration for 5-10 minutes; 3) Repeat the immersion and ultrasonic process 3-5 times to ensure the uniformity of graphene adsorption; After taking out the foam metal sheet, blow it dry with nitrogen, put it into an oven at 100-150°C and bake it for 10-40 minutes to enhance the bonding force between graphene and foam metal, and take it out after cooling.