HJT low-temperature conductive silver paste, HJT photovoltaic cell and preparation method thereof

By adopting the optimized formula of low-temperature conductive silver paste in HJT photovoltaic cells, it is divided into contact type silver paste and low-solid conductive silver paste, the problem of high cost of low-temperature silver paste in HJT photovoltaic cells is solved, and the amount of silver paste is reduced and Reduced costs.

CN119028632AInactive Publication Date: 2024-11-26DAS SOLAR CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411516145.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The cost of low-temperature silver paste of HJT photovoltaic cells is relatively high, resulting in the reduction of silver paste costs becoming a technical problem that needs to be solved urgently.

Method used

The HJT low-temperature conductive silver paste with an optimized formula is divided into contact type silver paste and low-solid conductive silver paste. The contact type silver paste is in contact with TCO to improve stability, and the low-solid conductive silver paste is installed on the basis of it. Form good electron collection and welding effects, thereby reducing the amount of silver paste.

Benefits of technology

By optimizing the silver paste formula, the amount of silver paste is used is reduced, the consumption of silver is significantly reduced, the cost is reduced, and the efficiency and performance of the battery are guaranteed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028632A_ABST
    Figure CN119028632A_ABST
Patent Text Reader

Abstract

The invention provides HJT low-temperature conductive silver paste, an HJT photovoltaic cell and a preparation method of the HJT photovoltaic cell, and relates to the field of HJT photovoltaic cell preparation. The HJT low-temperature conductive silver paste comprises contact type silver paste and low-solid-content conductive silver paste; the contact type silver paste comprises the following components in percentage by mass: 0.5-1.2% of an organic silicon additive, 71-85% of first silver powder and 14.2-27.5% of a first organic adhesive, wherein the total mass of the contact type silver paste is 100%; the low-solid-content conductive silver paste comprises the following components in percentage by weight: 0.3-0.8% of an organic additive, 45-55% of second silver powder and 44.3-54.7% of a second organic adhesive, wherein the total mass of the low-solid-content conductive silver paste is 100%. According to the low-temperature conductive silver paste provided by the invention, on the premise that the efficiency of an HJT photovoltaic cell is guaranteed, the usage amount of the conductive silver paste is reduced, so that the usage amount of the silver powder is reduced, and finally the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of HJT photovoltaic cell preparation, and in particular to a HJT low-temperature conductive silver paste, a HJT photovoltaic cell and a preparation method thereof. Background Art

[0002] HJT photovoltaic cells are an advanced solar cell technology. This technology combines the advantages of the stability of crystalline silicon cells and the high efficiency of thin-film cells, and is regarded as a strong competitor for the next generation of photovoltaic technology. Compared with traditional solar cells, HJT cells have higher photoelectric conversion efficiency, lower temperature coefficient, and better weak light response performance. These advantages make HJT cells have broad application prospects in many fields.

[0003] However, among the raw materials of HJT photovoltaic cells, the cost of silver paste is second only to silicon raw materials, accounting for about 55% of non-silicon costs. HJT photovoltaic cells are generally produced using a double-sided low-temperature silver paste process; the silver paste is mainly composed of flaky and spherical silver powder, nano-silver powder and organic components, and its metallization temperature is between 200°C and 400°C. The paste is not in contact with the PN junction but in contact with the TCO. Compared with high-temperature silver paste, the development of low-temperature silver paste started late, and the current technical maturity has not reached the level of high-temperature silver paste, and the cost has a premium of about 2,000 yuan / kg relative to high-temperature silver paste. In 2024, the average mass production silver paste consumption of HJT photovoltaic cells will be 120mg / piece, while the average mass production silver consumption of N-TOPcon cells will be 85mg / piece. In view of the high cost of low-temperature silver paste, reducing the cost of silver paste has become a technical problem that needs to be solved urgently. Summary of the invention

[0004] The purpose of this application is to provide a HJT low-temperature conductive silver paste, an HJT photovoltaic cell and a preparation method thereof to solve the above-mentioned problems.

[0005] To achieve the above objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a HJT low-temperature conductive silver paste.

[0006] Including contact type silver paste and low solid conductive silver paste.

[0007] The contact type silver paste, calculated with its own total mass as 100%, includes: 0.5-1.2% of organic silicon auxiliary agent, 71-85% of first silver powder, and 14.2-27.5% of first organic binder.

[0008] The low-solid conductive silver paste, calculated based on its total mass as 100%, includes: 0.3-0.8% of an organic additive, 45-55% of a second silver powder, and 44.3-54.7% of a second organic binder.

[0009] In the contact type silver paste: Preferably, the organosilicon additive comprises polysiloxane.

[0010] Preferably, the purity of the first silver powder is 99.9%.

[0011] Preferably, the first silver powder includes micron-sized flaky silver powder and nano-sized spherical silver powder, the mass percentage of the micron-sized flaky silver powder in the contact type silver paste is 65-75%, and the mass percentage of the nano-sized spherical silver powder in the contact type silver paste is 6-10%.

[0012] Preferably, the first organic binder comprises a high molecular polymer and an organic solvent.

[0013] Preferably, the high molecular polymer includes acrylic resin and epoxy resin.

[0014] Preferably, the mass percentage of the high molecular weight polymer in the first organic binder is 10-15%.

[0015] Preferably, the organic solvent includes at least five of terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0016] Preferably, the mass percentage of the organic solvent in the first organic binder is 85-90%.

[0017] In the low solid conductive silver paste: Preferably, the organic additive comprises polyacrylate.

[0018] Preferably, the second silver powder comprises micron-sized spherical silver powder, and the particle size of the micron-sized spherical silver powder is 1-3 μm.

[0019] Preferably, the second organic binder comprises a high molecular polymer and an organic solvent.

[0020] Preferably, the high molecular polymer includes acrylic resin.

[0021] Preferably, the mass percentage of the high molecular weight polymer in the second organic binder is 15-20%.

[0022] Preferably, the organic solvent includes at least five of terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0023] Preferably, the mass percentage of the organic solvent in the second organic binder is 80-95%.

[0024] In a second aspect, the present application provides a method for preparing a HJT low-temperature conductive silver paste, comprising: The first organic binder and the first silver powder are mixed, dispersed, and ground, and then mixed with the organosilicon additive, and dispersed to obtain the contact type silver paste; The second organic binder and the second silver powder are mixed and dispersed, and then mixed with the organic additive and dispersed to obtain the low-solid conductive silver paste.

[0025] In a third aspect, the present application provides a method for preparing a HJT photovoltaic cell, comprising: printing a contact-type conductive silver paste on a TCO, and overprinting a low-solid conductive silver paste on the contact-type silver paste after drying.

[0026] In a fourth aspect, the present application provides a HJT photovoltaic cell, which is prepared by the HJT photovoltaic cell preparation method described in the third aspect.

[0027] Compared with the prior art, the beneficial effects of this application include: The HJT low-temperature conductive silver paste provided in this application optimizes the formula of silver paste and divides the silver paste into contact type silver paste and low solid conductive silver paste. The contact type silver paste is in contact with TCO, which improves the stability of the contact type silver paste and TCO on the one hand, and the high-density silver paste ensures the conductivity of the contact type silver paste on the other hand; and the low solid conductive silver paste is set on the basis of the contact type silver paste, which can form a good electron collection effect and welding effect. Ultimately, the amount of paste used can be reduced, and the consumption of silver can be greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0029] Figure 1 A schematic diagram of the preparation process of the contact silver paste provided in the embodiment; Figure 2 A schematic diagram of a process flow for preparing a low-solid conductive silver paste provided in an embodiment; Figure 3 This is a front photograph of the HJT photovoltaic cell with a size of 182.2×183.75 prepared in Example 4 of the present application. DETAILED DESCRIPTION

[0030] As used herein: "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0031] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0032] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0033] In these examples, parts and percentages are by mass unless otherwise indicated.

[0034] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.

[0035] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0036] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows: In a first aspect, the present application provides a HJT low-temperature conductive silver paste.

[0037] Including contact type silver paste and low solid conductive silver paste.

[0038] The contact type silver paste, calculated with its own total mass as 100%, includes: 0.5-1.2% of organic silicon auxiliary agent, 71-85% of first silver powder, and 14.2-27.5% of first organic binder.

[0039] In an optional embodiment, the amount of the organosilicon additive can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, or any value between 0.5% and 1.2%; the amount of the first silver powder can be 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, or any value between 71% and 85%; the amount of the first organic binder can be 14.2%, 15.2%, 16.2%, 17.2%, 18.2%, 19.2%, 20.2%, 21.2%, 22.2%, 23.2%, 24.2%, 25.2%, 26.2%, 27.2%, 27.5%, or any value between 14.2% and 27.5%.

[0040] The low-solid conductive silver paste, calculated with its total mass as 100%, includes: 0.3-0.8% of an organic additive, 45-55% of a second silver powder, and 44.3-54.7% of a second organic binder.

[0041] In an optional embodiment, the amount of the organic additive can be 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, or any value between 0.3% and 0.8%; the amount of the second silver powder can be 45%, 46%, 47%, 48%, 49%, 50%, 5%, 52%, 53%, 54%, 55%, or any value between 45% and 55%; the amount of the second organic binder can be 44.3%, 45.3%, 46.3%, 47.3%, 48.3%, 49.3%, 50.3%, 51.3%, 52.3%, 53.3%, 54.3%, 54.7%, or any value between 44.3% and 54.7%.

[0042] In the contact type silver paste: In an optional embodiment, the organosilicon additive includes polysiloxane.

[0043] In an optional embodiment, the purity of the first silver powder is 99.99-99.999%.

[0044] The purity of the first silver powder may be any value between 99.99% and 99.999%.

[0045] In an optional embodiment, the first silver powder includes micron-sized flaky silver powder and nano-sized spherical silver powder, the mass percentage of the micron-sized flaky silver powder in the contact type silver paste is 65-75%, and the mass percentage of the nano-sized spherical silver powder in the contact type silver paste is 6-10%.

[0046] The mass percentage of the micron-sized flaky silver powder in the contact-type silver paste may be 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, or any value between 65 and 75%; the mass percentage of the nano-sized spherical silver powder in the contact-type silver paste may be 6%, 7%, 8%, 9%, 10%, or any value between 6 and 10%.

[0047] In an optional embodiment, the first organic binder includes a high molecular polymer and an organic solvent.

[0048] In an optional embodiment, the high molecular polymer includes acrylic resin and epoxy resin.

[0049] In an optional embodiment, the mass percentage of the high molecular weight polymer in the first organic binder is 10-15%.

[0050] The mass percentage of the high molecular polymer in the first organic binder may be 10%, 11%, 12%, 13%, 14%, 15%, or any value between 10 and 15%.

[0051] In an optional embodiment, the organic solvent includes at least five of terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester dodecahydrate.

[0052] In an optional embodiment, the mass percentage of the organic solvent in the first organic binder is 85-90%.

[0053] The mass percentage of the organic solvent in the first organic binder may be 85%, 86%, 87%, 88%, 89%, 90%, or any value between 85% and 90%.

[0054] In the low solid conductive silver paste: In an alternative embodiment, the organic additive comprises polyacrylate.

[0055] In an optional embodiment, the second silver powder includes micron-sized spherical silver powder, and the particle size of the micron-sized spherical silver powder is 1-3 μm.

[0056] The particle size of the micron-sized spherical silver powder may be 1 μm, 2 μm, 3 μm, or any value between 1 and 3 μm.

[0057] In an optional embodiment, the second organic binder includes a high molecular polymer and an organic solvent.

[0058] In an optional embodiment, the high molecular polymer includes acrylic resin.

[0059] In an optional embodiment, the mass percentage of the high molecular weight polymer in the second organic binder is 15-20%.

[0060] The mass percentage of the high molecular weight polymer in the second organic binder may be 15%, 16%, 17%, 18%, 19%, 20%, or any value between 15 and 20%.

[0061] In an optional embodiment, the organic solvent includes at least five of terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester dodecahydrate.

[0062] In an optional embodiment, the mass percentage of the organic solvent in the second organic binder is 80-95%.

[0063] The mass percentage of the organic solvent in the second organic binder can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, or any value between 80 and 95%.

[0064] In a second aspect, the present application provides a method for preparing a HJT low-temperature conductive silver paste, comprising: The first organic binder and the first silver powder are mixed, dispersed, and ground, and then mixed with the organosilicon additive and dispersed to obtain the contact type silver paste.

[0065] The second organic binder and the second silver powder are mixed and dispersed, and then mixed with the organic additive and dispersed to obtain the low-solid conductive silver paste.

[0066] In a third aspect, the present application provides a method for preparing a HJT photovoltaic cell, comprising: printing a contact-type conductive silver paste on a TCO, and overprinting a low-solid conductive silver paste on the contact-type silver paste after drying.

[0067] In a fourth aspect, the present application provides a HJT photovoltaic cell, which is prepared by the HJT photovoltaic cell preparation method described in the third aspect.

[0068] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0069] Example 1 This embodiment provides a HJT low-temperature conductive silver paste, including a contact type silver paste and a low-solid conductive silver paste, and the preparation method thereof is as follows: 1.1 Preparation of contact silver paste The contact type silver paste, calculated based on its total mass as 100%, includes: 0.8% polysiloxane (silicone oil), 72% 5-6 micron flaky silver powder with a purity of 99.99%, 7% nano-scale spherical silver powder with a purity of 99.99%, 2.424% thermosetting acrylic resin (purchased from Bolier Chemical Co., Ltd., model BM99) (i.e., accounting for 12% of the mass of the first organic binder), 17.776% of pine oil, butyl carbitol, butyl carbitol acetate, and tributyl citrate (i.e., accounting for 88% of the mass of the first organic binder).

[0070] The preparation process of contact silver paste is as follows: Figure 1 As shown, pinene alcohol, butyl carbitol, butyl carbitol acetate, tributyl citrate and acrylic resin are first added in a ratio of 25:10:45:20 and mixed to obtain a first organic adhesive; then the first organic adhesive is mixed with nano-scale silver powder and dispersed by a disperser with a disperser speed of 600 r / min for 2 hours to obtain a first powder.

[0071] Add micron-sized flaky silver powder to the first powder, set the speed of the disperser to 700 r / min, disperse for 1.5 hours, and grind through a three-roll mill after dispersion to obtain a second powder with a particle size of less than 10 μm.

[0072] Add polysiloxane to the second powder, set the disperser speed to 500 r / min, and disperse for 1 hour to obtain a contact type silver paste.

[0073] 1.2 Preparation of low solid conductive silver paste The low-solid conductive silver paste, calculated based on its total mass as 100%, includes: 0.5% polyacrylate, 48% spherical silver powder of 1-3 microns with a purity of 99.9%, 7.725% N200 (i.e., accounting for 15% of the mass of the second organic binder), and 43.775% of pineneol, butyl carbitol, butyl carbitol acetate, and tributyl citrate (i.e., accounting for 85% of the mass of the second organic binder).

[0074] The preparation process of low solid conductive silver paste is as follows: Figure 2 As shown, pinene alcohol, butyl carbitol, butyl carbitol acetate, tributyl citrate and N200 are first mixed to obtain a second organic binder; then the second organic binder is mixed with micron-sized spherical silver powder, and dispersed by a disperser with a disperser speed of 600 r / min for 2 hours to obtain a third powder after dispersion.

[0075] Add polyacrylate to the third powder, set the disperser speed to 600 r / min, and disperse for 2 hours to obtain a low-solid conductive silver paste.

[0076] Example 2 This embodiment provides a HJT low-temperature conductive silver paste, including a contact type silver paste and a low-solid conductive silver paste, and the preparation method thereof is as follows: 2.1 Preparation of contact silver paste The contact type silver paste, calculated based on its total mass as 100%, includes: 1% polysiloxane (silicone oil), 73% 5-6 micron flaky silver powder with a purity of 99.9%, 8% nano-scale spherical silver powder with a purity of 99.9%, 2.34% acrylic resin (i.e., 13% of the mass of the first organic binder), and 15.66% of pine oil, butyl carbitol, butyl carbitol acetate, and tributyl citrate (i.e., 87% of the mass of the first organic binder).

[0077] First, pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate and acrylic resin are mixed in a ratio of 25:10:45:20 to obtain a first organic adhesive; then the first organic adhesive is mixed with nano-scale silver powder and dispersed by a disperser with a disperser speed of 600 r / min for 2 hours to obtain a fourth powder after dispersion.

[0078] Add micron-sized flaky silver powder to the fourth powder, set the speed of the disperser to 700 r / min, disperse for 1.5 hours, and grind with a three-roll mill after dispersion to obtain a fifth powder with a particle size of less than 10 μm.

[0079] Add polysiloxane to the fifth powder, set the speed of the disperser to 500 r / min, and disperse for 1 hour to obtain a contact type silver paste.

[0080] 2.2 Preparation of low solid conductive silver paste The low-solid conductive silver paste, calculated based on its total mass as 100%, includes: 0.6% polyacrylate, 50% spherical silver powder of 1-3 microns with a purity of 99.9%, 7.904% N200 (i.e., accounting for 16% of the mass of the second organic binder), and 41.496% of pineneol, butyl carbitol, butyl carbitol acetate, and tributyl citrate (i.e., accounting for 84% of the mass of the second organic binder).

[0081] First, pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate and N200 are mixed to obtain a second organic binder; then the second organic binder is mixed with micron-sized spherical silver powder, and dispersed by a disperser with a disperser speed of 600 r / min for 2 hours to obtain a sixth powder after dispersion.

[0082] Add polyacrylate to the sixth powder, set the speed of the disperser to 600 r / min, and disperse for 2 hours to obtain a low-solid conductive silver paste.

[0083] Example 3 This embodiment provides a HJT low-temperature conductive silver paste, including a contact type silver paste and a low-solid conductive silver paste, and the preparation method thereof is as follows: 3.1 Preparation of contact silver paste The contact type silver paste, calculated based on its total mass as 100%, includes: 1.2% polysiloxane (silicone oil), 75% 5-6 micron flaky silver powder with a purity of 99.9%, 10% nano-scale spherical silver powder with a purity of 99.9%, 1.794% acrylic resin (i.e., 13% of the mass of the first organic binder), and 12.006% of pine oil, butyl carbitol, butyl carbitol acetate, and tributyl citrate (i.e., 87% of the mass of the first organic binder).

[0084] First, pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate and acrylic resin are mixed to obtain a first organic adhesive; then the first organic adhesive is mixed with nano-scale silver powder and dispersed by a disperser with a disperser speed of 600 r / min for 2 hours to obtain a seventh powder after dispersion.

[0085] Add micron-sized flaky silver powder to the seventh powder, set the speed of the disperser to 700 r / min, disperse for 1.5 hours, and grind with a three-roller mill after dispersion to obtain an eighth powder with a particle size of less than 10 μm.

[0086] Add polysiloxane to the eighth powder, set the disperser speed to 500 r / min, and disperse for 1 hour to obtain a contact type silver paste.

[0087] 3.2 Preparation of low solid conductive silver paste The low-solid conductive silver paste, calculated based on its total mass as 100%, includes: 0.8% polyacrylate, 55% spherical silver powder of 1-3 microns with a purity of 99.9%, 7.072% N200 (i.e., accounting for 16% of the mass of the second organic binder), and 37.128% of pineneol, butyl carbitol, butyl carbitol acetate, and tributyl citrate (i.e., accounting for 84% of the mass of the second organic binder).

[0088] First, pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate and N200 are mixed to obtain a second organic binder; then the second organic binder is mixed with micron-sized spherical silver powder, and dispersed by a disperser with a disperser speed of 600 r / min for 2 hours to obtain a ninth powder after dispersion.

[0089] Add polyacrylate to the ninth powder, set the speed of the disperser to 600 r / min, and disperse for 2 hours to obtain a low-solid conductive silver paste.

[0090] Example 4 This embodiment provides a HJT photovoltaic cell made from the HJT low-temperature conductive silver paste obtained in Example 1, and the preparation method is as follows: The contact silver paste prepared in Example 1 was screen printed with 520 mesh on a single crystal HJT silicon wafer with a specification of 182.2 mm × 183.75 mm to form a silver fine grid with a wet weight of 18 mg. The silver paste was then dried in a drying furnace at 250 degrees Celsius. The battery cell after the printed contact silver paste fine grid was taken out and dried was used to start printing low-solid conductive silver paste. The printing was performed through 520 mesh screen printing. Through precise positioning, the printed low-solid conductive silver paste was required to be overprinted on the fine grid formed by the contact silver paste. The wet weight was 22 mg. The battery after printing B paste was dried at a temperature set to 220°C.

[0091] The other steps are carried out by conventional methods, and finally a finished HJT photovoltaic cell is prepared. The prepared HJT photovoltaic cell is as follows Figure 3 shown.

[0092] Example 5 This embodiment provides a HJT photovoltaic cell made from the HJT low-temperature conductive silver paste obtained in Example 2, and the preparation method is as follows: The contact silver paste prepared in Example 1 was screen printed with 520 mesh on a single crystal HJT silicon wafer with a specification of 182.2 mm × 183.75 mm to form a silver fine grid with a wet weight of 18.3 mg. The silver paste was then dried in a drying furnace at 250 degrees Celsius. The battery cell after the printed contact silver paste fine grid was taken out and dried was used to start printing low-solid conductive silver paste. The printing was performed through 520 mesh screen printing. Through precise positioning, the printed low-solid conductive silver paste was required to be overprinted on the fine grid formed by the contact silver paste. The wet weight was 22.2 mg. The battery after printing B paste was dried at a temperature set to 220°C.

[0093] Conventional methods are used in other steps to ultimately produce a finished HJT photovoltaic cell.

[0094] Example 6 This embodiment provides a HJT photovoltaic cell made from the HJT low-temperature conductive silver paste obtained in Example 3, and the preparation method is as follows: The contact silver paste prepared in Example 1 was screen printed with 520 mesh on a single crystal HJT silicon wafer with a specification of 182.2 mm × 183.75 mm to form a silver fine grid with a wet weight of 19.5 mg. The silver paste was then dried in a drying furnace at 250 degrees Celsius. The battery cell after the printed contact silver paste fine grid was taken out and dried was used to start printing low-solid conductive silver paste. The printing was performed through 520 mesh screen printing. Through precise positioning, the printed low-solid conductive silver paste was required to be overprinted on the fine grid formed by the contact silver paste. The wet weight was 23.2 mg. The battery after printing B paste was dried at a temperature set to 220°C.

[0095] Conventional methods are used in other steps to ultimately produce a finished HJT photovoltaic cell.

[0096] Comparative Example 1 This comparative example provides a HJT photovoltaic cell made from a conventional HJT low-temperature conductive silver paste. The silver paste used is a conventional HJT low-temperature conductive silver paste. The preparation method is as follows: The materials are calculated based on their total mass as 100%, including: 0.7% polysiloxane, 78% flaky silver powder with a purity of 99.9%, 2% nano silver powder with a purity of 99.99%, 1.93% acrylic resin, and 17.37% of pine oil, butyl carbitol, butyl carbitol acetate, tributyl citrate, and Span 85.

[0097] First, pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate, and Span 85 were added in a ratio of 15:15:50:15:5 and mixed to obtain an organic binder; the organic binder was mixed with nano silver powder and dispersed using a disperser with a dispersant speed of 600 r / min for 2 hours, and then flaky silver powder was added, the dispersant speed was set to 700 r / min for 1.5 hours, and after dispersion, it was ground by a three-roller mill to obtain a powder with a particle size of less than 10 μm. Polysiloxane was added to the powder to obtain a conventional HJT low-temperature conductive silver paste.

[0098] The above conventional HJT low-temperature conductive silver paste is screen-printed with 520 mesh on a single crystal HJT silicon wafer with a specification of 182.2 mm×183.75 mm to form a silver fine grid with a wet weight of 41.2 mg, and then dried in a drying furnace at 250 degrees Celsius.

[0099] Conventional methods are used in other steps to finally prepare HJT photovoltaic cells.

[0100] Comparative Example 2 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that only contact silver paste printing is used, and the other steps use conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0101] Comparative Example 3 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that only low-solid conductive silver paste printing is used, and the other steps adopt conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0102] Comparative Example 4 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that the organosilicon additive polysiloxane is replaced by BYK111 (other organosilicon additives), and the other steps adopt conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0103] Comparative Example 5 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that, in preparing the contact type silver paste, only micron-sized flake silver powder is used in the first silver powder (i.e., the amount of micron-sized flake silver powder is 79% of the total mass of the contact type silver paste), and the other steps use conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0104] Comparative Example 6 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that, in preparing the contact type silver paste, only nano-scale spherical silver powder is used in the first silver powder (i.e., the amount of nano-scale spherical silver powder is 79% of the total mass of the contact type silver paste), and the other steps use conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0105] Comparative Example 7 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that, in the preparation of the contact silver paste, only the high molecular polymer acrylic resin is replaced by other materials in the first organic adhesive, and the other steps adopt conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0106] Comparative Example 8 This comparative example provides a HJT photovoltaic cell made from a HJT low-temperature conductive silver paste: The only difference from Example 4 is that, in the preparation of the low-solid conductive silver paste, only the high molecular polymer N200 is replaced by other materials in the second organic binder, and the other steps adopt conventional methods to prepare HJT photovoltaic cells and test their electrical properties.

[0107] Experimental example The electrical properties of the HJT photovoltaic cells prepared in Examples 4 to 6 and Comparative Examples 1 to 8 are shown in Table 1: Table 1 Electrical properties of different treatments

[0108] As shown in Table 1, the technical solution of the present application can reduce the amount of slurry used while ensuring that the overall efficiency remains unchanged, thereby reducing the overall cost by more than 30%.

[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0110] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A HJT low temperature conductive silver paste, characterized in that: Including contact silver paste and low solid conductive silver paste; The contact type silver paste is calculated based on its total mass as 100%, including: Silicone additive 0.5~1.2%, first silver powder 71~85%, first organic binder 14.2~27.5%; The low-solid conductive silver paste, calculated with its total mass as 100%, includes: Organic additive 0.3~0.8%, second silver powder 45~55%, second organic binder 44.3~54.7%.

2. The HJT low temperature conductive silver paste according to claim 1, characterized in that: One or more of the following conditions are met: a. In the contact type silver paste, the organosilicon additive comprises polysiloxane; b. The purity of the first silver powder is 99.99~99.999%; c. The first silver powder includes micron-sized flaky silver powder and nano-sized spherical silver powder, the mass percentage of the micron-sized flaky silver powder in the contact type silver paste is 65-75%, and the mass percentage of the nano-sized spherical silver powder in the contact type silver paste is 6-10%.

3. The HJT low temperature conductive silver paste according to claim 1, characterized in that: The first organic binder includes a high molecular polymer and an organic solvent.

4. The HJT low temperature conductive silver paste according to claim 3, characterized in that: Satisfy one or more of the following conditions d~g: d. The polymer includes acrylic resin and epoxy resin; e. The mass percentage of the polymer in the first organic binder is 10 to 15%; f. The organic solvent comprises at least five of pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve; g. The mass percentage of the organic solvent in the first organic binder is 85-90%.

5. The HJT low temperature conductive silver paste according to claim 1, characterized in that: The low-solid conductive silver paste satisfies at least one of the following conditions: h. The organic additive comprises a polyacrylate; i. The second silver powder includes micron-sized spherical silver powder, and the particle size of the micron-sized spherical silver powder is 1-3 μm.

6. The HJT low temperature conductive silver paste according to claim 1, characterized in that: The second organic binder includes a high molecular polymer and an organic solvent.

7. The HJT low-temperature conductive silver paste according to claim 6, characterized in that: Satisfy one or more of the following conditions j~m: j. The polymer comprises an acrylic resin; k. The mass percentage of the polymer in the second organic binder is 15 to 20%; l. The organic solvent comprises at least five of pineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve; m. The mass percentage of the organic solvent in the second organic binder is 80~85%.

8. A method for preparing the HJT low-temperature conductive silver paste according to any one of claims 1 to 7, characterized in that: include: The first organic binder and the first silver powder are mixed, dispersed, and ground, and then mixed with the organosilicon additive, and dispersed to obtain the contact type silver paste; The second organic binder and the second silver powder are mixed and dispersed, and then mixed with the organic additive and dispersed to obtain the low-solid conductive silver paste.

9. A method for preparing a HJT photovoltaic cell, characterized in that: include: The contact type conductive silver paste is printed on the TCO, and after drying, the low solid conductive silver paste is overprinted on the contact type silver paste.

10. A HJT photovoltaic cell, characterized in that: The HJT photovoltaic cell is prepared by the method for preparing the HJT photovoltaic cell described in claim 9.

Citation Information

Patent Citations

  • Method for printing metal gate line

    CN102332494A

  • Method for manufacturing solar cell grid line

    CN104377272A

  • Printing method for silver line of toughened glass and toughened glass

    CN106494105A

  • Graded front side silver paste for crystalline silicon solar cell and preparation method of graded front side silver paste

    CN110415858A

  • N-type TOPCon battery back polishing silver paste and preparation method and application thereof

    CN114373568A