Non-polar two-dimensional GaN in-situ epitaxial preparation method
By conducting competitive nucleation and annealing-induced reconstruction on the SiC substrate, a non-polar two-dimensional GaN film was prepared, which solved the problems of large thickness, uneven mass and many defects in the existing non-polar GaN film, and achieved the High carrier mobility and excellent optical properties improve the performance of electronic devices.
Patent Information
- Application Number
- CN202411128530.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The existing non-polar GaN films have problems such as thick thickness, uneven mass and many defects, which affect the performance of materials and devices.
Non-polar two-dimensional GaN in situ epitaxial preparation method, including competitive nucleation of Ga polar GaN3 and N polar Ga3N on SiC substrate, stably link to form a single-layer GaN film, and induced structural reconstruction by annealing. , a non-polar two-dimensional GaN film was obtained.
The preparation of non-polar GaN film is realized, which weakens the internal electric field and reduces the scattering of the surface state on carriers. It has the characteristics of non-layered two-dimensional material, has thin thickness, large band gap, high carrier mobility and optical Excellent properties, improving device performance and stability.
Smart Images

Figure CN119028806A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor technology, relates to a two-dimensional semiconductor process, and particularly relates to a method for preparing non-polar two-dimensional GaN by in-situ epitaxy. Background Art
[0002] As a typical representative of the third-generation semiconductor technology, GaN technology is an important semiconductor material in the field of electronic information. It has the advantages of wide bandgap and high carrier mobility, and is widely used in many fields.
[0003] At present, GaN prepared by methods such as metal organic chemical vapor deposition (MOCVD), hydrogen plasma vapor exfoliation (HPVE) and molecular beam epitaxy (MBE) is mainly Ga polar. There are also reports of N polar GaN prepared by nitriding the surface of the substrate. Due to its large spontaneous polarization, this polar GaN material can introduce characteristics such as two-dimensional electron gas (2DEG) in electronic devices such as high electron mobility transistors (HEMT), greatly improving device performance. However, whether it is Ga polarity or N polarity GaN material, the existence of its polarity also introduces interface surface states. This surface state trap effect will produce a scattering effect on carriers, affecting the performance of materials and devices.
[0004] The existing method for preparing non-polar GaN materials mainly reduces the internal electric field of non-polar GaN and reduces the quantum restricted Stark effect (QRSE). For example, by controlling the crystal orientation of epitaxial growth, non-polar GaN materials are prepared along GaN (10-10). However, the basic structure of this non-polar GaN material with a specific crystal orientation is still derived from traditional polar GaN. The specific crystal orientation easily destroys the integrity of the crystal structure, resulting in problems such as thick thickness, uneven quality, and many defects.
[0005] For example, Kolobov et al. predicted a non-polar two-dimensional structure of GaN in their paper "Instability and Spontaneous Reconstruction of Few-Monolayer Thick GaN Graphitic Structures". Unlike the traditional bulk polar GaN material, this new GaN exhibits non-layered two-dimensional 4|8 configuration characteristics. This new non-polar two-dimensional 4|8GaN can exist stably at a thickness of more than a dozen atomic layers and has excellent optoelectronic properties comparable to traditional GaN. However, there is currently no stable and effective preparation method that can achieve the preparation of this non-polar two-dimensional GaN. Summary of the invention
[0006] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for in-situ epitaxial preparation of non-polar two-dimensional GaN to solve the problems of thick thickness, uneven quality, and many defects in existing non-polar GaN films, so that it can be used in high-performance electronic devices.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing non-polar two-dimensional GaN in-situ epitaxially comprises the following steps:
[0009] Step 1, preparing a SiC substrate having a C-terminal surface;
[0010] Step 2, performing competitive polar nucleation of Ga-polar GaN3 and N-polar Ga3N on the C-terminal surface;
[0011] Step 3, stably linking the nucleation structure to obtain a single-layer GaN film;
[0012] Step 4, continuing to prepare a GaN film on the single-layer GaN film, and then annealing to induce structural reconstruction and stabilize it to obtain a non-polar two-dimensional GaN film.
[0013] In one embodiment, in step 1, the SiC substrate is placed in a hydrogen environment for annealing, then cleaned, and then placed in a hydrogen-argon mixed gas for hydrogen etching, and the SiC substrate is polished by chemical mechanical polishing to prepare a SiC substrate with a C-terminal surface.
[0014] In one embodiment, the competitive polar nucleation in step 2 is carried out by using any one of metal organic chemical vapor deposition, hydrogen plasma vapor exfoliation and molecular beam epitaxy.
[0015] In one embodiment, the metal organic chemical vapor deposition is used to achieve competitive polar nucleation, and the method is as follows:
[0016] The SiC substrate with C-terminal surface was placed in the reaction chamber, H2 was introduced as the carrier gas, and the reaction chamber was evacuated to a pressure of 10 -7 ~10 -8 Torr, the reaction chamber is heated to 800-1000°C by radio frequency induction, Ga source and N source are introduced, and the pressure of the reaction chamber is maintained at 500 Torr. The epitaxial time is 5-10 minutes. Combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface;
[0017] The hydrogen plasma gas phase exfoliation is used to achieve competitive polar nucleation, and the method is as follows:
[0018] The SiC substrate with C-terminal surface was placed in the reaction chamber, H2 and N2 were introduced as carrier gas, HCl gas was used as reaction gas, and the reaction chamber was first evacuated to a pressure of 10 -7 ~10 -8 Torr, heating the reaction chamber to 1000-1050°C, introducing Ga source and N source, the epitaxial time is 10-15 minutes, and combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface;
[0019] The competitive polar nucleation is achieved by using the molecular beam epitaxy as follows:
[0020] The SiC substrate with C-terminal surface was placed in the reaction chamber and evacuated to 10 -7 ~10 -8 Torr, Ga source and N source are introduced, the temperature is set to 700-800°C, the epitaxial time is 5-10 min, and combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface.
[0021] In one embodiment, the real-time monitoring technology is a high energy electron diffraction technology, which monitors the formation of Ga polar tripod GaN3 and N polar tripod Ga3N on the C terminal surface to simultaneously form nucleation islands.
[0022] In one embodiment, in step 3, based on step 2, metal organic chemical vapor deposition, hydrogen plasma vapor stripping or molecular beam epitaxial deposition is continued, the temperature and pressure of metal organic chemical vapor deposition and hydrogen plasma vapor stripping remain unchanged, the temperature of the reaction chamber of molecular beam epitaxy is increased to 800-900°C, and the pressure remains unchanged, so that the Ga polar GaN3 and N polar Ga3N nucleation clusters and nucleation islands on the C terminal surface are stably linked to prepare a single-layer GaN film.
[0023] In one embodiment, in step 4, on the basis of step 3, metal organic chemical vapor deposition, hydrogen plasma gas phase stripping or molecular beam epitaxial deposition is continued, the temperature of the reaction chamber of the metal organic chemical vapor deposition is increased to 1000-1100°C, and the rate of introducing Ga source and N source is increased, and the pressure remains unchanged; the temperature of the reaction chamber of the hydrogen plasma gas phase stripping is increased to 1050-1150°C, and the rate of introducing Ga source and N source is increased, and the pressure remains unchanged; the temperature of the reaction chamber of the molecular beam epitaxy is increased to 900-1100°C, and the pressure remains unchanged; a GaN film with a certain thickness is prepared, and then annealed at 800-1000°C to induce its structural reconstruction and stabilize it, thereby completing the preparation of a non-polar two-dimensional GaN film.
[0024] In one embodiment, in step 2, in metal organic chemical vapor deposition, the rates of introducing Ga source and N source are 20 umol / min and 0.05 umol / min respectively; in hydrogen plasma gas phase stripping, the rates of introducing Ga source and N source are 100 mL / min and 1000 mL / min respectively;
[0025] In step 3, the epitaxial time of continuing metal organic chemical vapor deposition is 10 to 15 minutes, and the epitaxial time of continuing hydrogen plasma vapor phase stripping is 15 to 20 minutes;
[0026] In the step 4, the metal organic chemical vapor deposition is continued, the rates of introducing the Ga source and the N source are 25umol / min and 0.1umol / min respectively, and the epitaxial time is 20 to 25min; the hydrogen plasma gas phase stripping is continued, the rates of introducing the Ga source and the N source are 120mL / min and 1200mL / min respectively, and the epitaxial time is 20 to 25min; the molecular beam epitaxy is continued, and the epitaxial time is 20 to 30min.
[0027] In one embodiment, the thickness of the non-polar two-dimensional GaN film is controlled within 2 nm.
[0028] The non-polar two-dimensional GaN film obtained by the present invention can be used for future advanced nano-level electronics, optoelectronic devices or high-mobility carrier LEDs.
[0029] Compared with the existing non-polar GaN film, the GaN film prepared by the present invention has the following advantages: (1) the preparation of non-polar GaN film is realized, the internal electric field of GaN is weakened, and the scattering of carriers by surface states is reduced; (2) the prepared non-polar GaN exhibits the characteristics of non-layered two-dimensional materials, and has the characteristics of thin two-dimensional material thickness, large band gap, high carrier mobility and excellent optical properties.
[0030] In summary, the GaN film prepared by the present invention can achieve intralayer non-polarity, high carrier mobility, low interface state defect density and controllable atomic-level thickness, further improving device performance and its stability and reliability, and can be used in high electron mobility transistors (HEMTs), light-emitting diodes, photodetectors and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a flow chart of the in-situ epitaxial preparation of non-polar two-dimensional GaN according to the present invention. DETAILED DESCRIPTION
[0032] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.
[0033] As mentioned above, existing Ga-polar and N-polar GaN films will generate spontaneous polarization and piezoelectric polarization electric fields at the GaN-based heterojunction interface, which will separate electrons and holes in the quantum well, resulting in lower internal quantum efficiency; at the same time, it will lead to a larger interface state defect density, enhance the scattering of carriers, and affect the performance of electronic devices. At the same time, non-polar GaN films such as (10-10) and (11-20) are still derived from traditional polar GaN crystal structures, and still have problems such as thick thickness, uneven quality, and many defects.
[0034] To this end, the present invention provides a method for in-situ epitaxial preparation of non-polar two-dimensional GaN, such as Figure 1 As shown, the preparation process mainly includes:
[0035] Step (1), pre-treating the SiC substrate.
[0036] The purpose of this step is to prepare a SiC substrate with a C-terminal surface.
[0037] Step (2), competitive polar nucleation.
[0038] The purpose of this step is to perform competitive polar nucleation of Ga-polar GaN3 and N-polar Ga3N on the C-terminal surface of the SiC substrate.
[0039] Step (3), preparing a single-layer GaN film.
[0040] The purpose of this step is to stabilize the nucleation structure obtained in step (2).
[0041] Step (4), preparing a non-polar two-dimensional GaN thin film.
[0042] The purpose of this step is to form a non-polar two-dimensional GaN film with a stable structure.
[0043] The preparation principle of the present invention can be described as follows:
[0044] In an N-rich and Ga-poor atmosphere, GaN tends to nucleate on the substrate surface through tripod GaN3 with Ga polarity, while in a Ga-rich and N-poor atmosphere, GaN tends to nucleate on the substrate surface through tripod Ga3N with N polarity. Therefore, GaN with Ga polarity and N polarity can be formed in situ at the C atom terminal on the surface of the SiC substrate. When more Ga and N atoms are introduced, these two polarities of GaN will be connected by independent nucleation islands to form a single-layer GaN film. There is a polarity competition between the single-layer GaN films, which will induce its structural reconstruction.
[0045] Therefore, compared with the current mainstream Ga polarity and N polarity GaN films, the non-polar two-dimensional GaN film prepared by the present invention does not have intrinsic polarity, and will not introduce factors such as polarization electric field and interface state that limit the carrier transport capacity, thereby effectively reducing the scattering effect of the interface state trap effect on the carrier. Compared with the non-polar (10-10) and (11-20) GaN films, the non-polar two-dimensional GaN prepared by the present invention has the advantages of atomic-level thickness, large band gap, high carrier mobility, excellent optical properties and the like of two-dimensional materials through the two-dimensional structure of in-situ epitaxy, effectively overcoming the disadvantages of large thickness, uneven crystal quality, and more internal defects of non-polar (10-10) and (11-20) GaN films, and can be used for future advanced nano-level electronic and optoelectronic devices such as micro-nano HEMT or high-mobility carrier LED. As microelectronics enter micro-nano technology, the non-polar two-dimensional GaN film provided in the present invention can be compatible with the characteristics of two-dimensional materials, effectively reduce the device size, and break through the polarity of Moore's Law.
[0046] In an embodiment of the present invention, step (1) pre-treats the SiC substrate to use its C-terminated surface as the epitaxial surface, and its specific implementation method can be described as follows:
[0047] The SiC substrate was placed in a hydrogen environment for annealing, and then cleaned in deionized water, butyl acetate, acetone, ethanol and 50°C ultrasonic cleaning.
[0048] The ultrasonically cleaned SiC substrate is placed in a hydrogen-argon mixed gas for hydrogen etching. For example, the mixed gas is 95% Ar and 5% H2 by volume. After the hydrogen etching is completed, the SiC substrate needs to be precisely polished by chemical mechanical polishing (CMP), and the surface of the SiC substrate is observed by atomic force microscopy (AFM) to prepare a SiC substrate with a C-terminal surface for subsequent use.
[0049] In an embodiment of the present invention, the competitive polar nucleation in step (2) is carried out by any one of metal organic chemical vapor deposition (MOCVD), hydrogen plasma vapor exfoliation (HPVE) and molecular beam epitaxy (MBE).
[0050] Specifically, metal organic chemical vapor deposition (MOCVD) is used to achieve competitive polar nucleation, and the method is as follows:
[0051] The SiC substrate with a C-terminal surface was placed in a reaction chamber, and high-purity H2 was introduced as a carrier gas, trimethylgallium as a Ga source, and NH3 as a N source. The reaction chamber was first evacuated to a pressure of 10 -7 ~10 -8Torr, the reaction chamber is heated to 800-1000°C by radio frequency induction heating, trimethylgallium and NH3 are introduced at 20umol / min and 0.05umol / min, and H2 is used as the ambient gas to keep the reaction chamber pressure at 500Torr. The epitaxial time is 5-10min, and combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface.
[0052] Competitive polar nucleation was achieved using hydrogen plasma vapor exfoliation (HPVE) as follows:
[0053] Place the SiC substrate with a C-terminal surface into a reaction chamber, introduce high-purity H2 and N2 as carrier gases, high-purity HCl gas as reaction gas, trimethylgallium as Ga source and NH3 as N source, respectively. First, evacuate the reaction chamber to a pressure of 10 -7 ~10 -8 Torr, heat the reaction chamber to 1000-1050°C, introduce trimethylgallium at 100mL / min and NH3 at 1000mL / min, the epitaxial time is 10-15min, and combine with real-time monitoring technology to simultaneously nucleate Ga-polar GaN3 and N-polar Ga3N on the C-terminal surface.
[0054] Competitive polar nucleation was achieved using molecular beam epitaxy (MBE) as follows:
[0055] The SiC substrate with C-terminal surface was placed in the reaction chamber and evacuated to 10 -7 ~10 -8 Torr (more preferably 10 -7 Torr), introduce Ga source and N source, set the temperature to 700-800°C (more preferably 700°C), the epitaxial time to 5-10min, and combine with real-time monitoring technology to simultaneously nucleate Ga-polar GaN3 and N-polar Ga3N on the C-terminal surface.
[0056] In an embodiment of the present invention, a real-time monitoring technology such as high energy electron diffraction (RHEED) is used to perform simultaneous nucleation of Ga-polar GaN3 and N-polar Ga3N clusters on the C-terminal surface of a SiC substrate. In the high energy electron diffraction technology, when a high energy electron beam is incident on a crystal sample at a specific angle, the electrons interact with the atoms in the crystal to generate elastic scattering waves. These scattered waves interfere with each other to form an electron diffraction pattern corresponding to the crystal structure. The formation of Ga-polar tripod GaN3 and N-polar tripod Ga3N on the C-terminal surface is monitored to simultaneously form nucleation islands.
[0057] In the embodiment of the present invention, step (3) is to continue metal organic chemical vapor deposition, hydrogen plasma vapor exfoliation or molecular beam epitaxy deposition on the basis of step (2). That is, when step (2) adopts metal organic chemical vapor deposition, step (3) also preferably adopts metal organic chemical vapor deposition, which is obviously the preferred process route, and the same applies to other cases.
[0058] Specifically, when metal organic chemical vapor deposition is used in step (2), the temperature and pressure conditions of the metal organic chemical vapor deposition in step (2) are kept unchanged in step (3), and the epitaxial time is 10 to 15 minutes, so that the Ga polar GaN3 and N polar Ga3N nucleation clusters and nucleation islands on the C terminal surface can be stably linked to prepare a single-layer GaN film.
[0059] When hydrogen plasma vapor stripping is used in step (2), the temperature and pressure conditions of the hydrogen plasma vapor stripping in step (2) are kept unchanged in step (3), and the epitaxial time is 15 to 20 minutes, so that the Ga-polar GaN3 and N-polar Ga3N nucleation clusters and nucleation islands on the C-terminal surface can be stably linked to prepare a single-layer GaN film.
[0060] When molecular beam epitaxy is used in step (2), the molecular beam epitaxy pressure conditions of step (2) are kept unchanged in step (3), but the temperature of the reaction chamber needs to be increased to 800-900°C (preferably 800°C) so that the Ga-polar GaN3 and N-polar Ga3N nucleation clusters and nucleation islands on the C-terminal surface are stably linked to prepare a single-layer GaN film.
[0061] In this step, the quality of the film can be detected by high energy electron diffraction (RHEED).
[0062] In the embodiment of the present invention, step (4) is to continue metal organic chemical vapor deposition, hydrogen plasma vapor exfoliation or molecular beam epitaxial deposition on the basis of step (3). That is, when step (3) adopts metal organic chemical vapor deposition, step (3) also preferably adopts metal organic chemical vapor deposition, which is obviously the preferred process route, and the same applies to other cases.
[0063] Specifically, when metal organic chemical vapor deposition is used in step (3), the pressure conditions of the metal organic chemical vapor deposition in step (3) are kept unchanged in step (4), but the temperature of the reaction chamber needs to be increased to 1000-1100° C., and the rates of introducing the Ga source and the N source are increased, for example, from 20 umol / min to 25 umol / min, and from 0.05 umol / min to 0.1 umol / min, respectively. The epitaxial time is generally 20-25 min to prepare a GaN film with a certain thickness.
[0064] When hydrogen plasma gas phase stripping is used in step (3), the pressure condition of hydrogen plasma gas phase stripping in step (3) is maintained unchanged in step (4), but the temperature of the reaction chamber needs to be increased to 1050-1150° C., and the rate of introducing Ga source and N source is increased. For example, from 100 mL / min to 120 mL / min, and from 1000 mL / min to 1200 mL / min, respectively. The epitaxial time is generally 20-25 minutes, and a GaN film with a certain thickness is prepared.
[0065] When molecular beam epitaxy is used in step (3), the pressure conditions of the molecular beam epitaxy in step (3) are kept unchanged in step (4), but the temperature of the reaction chamber needs to be increased to 900-1100° C. (preferably 900° C.) and the epitaxy time is 20-30 min (preferably 30 min) to prepare a GaN film with a certain thickness.
[0066] The GaN film of a certain thickness obtained above is annealed in a tube furnace, and the annealing temperature is set to 800-1000°C (preferably 1000°C) to induce its structural reconstruction and stability, that is, the preparation of the non-polar two-dimensional GaN film is completed. Among them, in order to ensure the integrity of the 4|8GaN film structure and maintain the excellent properties of the two-dimensional material, the thickness of the non-polar two-dimensional GaN film is generally controlled within 2nm.
[0067] The above describes the specific technical solutions of the present invention. It should be understood that the present invention is not limited to the above specific implementations, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essential content of the present invention.
Claims
1. A method for preparing non-polar two-dimensional GaN in-situ epitaxially, characterized in that: The steps include: Step 1, preparing a SiC substrate having a C-terminal surface; Step 2, performing competitive polar nucleation of Ga-polar GaN3 and N-polar Ga3N on the C-terminal surface; Step 3, stably linking the nucleation structure to obtain a single-layer GaN film; Step 4, continuing to prepare a GaN film on the single-layer GaN film, and then annealing to induce structural reconstruction and stabilize it to obtain a non-polar two-dimensional GaN film.
2. The method for preparing non-polar two-dimensional GaN by in-situ epitaxy according to claim 1, characterized in that: In the step 1, the SiC substrate is placed in a hydrogen environment for annealing, then cleaned, and then placed in a hydrogen-argon mixed gas for hydrogen etching, and the SiC substrate is polished by a chemical mechanical polishing method to prepare a SiC substrate with a C-terminal surface.
3. The method for preparing non-polar two-dimensional GaN by in-situ epitaxy according to claim 1, characterized in that: In the step 2, the competitive polar nucleation is carried out by metal organic chemical vapor deposition, hydrogen plasma vapor exfoliation and molecular beam epitaxy.
4. The method for preparing non-polar two-dimensional GaN in-situ epitaxially according to claim 3, characterized in that: The metal organic chemical vapor deposition is used to achieve competitive polar nucleation, and the method is as follows: The SiC substrate with C-terminal surface was placed in the reaction chamber, H2 was introduced as the carrier gas, and the reaction chamber was evacuated to a pressure of 10 -7 ~10 -8 Torr, the reaction chamber is heated to 800-1000°C by radio frequency induction, Ga source and N source are introduced, and the pressure of the reaction chamber is maintained at 500 Torr. The epitaxial time is 5-10 minutes. Combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface; The hydrogen plasma gas phase exfoliation is used to achieve competitive polar nucleation, and the method is as follows: The SiC substrate with C-terminal surface was placed in the reaction chamber, H2 and N2 were introduced as carrier gas, HCl gas was used as reaction gas, and the reaction chamber was first evacuated to a pressure of 10 -7 ~10 -8 Torr, heating the reaction chamber to 1000-1050°C, introducing Ga source and N source, the epitaxial time is 10-15 minutes, and combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface; The competitive polar nucleation is achieved by using the molecular beam epitaxy as follows: The SiC substrate with C-terminal surface was placed in the reaction chamber and evacuated to 10 -7 ~10 -8 Torr, Ga source and N source are introduced, the temperature is set to 700-800°C, the epitaxial time is 5-10 min, and combined with real-time monitoring technology, Ga-polar GaN3 and N-polar Ga3N are simultaneously nucleated on the C-terminal surface.
5. The method for preparing non-polar two-dimensional GaN in-situ epitaxially according to claim 4, characterized in that: The real-time monitoring technology is a high-energy electron diffraction technology, which monitors the formation of Ga-polar tripod GaN3 and N-polar tripod Ga3N on the C-terminal surface to simultaneously form nucleation islands.
6. The method for preparing non-polar two-dimensional GaN by in-situ epitaxy according to claim 3, 4 or 5, characterized in that: In the step 3, based on the step 2, metal organic chemical vapor deposition, hydrogen plasma vapor stripping or molecular beam epitaxy deposition is continued, the temperature and pressure of metal organic chemical vapor deposition and hydrogen plasma vapor stripping remain unchanged, the temperature of the reaction chamber of molecular beam epitaxy is increased to 800-900°C, and the pressure remains unchanged, so that the Ga polar GaN3 and N polar Ga3N nucleation clusters and nucleation islands on the C terminal surface are stably linked to prepare a single-layer GaN film.
7. The method for preparing non-polar two-dimensional GaN in-situ epitaxially according to claim 6, characterized in that: In the step 4, on the basis of step 3, metal organic chemical vapor deposition, hydrogen plasma gas phase stripping or molecular beam epitaxial deposition is continued, the temperature of the reaction chamber of the metal organic chemical vapor deposition is increased to 1000-1100° C., and the rate of introducing Ga source and N source is increased, and the pressure remains unchanged; the temperature of the reaction chamber of the hydrogen plasma gas phase stripping is increased to 1050-1150° C., and the rate of introducing Ga source and N source is increased, and the pressure remains unchanged; the temperature of the reaction chamber of the molecular beam epitaxy is increased to 900-1100° C., and the pressure remains unchanged; a GaN film with a certain thickness is prepared, and then annealed at 800-1000° C. to induce its structural reconstruction and stabilize it, thereby completing the preparation of a non-polar two-dimensional GaN film.
8. The method for preparing non-polar two-dimensional GaN in-situ epitaxially according to claim 7, characterized in that: In the step 2, in the metal organic chemical vapor deposition, the rates of the introduction of the Ga source and the N source are 20 umol / min and 0.05 umol / min, respectively; in the hydrogen plasma gas phase stripping, the rates of the introduction of the Ga source and the N source are 100 mL / min and 1000 mL / min, respectively; In step 3, the epitaxial time of continuing metal organic chemical vapor deposition is 10 to 15 minutes, and the epitaxial time of continuing hydrogen plasma vapor phase stripping is 15 to 20 minutes; In the step 4, the metal organic chemical vapor deposition is continued, the rates of introducing the Ga source and the N source are 25umol / min and 0.1umol / min respectively, and the epitaxial time is 20 to 25min; the hydrogen plasma gas phase stripping is continued, the rates of introducing the Ga source and the N source are 120mL / min and 1200mL / min respectively, and the epitaxial time is 20 to 25min; the molecular beam epitaxy is continued, and the epitaxial time is 20 to 30min.
9. The method for preparing non-polar two-dimensional GaN in-situ epitaxially according to claim 1, characterized in that: The thickness of the non-polar two-dimensional GaN film is controlled within 2 nm.
10. The non-polar two-dimensional GaN film obtained by the in-situ epitaxial preparation method of non-polar two-dimensional GaN according to any one of claims 1 to 9 is used for future advanced nanoscale electronics, optoelectronic devices or high-mobility carrier LEDs.