Method for growing P-type 4H-SiC single crystal by PVT method

By performing electrochemical etching pretreatment on the Si surface of SiC substrate, nucleation sites and windows are provided, the problem of P-type 4H-SiC single crystal cannot grow stably on the Si surface and the difficulty of doping aluminum sources is achieved, and aluminum is achieved The high absorption of elements and single crystal growth improve the quality and application of P-type 4H-SiC single crystal.

CN119028811AActive Publication Date: 2024-11-26TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411150486.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

P-type 4H-SiC single crystal cannot grow stably on the Si surface, and the aluminum source is difficult to dopant, resulting in limited growth quality and application.

Method used

Electrochemical etching pretreatment is performed on the Si surface of the SiC substrate to provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for 4H-SiC nucleation growth, increase doping of aluminum elements, and stabilize Growth of P-type 4H-SiC single crystal.

Benefits of technology

The stable growth of P-type 4H-SiC single crystal form on the Si surface is achieved, while increasing the absorption of aluminum elements, improving the growth quality of single crystals, avoiding the generation of grain boundaries and multi-types, and solving the problem of difficult doping of aluminum sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028811A_ABST
    Figure CN119028811A_ABST
Patent Text Reader

Abstract

The invention discloses a method for growing a P-type 4H-SiC single crystal through a PVT method, and belongs to the technical field of semiconductors. Before SiC single crystal growth, electrochemical etching pretreatment is carried out on the Si surface of the SiC substrate, specifically, the Si surface of the SiC substrate is exposed, and the C surface of the SiC substrate is covered; the covered surface of the substrate is connected with a graphite electrode as an anode, and a graphite electrode or a platinum electrode is selected as a cathode; placing the anode and the cathode symmetrically, placing the SiC substrate in the electrolyte, and connecting a power supply to carry out electrochemical etching on the growth surface of the substrate; and continuously soaking the substrate subjected to electrochemical etching in the electrolyte, then soaking the substrate in deionized water for ultrasonic treatment, and finally blow-drying the substrate with inert gas. According to the method for growing the P-type 4H-SiC single crystal by the PVT method, the Si surface of the SiC substrate is subjected to electrochemical etching pretreatment before the growth of the SiC single crystal by the PVT method, so that more nucleation sites can be provided, the nucleation energy of 4H on the Si surface is reduced, a window is provided for the nucleation growth of 4H-SiC, the doping of an aluminum element is increased, and the growth of the P-type 4H-SiC single crystal is stabilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, and in particular to a method for growing a P-type 4H-SiC single crystal using a PVT method. Background Art

[0002] SiC material not only has high high temperature strength and creep resistance, excellent corrosion resistance, good thermal conductivity, but also has unique characteristics such as large bandgap, high breakdown field strength, high electron saturation drift velocity, small dielectric constant, strong radiation resistance, etc. It is more suitable for manufacturing high temperature, high power, high frequency devices, and substrates of other thin film materials (such as AlN, GaN, diamond) and X-ray masks, etc. SiC is widely used in white light illumination, optical storage, screen display, aerospace, high temperature radiation environment, oil exploration, automation, radar and communication, automotive electronics, etc. It is an ideal semiconductor material for manufacturing optoelectronic devices, high frequency and high power devices, and high temperature electronic devices.

[0003] At present, the main quality issues of SiC crystal growth are the generation of defects and the control of doping, which will directly affect the yield of the wafer. As for defects, micropipes can be reduced to a very low level, but there are still defects such as through-edge dislocation (TED), through-screw dislocation (TSD), and base plane dislocation (BPD) that need to be further controlled and reduced. As for doping, the control of doping concentration and elements requires more rigorous requirements.

[0004] The application of SiC in power electronic devices requires SiC to have higher P-type and N-type doping concentrations, which can only be achieved through doping. At present, physical vapor transport (PVT) is the mainstream growth method for SiC single crystals. If P-type or N-type SiC is to be grown, the growth materials and growth process need to be adjusted. At present, the growth process of N-type 4H-SiC single crystals is relatively complete. The C-face is generally used as the growth face for growing N-type 4H-SiC single crystals. The surface energy of the C-face is low, which can provide a suitable growth window for the nucleation growth of 4H-SiC. Nitrogen is also easier to be incorporated into the C-face and the nitrogen source can be continuously supplied, which makes it possible to control the nitrogen doping concentration and uniformity well, and the doping concentration can reach 1.0E18cm -3 (or even higher), therefore, the supply and application of N-type 4H-SiC in the market account for a relatively large proportion. However, when P-type 4H-SiC single crystal is doped and grown on the C surface, although the single crystal form of 4H-SiC can be guaranteed, the doping of aluminum on the C surface is much lower than that of nitrogen, and it is difficult to continuously supply aluminum sources. Therefore, the growth of P-type 4H-SiC single crystal still has the problems of difficult doping and uneven doping, which seriously affects the growth quality and application of P-type 4H-SiC single crystal.

[0005] Relevant studies have shown that when growing P-type SiC single crystals, the aluminum content of 6H-SiC single crystals grown on the Si surface is much higher than that of 4H-SiC single crystals grown on the C surface. It is easier to incorporate aluminum on the Si surface of the SiC seed crystal. However, in the traditional PVT process, 4H-SiC single crystals cannot be grown on the Si surface, and generally only 6H-SiC single crystals can be grown on the Si surface of the seed crystal. However, the bandgap width of 6H-SiC single crystals is smaller than that of 4H-SiC, and the performance is worse than that of 4H. In response to this problem, the present invention proposes a method for growing P-type 4H-SiC single crystals on the Si surface of a SiC seed crystal by a PVT method. Summary of the invention

[0006] The purpose of the present invention is to provide a method for growing P-type 4H-SiC single crystal by PVT method, which solves the problem that 4H-SiC single crystal cannot be stably grown on Si surface and aluminum source is difficult to be doped, and can increase the absorption of aluminum while ensuring the growth of P-type 4H-SiC single crystal on Si surface, so as to achieve the purpose of reducing cost and increasing efficiency.

[0007] To achieve the above-mentioned purpose, the present invention provides a method for growing a P-type 4H-SiC single crystal by a PVT method. Before the SiC crystal is grown by the PVT method, the Si surface of the SiC substrate is pretreated by electrochemical etching, which can provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for the nucleation growth of 4H-SiC, increase the doping of aluminum elements, and stabilize the growth of the P-type 4H-SiC single crystal.

[0008] Preferably, the specific steps of performing electrochemical etching pretreatment on the Si surface of the SiC substrate are:

[0009] (1) Exposing the Si surface of the SiC substrate to be pretreated and covering the C surface;

[0010] (2) The C-side of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode;

[0011] (3) The anode and cathode are placed symmetrically, the SiC substrate is placed in the electrolyte, the power supply is connected and the Si surface of the substrate is electrochemically etched;

[0012] (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.

[0013] Preferably, in step (2), the C surface of the substrate and the graphite electrode are connected by conductive adhesive bonding or vacuum adsorption.

[0014] Preferably, in step (3), the distance between the cathode and the anode is 1-20 cm, the power supply voltage is 0-50 V, and the current is 0-500 mA.

[0015] Preferably, in step (3), the electrolyte is an HF solution with a concentration of 0-60wt%, a temperature of 0-50°C, and an electrochemical etching time of 0-5h.

[0016] Preferably, in step (4), the electrolyte is immersed for 0-12 hours, and the ultrasonic immersion is performed in deionized water for 0-10 hours.

[0017] Preferably, in step (4), the inert gas is Ar or He.

[0018] The electrochemical etching process basically includes two parts: In the first part, holes are generated during the etching process, current is formed at the SiC-electrolyte interface, and SiC is oxidized to SiO x Thin Films, Part II, SiO x The film is dissolved in the electrolyte. The type / concentration of the electrolyte, electrochemical etching time / temperature, additional auxiliary conditions (such as ultraviolet light irradiation, ultrasonic vibration, etc.), load voltage / current, and electrode spacing will all affect the electrochemical etching effect.

[0019] The main method of the present invention is to perform electrochemical etching pretreatment on the Si surface of the SiC substrate before growing SiC crystal by PVT method, and after the electrochemical etching pretreatment, use SiC powder doped with aluminum source as raw material to grow P-type 4H-SiC single crystal by PVT method on the Si surface. The basic principle of electrochemical etching pretreatment is: electrochemical etching can provide more nucleation sites on the substrate, reduce the nucleation energy of 4H on the Si surface, provide a suitable window for 4H-SiC nucleation growth, break the current situation that only 6H-SiC can be grown on the Si surface and 4H-SiC can only grow on the C surface, make full use of the characteristic that aluminum element is easier to be doped when growing on the Si surface, increase the absorption of aluminum element, improve the growth quality of single crystal, avoid the generation of grain boundary and polymorphism, thereby stabilizing the single crystal type of 4H-SiC on the Si surface, and making the doping and growth of P-type 4H-SiC single crystal easier.

[0020] Therefore, the present invention provides a method for growing P-type 4H-SiC single crystal by PVT method, selects a suitable substrate pretreatment scheme, utilizes electrochemical etching to reduce the surface nucleation energy of Si surface, and increases the absorption of aluminum element while ensuring the growth of P-type 4H-SiC single crystal on Si surface, so as to achieve the purpose of reducing cost and increasing efficiency.

[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A diagram of the device used for electrochemical etching of the present invention;

[0023] Figure 2The thermal field structure diagram for growing P-type 4H-SiC single crystal by the PVT method of the present invention;

[0024] Figure 3 This is the Raman mapping image of SiC single crystal grown by PVT method without processing the Si surface of SiC substrate;

[0025] Figure 4 This is the Raman mapping image of SiC single crystal grown by PVT method after the Si surface of SiC substrate was pretreated by electrochemical etching;

[0026] Reference Numbers

[0027] 1-anode electrode; 2-cathode electrode; 3-tetrafluoroethylene cover plate; 4-power supply; 5-electrolyte; 6-SiC substrate; 7-graphite threaded rod; 8-conducting wire; 9-upper temperature measuring hole; 10-lower temperature measuring hole; 11-upper insulation; 12-lower insulation; 13-side insulation; 14-seed crystal holder; 15-seed crystal; 16-crystal growth crucible; 17-P-type SiC powder. DETAILED DESCRIPTION

[0028] The present invention provides a method for growing a P-type 4H-SiC single crystal by a PVT method. Before the SiC crystal is grown by the PVT method, the Si surface of the SiC substrate is pretreated by electrochemical etching, which can provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for the nucleation growth of 4H-SiC, increase the doping of aluminum elements, and stabilize the growth of the P-type 4H-SiC single crystal.

[0029] In the present invention, the specific steps of electrochemical etching pretreatment of the Si surface of the SiC substrate are:

[0030] (1) Exposing the Si surface of the SiC substrate to be pretreated and covering the C surface;

[0031] (2) The C-side of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode;

[0032] (3) The anode and cathode are placed symmetrically, the SiC substrate is placed in the electrolyte, the power supply is connected and the Si surface of the substrate is electrochemically etched;

[0033] (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.

[0034] In the present invention, the device used for electrochemical etching is as follows Figure 1As shown, it includes an anode electrode 1, a cathode electrode 2, a tetrafluoroethylene cover plate 3, a power source 4, an electrolyte 5, a SiC substrate 6, a graphite threaded rod 7, and a wire 8, wherein the anode and the cathode are placed symmetrically up and down, the graphite threaded rod 7 and the tetrafluoroethylene cover plate 3 are fixed and adjusted by threads between the two electrodes, the distance between the cathode and the anode is 1-20 cm, the masking surface of the SiC substrate 6 is bonded to the anode electrode 1 by conductive glue or vacuum adsorption, the pre-etched surface is in contact with the electrolyte 5, the graphite threaded rod 7 and the tetrafluoroethylene cover plate 3 are fixed and adjusted by threads between the anode electrode 1 (graphite electrode) and the cathode electrode 2 (graphite electrode), the graphite threaded rod 7 is tightened with the graphite electrodes 1 and 2 for conduction, and the wire 8 is connected to the graphite threaded rod 7 by a conductive clamp for conduction.

[0035] The power supply is powered on, the power supply voltage is 0-50V, the current is 0-500mA, and the hydroxide (OH) is generated by electrolysis of water. - ) gather at the anode, and hydroxide (OH - ) and holes (h + ) forms free radicals ( . OH), the free radical is unstable and easily diffuses to the interface between the anode SiC and the electrolyte, oxidizing SiC to SiO x and CO x , and then the oxidation product SiO x and CO x Dissolved in HF electrolyte. The process can be expressed as:

[0036] 4OH - -4e - →2H2O+O2;

[0037] OH - +h + → . OH;

[0038] SiC+4 . OH+O2→SiO2+CO2+2H2O;

[0039] SiO2+6HF→2H + +SiF6 2- +2H2O.

[0040] In the present invention, the specific steps of electrochemical etching + P-type 4H-SiC single crystal growth are as follows:

[0041] Step 1: expose the Si surface of the SiC substrate to be pretreated and cover the C surface;

[0042] Step 2: The C surface of the substrate is connected to a graphite electrode as an anode, and a graphite electrode or a platinum electrode is selected as a cathode (the C surface of the substrate is preferably conductive glue or vacuum adsorbed on the graphite electrode);

[0043] Step 3: The anode and cathode are placed symmetrically in an electrolyte with a concentration of 0-60wt%, and a power source is connected to perform electrochemical etching on the growth surface of the substrate for 0-5h;

[0044] The electrolyte temperature is controlled at 0-50°C, and auxiliary conditions can be added, such as ultraviolet light irradiation, ultrasonic vibration, etc. The electrolyte type can be neutral (such as NaCl solution), alkaline (such as KOH solution), acidic (such as HF solution). In the present invention, HF solution is preferably selected as the electrolyte.

[0045] Step 4: Soak the electrochemically etched substrate in an electrolyte for 0-12 hours, then soak it in deionized water for several times with ultrasonic vibrations for 0-10 hours, and finally dry it with an inert gas such as Ar or He for later use.

[0046] Step 5: Use the Si surface of the pretreated seed crystal 15 as the growth surface and fix it on the seed crystal holder 14 (the fixing method is not limited, it can be: adhesive bonding, mechanical fixing, chemical fixing, etc.), place the P-type SiC powder 17 at the bottom of the crystal growth crucible 16, tighten the crucible, and place it in a corresponding heat preservation field (the material of the crystal growth crucible can be selected from isostatic graphite, tantalum carbide, tantalum carbide coating or metal tungsten, etc.).

[0047] Step 6: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10^ -6 mbar, set the corresponding temperature and pressure control programs.

[0048] Step seven: under vacuum conditions, set the temperature rising program, after heating to 1100-1450°C for 2-6 hours, open the argon gas inlet (gas flow rate is controlled at 0-5L / min), increase the pressure to 200-900mbar for 0.5-3 hours, under the condition of flowing argon constant pressure, increase the temperature to 2000-2300°C for 2-6 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 0.1-50mbar within 0.5-50 hours. Under the growth conditions of temperature: 2000-2300°C, pressure: 0.1-50mbar, the crystal grows for 3-15 days.

[0049] Step 8: Before increasing the pressure and lowering the temperature, keep the argon gas inlet open (gas flow rate controlled at 0-5L / min), increase the pressure to 200-900mbar for 0.5-3 hours, and lower the temperature to 700-1400℃ for 10-20 hours, then cool naturally, and the entire crystal growth is completed.

[0050] In the present invention, the thermal field device used for crystal growth is as follows Figure 2 As shown, it includes an upper temperature measuring hole 9, a lower temperature measuring hole 10, an upper insulation 11, a lower insulation 12, a side insulation 13, a seed crystal holder 14, a pre-treated seed crystal 15, a crystal growth crucible 16, and a P-type SiC powder 17. From top to bottom, they are the upper insulation 11, the side insulation 13 and the lower insulation 12, wherein the upper and lower temperature measuring holes 9 and 10 are respectively located in the middle of the upper and lower insulations, the crystal growth crucible 16 is placed in the middle of the lower insulation 12, the P-type SiC powder 17 is placed at the bottom of the crystal growth crucible 16, the pre-treated seed crystal 15 is fixed on the seed crystal holder 14, and the seed crystal holder 14 is connected to the crystal growth crucible by a threaded knob.

[0051] The present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.

[0052] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0053] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.

[0054] Example

[0055] This embodiment provides a method for growing a P-type 4H-SiC single crystal on the Si surface of a SiC substrate by a PVT method after pre-treating the Si surface of the SiC substrate by electrochemical etching. The specific steps are as follows:

[0056] Step 1: The Si surface of the SiC substrate 6 is exposed, and the C surface is connected to the graphite electrode 1 using a conductive adhesive so that the SiC substrate 6 and the graphite electrode 1 are in full contact.

[0057] Step 2: SiC substrate 6 and graphite electrode 1 are used as anodes and connected to the positive pole of the power supply. Graphite electrode 2 of the same size and thickness is used as cathode and connected to the negative pole of the power supply. The distance between the two electrodes is 6 cm. The output voltage of power supply 4 is 15 V and the current is 50 mA.

[0058] Step 3: electrochemically etch the SiC substrate with exposed Si surface in HF electrolyte 5 with a concentration of 10 wt% for 10 minutes, and the temperature of the electrolyte 5 is controlled at 30°C.

[0059] Step 4: The electrochemically etched substrate is first immersed in electrolyte 5 for 12 hours, then immersed in deionized water for 2 hours by ultrasonic wave, and finally dried with Ar gas for later use.

[0060] Step 5: Use the Si surface of the pretreated seed crystal 15 as the growth surface and fix it on the seed crystal holder 14 (the fixing method is not limited, it can be: adhesive bonding, mechanical fixing, chemical fixing, etc.), place the P-type SiC powder 17 at the bottom of the crystal growth crucible 16, tighten the crucible, and place it in the corresponding insulation heat field.

[0061] Step 6: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.

[0062] Step 7: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the argon inlet line (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, and under the condition of flowing argon constant pressure, increase the temperature to 2100°C in 3 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour. Under the growth conditions of temperature: 2100°C and pressure: 5mbr, the crystal is grown for 5 days.

[0063] Step 8: Before increasing the pressure and lowering the temperature, keep the Ar gas inlet open (gas flow rate is 1L / min), increase the pressure to 800mbar for 1 hour, and lower the temperature to 1100℃ in 15 hours, then cool naturally, and the entire crystal growth is completed.

[0064] SIMS test was performed on two N-type 4H-SiC substrates with different crystal planes, which were used as seed crystals for growth after electrochemical etching pretreatment. The results are shown in Table 1.

[0065] Table 1

[0066] Growing conditions <![CDATA[Aluminum concentration (cm -3 )]]> Growth of P-type 4H-SiC on Si Surface of N-type 4H Seed Crystal 4.0E15—6.0E15 Growth of P-type 4H-SiC on C-surface of N-type 4H seed crystal 1.0E15—2.0E15

[0067] From the data in Table 1, it can be seen that the absorption of aluminum by the P-type 4H-SiC single crystal grown on the Si surface is much higher than that by the P-type 4H-SiC single crystal grown on the C surface (2-6 times), indicating that if the growth of the 4H-SiC single crystal is stabilized on the Si surface, the absorption of aluminum can be increased, which is beneficial to the doping growth of the P-type 4H-SiC single crystal.

[0068] Raman mapping scanning test was performed on the SiC single crystal grown by PVT method directly without treating the Si surface of the SiC substrate and the SiC single crystal grown by PVT method after the Si surface of the SiC substrate was pretreated by electrochemical etching.

[0069] Raman mapping scan test can determine the distribution of SiC crystal types. The same color means the same characteristic peaks, which means the same crystal type. The blue characteristic peaks are 204 and 776, which represent 4H-SiC; the green characteristic peaks are 150 and 789, which represent 6H-SiC; and the red characteristic peaks are 173 and 785, which represent 15R-SiC. Figure 3 In the case of SiC substrate, the Si surface is not treated and the single crystal is grown directly. The Raman mapping image is not uniform in color, indicating the presence of 6H, 4H, and 15R crystal types, and the presence of polymorphic inclusions. Figure 4 This is the Raman mapping image of SiC single crystal grown by PVT method after electrochemical etching pretreatment on Si surface of SiC substrate. After electrochemical etching pretreatment, the Raman mapping image has a single color, all blue, indicating that the grown crystals are all 4H-SiC single crystals, which indicates that electrochemical etching pretreatment can promote and stabilize the growth of 4H-SiC single crystal on Si surface.

[0070] In summary, before growing SiC crystals by the PVT method, electrochemical etching pretreatment is performed on the Si surface of the SiC substrate, which can provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, and provide a window for the nucleation and growth of 4H-SiC. While stabilizing the growth of 4H-SiC single crystal on the Si surface, it can increase the doping of aluminum elements, which is beneficial to solving the problem of difficult aluminum doping in the growth of P-type SiC single crystals, breaking the technical barriers of growing 4H on the C surface and 6H on the Si surface, and providing new ideas for the growth of P-type SiC crystals.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for growing a P-type 4H-SiC single crystal by a PVT method, characterized in that: Before the PVT growth of SiC single crystal, the Si surface of the SiC substrate is pretreated by electrochemical etching, which can provide more nucleation sites, reduce the nucleation energy of 4H on the Si surface, provide a window for the nucleation growth of 4H-SiC, increase the doping of aluminum elements, and stabilize the growth of P-type 4H-SiC single crystal.

2. The method for growing a P-type 4H-SiC single crystal by a PVT method according to claim 1, characterized in that: The specific steps of electrochemical etching pretreatment of the Si surface of the SiC substrate are: (1) Exposing the Si surface of the SiC substrate to be pretreated and covering the C surface; (2) The C-side of the substrate is connected to a graphite electrode as the anode, and a graphite electrode or a platinum electrode is selected as the cathode; (3) The anode and cathode are placed symmetrically, the SiC substrate is placed in the electrolyte, the power supply is connected and the Si surface of the substrate is electrochemically etched; (4) The electrochemically etched substrate is further immersed in the electrolyte, then immersed in deionized water for ultrasonic treatment, and finally dried with an inert gas.

3. The method for growing a P-type 4H-SiC single crystal by a PVT method according to claim 2, characterized in that: In the step (2), the C surface of the substrate and the graphite electrode are connected by conductive adhesive bonding or vacuum adsorption.

4. The method for growing a P-type 4H-SiC single crystal by a PVT method according to claim 2, characterized in that: In the step (3), the distance between the cathode and the anode is 1-20 cm, the power supply voltage is 0-50 V, and the current is 0-500 mA.

5. The method for growing P-type 4H-SiC single crystal by PVT method according to claim 2, characterized in that: In the step (3), the electrolyte is an HF solution with a concentration of 0-60wt%, a temperature of 0-50°C, and an electrochemical etching time of 0-5h.

6. The method for growing a P-type 4H-SiC single crystal by a PVT method according to claim 2, characterized in that: In the step (4), the sample is immersed in the electrolyte for 0-12 hours, and immersed in deionized water for 0-10 hours.

7. The method for growing a P-type 4H-SiC single crystal by a PVT method according to claim 2, characterized in that: In the step (4), the inert gas is Ar or He.

Citation Information

Patent Citations

  • Low-resistivity P-type 4H-SiC single crystal and preparation method thereof

    CN112725894A

  • Method for growing low-resistance p-type 4H-SiC by PVT method and low-resistance p-type 4H-SiC

    CN115404549A

  • Homoepitaxial growth of SiC on low off-axis SiC wafers

    US20060011128A1

  • Compound semiconductor device and method for manufacturing the same

    US20160218201A1

  • Enabling low-cost iii-v / si integration through nucleation of gap on v-grooved si substrates

    US20190378952A1