Method for detecting metal impurities in silicon wafer

By reacting silicon wafers with metal impurities in the semiconductor manufacturing process to generate silicon rings, and through layered corrosion detection, the problem of metal impurities detection in semiconductor manufacturing is solved, early screening and efficient removal are achieved, and production line efficiency and analysis accuracy are improved. sex.

CN119028856APending Publication Date: 2024-11-26SHANGHAI ADVANCED SILICON TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135729.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently detect metal impurities in silicon wafers during semiconductor manufacturing, especially at the front end of the original wafer production, resulting in waste of resources and inaccuracy of subsequent analysis.

Method used

By heat treatment of the silicon wafer at 600-1200℃, metal impurities react with silicon to form metal silicide (silicon ring), and the presence of the silicon ring is observed through layered corrosion treatment to determine whether the silicon wafer contains metal impurities, thereby Realize early screening and elimination of wafers with high impurity content.

Benefits of technology

It realizes early screening of original wafers and pre-elimination of high metal impurity content wafers, improves detection rate and accuracy, concentrates analysis resources on high-quality wafers, optimizes production line efficiency and subsequent ICP analysis accuracy and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028856A_ABST
    Figure CN119028856A_ABST
Patent Text Reader

Abstract

The invention relates to a method for detecting metal impurities in a silicon wafer, which comprises the following steps of: carrying out heat treatment on the silicon wafer to be detected at 600-1200 DEG C to enable the metal impurities to react with silicon to generate metal silicide; cooling the silicon wafer after heat treatment, so that the solubility of the metal silicide is reduced, and the metal silicide is separated out in a silicon ring form; and carrying out layered corrosion treatment on the cooled silicon wafer, observing whether a bright ring-shaped silicon ring exists on the corrosion surface under different corrosion depths, and if so, proving that the silicon wafer contains metal impurities. According to the method provided by the invention, whether the silicon ring contains the metal impurities or not is judged by detecting the silicon ring, so that early screening of the original wafer and pre-removal of the wafer with high metal impurity content are realized, and the method has relatively good detection precision.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor detection, and in particular to a method for detecting metal impurities in a silicon wafer. Background Art

[0002] In the process of semiconductor manufacturing, impurities can affect the conductivity of semiconductors, resulting in performance degradation or failure, so the control of impurities is crucial. Among these impurities, metal impurities are one of the most important sources. Metal impurities can diffuse rapidly in the chip through diffusion or electromigration, so in the production process of silicon wafers, how to detect and control metal impurities is very important.

[0003] In the semiconductor field, there are various methods for testing metal impurities. The most common method is to use ICP-MS analysis technology to detect metal impurities on the surface of silicon wafers and obtain quantitative data. However, since ICP-MS can only measure liquids, it is necessary to sample the surface of the silicon wafer before using ICP-MS testing. The sampling process is likely to affect the sample itself, and ICP-MS analysis technology has high requirements for sample cleanliness. Testing uncleaned samples may cause equipment contamination, affecting the accuracy of subsequent tests.

[0004] In actual silicon wafer production, if the original wafers can be screened early at the front end of production, the wafers with higher impurity content can be identified and unqualified wafers can be eliminated, it is possible to avoid investing too much analysis cost in these wafers and concentrate analysis resources and energy on higher-quality wafers. This can not only improve the efficiency and output of the production line, optimize the allocation of production resources, and reduce the complexity of the process, but also help maintain and ensure the accuracy and stability of subsequent analysis results.

[0005] Therefore, how to detect metal impurities in the original wafers at the front end of silicon wafer production and ensure a certain detection accuracy is a technical problem that needs to be solved in this field. Summary of the invention

[0006] In view of the above problems, the purpose of the present invention is to provide a method for detecting metal impurities in silicon wafers. Compared with the prior art, the method provided by the present invention utilizes the reaction of silicon wafers with metal impurities contained in themselves to generate metal silicide (silicon ring), and determines whether the silicon ring contains metal impurities by detecting the silicon ring, thereby realizing early screening of original wafers and pre-elimination of wafers with high metal impurity content, effectively improving the detection rate of original wafers and having good detection accuracy.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for detecting metal impurities in a silicon wafer, the method comprising the following steps:

[0009] The silicon wafer to be tested is heat treated at 600-1200°C to make the metal impurities react with silicon to form metal silicide;

[0010] The heat-treated silicon wafer is cooled to reduce the solubility of the metal silicide and precipitate in the form of silicon rings;

[0011] The cooled silicon wafer is subjected to layered etching treatment to observe whether there is a bright ring-shaped silicon ring on the corrosion surface at different etching depths. If there is, it proves that the silicon wafer contains metal impurities.

[0012] In the present invention, firstly, in the heat treatment, the silicon wafer is used to react with the metal impurities contained in the silicon wafer to generate metal silicide (silicon ring), such as lithium, calcium, magnesium, iron, chromium and other metal impurities. The formed metal silicide has different physical properties from silicon, such as refractive index, metallic luster, etc., and the metal silicide nucleates and grows during the heat treatment; then, the solubility of the metal silicide is reduced by cooling and precipitated in the form of silicon rings, so as to facilitate subsequent better detection; then, the silicon wafer is subjected to layered corrosion treatment, and the corrosion surface of the silicon wafer in different ranges is observed, generally using a microscope for observation. If there is a silicon ring, it means that the content of metal impurities is too high and cannot be used for subsequent silicon wafer production, and the silicon wafer is removed. The method provided by the present invention can realize the early screening of original wafers and the pre-removal of wafers with high metal impurity content, and has good detection accuracy.

[0013] The temperature of the heat treatment is 600-1200°C, for example, it can be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] Preferably, the heat treatment time is 1-120 min, for example, it can be 1 min, 2 min, 4 min, 6 min, 8 min, 10 min, 20 min, 40 min, 60 min, 80 min, 100 min or 120 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] In the present invention, by controlling the range of heat treatment temperature, and preferably controlling the time of heat treatment, it is possible to further promote the reaction of the silicon wafer with the metal impurities contained in it to form metal silicide, thereby utilizing the difference in physical properties between metal silicide and silicon to determine whether the content of metal impurities is too high by detecting whether metal silicide is detected.

[0016] Preferably, the cooling time is 5-120 min, for example, it can be 5 min, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] In the present invention, the cooling is to cool the silicon wafer to room temperature, generally 10-40°C. The present invention preferably controls the cooling time within a specific range, the purpose of which is to combine the cooling atmosphere introduced for rapid cooling. The solubility of the metal silicide is reduced by cooling, thereby causing it to precipitate in the form of a silicon ring, which is convenient for subsequent detection.

[0018] Preferably, argon gas is filled during the heat treatment.

[0019] In the present invention, argon gas is introduced in advance before the heat treatment to discharge the impurity gas in the reaction chamber.

[0020] Preferably, the flow rate of argon gas in the heat treatment is less than 5SLM, for example, it can be 4.8SLM, 4.5SLM, 4.2SLM, 4SLM, 3.8SLM, 3.5SLM, 3.2SLM, 3SLM, 2.8SLM, 2.5SLM, 2.2SLM, 2SLM, 1.8SLM, 1.5SLM, 1.2SLM, 1SLM or 0SLM, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] In the present invention, the reaction between metal and silicon can be promoted by introducing argon gas during the heat treatment and preferably controlling the flow rate of the argon gas within a specific range.

[0022] In the present invention, oxygen can generally be introduced during the heat treatment process, and the oxygen flow rate is controlled to be ≤10SLM, in order to form a silicon oxide layer during the heat treatment, which is beneficial for achieving good flatness of the wafer in the subsequent thinning process.

[0023] Preferably, argon gas is filled during the cooling process.

[0024] Preferably, the flow rate of argon gas in the cooling process is 5-10 SLM, for example, it can be 5 SLM, 5.5 SLM, 6 SLM, 6.5 SLM, 7 SLM, 7.5 SLM, 8 SLM, 8.5 SLM, 9 SLM, 9.5 SLM or 10 SLM, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] In the present invention, by introducing argon gas during the cooling process and preferably controlling the flow rate of argon gas within a specific range, the cooling of the reaction chamber can be accelerated, and the cooling of the silicon wafer can be accelerated. In the present invention, if the terminal temperature of the cooling is relatively low, such as below 400°C, hydrogen gas can be introduced, and if the cooling is below 750°C, nitrogen gas can be introduced, preferably argon gas.

[0026] Preferably, the layered etching process includes a first etching and a second etching performed sequentially.

[0027] In the present invention, the formation process of metal silicide is: first, the initial metal silicide nucleus is generated by reaction at the metal-silicon interface, and then the metal or silicon atoms diffuse to make the metal silicide grow until the metal atoms are exhausted. This process belongs to a reaction diffusion process, so the silicon ring cannot be effectively detected by observing the surface of the silicon wafer alone. It is necessary to perform a first corrosion to remove part of the oxide layer, at which time most of the silicon ring can be observed; then a second corrosion is required to remove part of the silicon layer to further detect whether there is a silicon ring to ensure a certain detection accuracy.

[0028] Preferably, the first etching includes etching the cooled silicon wafer and eating away the oxide layer.

[0029] Preferably, the etching solution used in the first etching comprises a hydrofluoric acid solution.

[0030] Preferably, the mass concentration of the hydrofluoric acid solution used for the first corrosion is 1-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the first corrosion time is 1-20 min, for example, it can be 1 min, 2 min, 4 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min or 20 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the first etching eats away the oxide layer. For example it could be

[0033] or However, it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the second etching comprises etching the silicon wafer after the first etching and eating away the silicon layer.

[0035] Preferably, the etching solution used in the second etching comprises a hydrofluoric acid solution.

[0036] Preferably, the mass concentration of the hydrofluoric acid solution used for the second etching is 1-40%, for example, it can be 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38% or 40%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0037] Preferably, the second corrosion time is 20-180 min, for example, it can be 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the thickness of the silicon layer eaten away by the second etching is ≤3μm, for example, it can be 3μm, 2.8μm, 2.5μm, 2.2μm, 2μm, 1.8μm, 1.5μm, 1.2μm, 1μm, 0.8μm, 0.5μm or 0.2μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] As a preferred technical solution of the present invention, the method comprises the following steps:

[0040] The silicon wafer to be tested is subjected to heat treatment at 600-1200° C. The heat treatment time is 1-120 min. Argon gas is filled in the heat treatment. The flow rate of argon gas in the heat treatment is less than 5 SLM. During the heat treatment, metal impurities react with silicon to generate metal silicide.

[0041] Cooling the heat-treated silicon wafer, wherein the cooling time is 5-120 minutes, and argon gas is filled in the cooling process, wherein the flow rate of argon gas in the cooling process is 5-10 SLM, and the cooling process reduces the solubility of metal silicide and precipitates it in the form of silicon rings;

[0042] The cooled silicon wafer is first subjected to a first etching to remove the oxide layer. The etching solution used in the first etching is a hydrofluoric acid solution with a mass concentration of 1-10%. The first etching time is 1-20 minutes. Then, the silicon wafer after the first corrosion is subjected to a second corrosion to eat away the silicon layer. The etching liquid used in the second corrosion is a hydrofluoric acid solution with a mass concentration of 1-40%. The second corrosion time is 20-180 minutes. The thickness of the silicon layer eaten away by the second corrosion is ≤3μm. The corrosion surfaces after the first corrosion and the second corrosion are observed respectively to see whether there are bright ring-shaped silicon rings. If there are, it proves that the silicon wafer contains metal impurities.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] The method provided by the present invention utilizes the reaction between a silicon wafer and the metal impurities contained in the silicon wafer to generate a metal silicide (silicon ring), and determines whether the silicon ring contains metal impurities by detecting the silicon ring, thereby achieving early screening of original wafers and pre-elimination of wafers with high metal impurity content. The method has good detection accuracy and can effectively detect metal impurities with a content of more than 10ppt, so that subsequent analysis resources and energy can be concentrated on higher-quality wafers, thereby improving the efficiency and output of the production line and maintaining the accuracy and stability of subsequent ICP analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a microscope photo of the corrosion surface detected in Example 1 of the present invention;

[0046] Figure 2 This is a microscope photo of the corrosion surface detected in Example 2 of the present invention;

[0047] Figure 3 This is a microscope photo of the corrosion surface detected in Example 3 of the present invention;

[0048] Figure 4 This is a microscope photo of the corrosion surface detected in Example 4 of the present invention;

[0049] Figure 5 This is a microscope photo of the corrosion surface detected in Comparative Example 1 of the present invention;

[0050] Figure 6 This is a microscope photograph of the corrosion surface detected in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] Example 1

[0053] This embodiment provides a method for detecting metal impurities in a silicon wafer, the method comprising the following steps:

[0054] The silicon wafer to be tested is subjected to heat treatment at 1200° C. The heat treatment time is 10 min. Argon gas is filled during the heat treatment. The flow rate of argon gas during the heat treatment is 4 SLM. During the heat treatment, metal impurities react with silicon to generate metal silicide.

[0055] The heat-treated silicon wafer is cooled to 25° C. The cooling time is 120 min. Argon gas is filled in the cooling process. The flow rate of argon gas in the cooling process is 6 SLM. The cooling process reduces the solubility of metal silicide and precipitates it in the form of silicon rings.

[0056] The silicon wafer after cooling is first subjected to a first etching to remove the oxide layer. The etching solution used in the first etching is a hydrofluoric acid solution with a mass concentration of 5%. The first etching time is 10 minutes. The thickness of the oxide layer removed by the first etching is The silicon wafer after the first corrosion is then subjected to a second corrosion to eat away the silicon layer. The etching liquid used for the second corrosion is a hydrofluoric acid solution with a mass concentration of 20%. The second corrosion time is 150 minutes, and the thickness of the silicon layer eaten away by the second corrosion is 1.5 μm. The corrosion surfaces after the first corrosion and the second corrosion are observed respectively to see whether there are bright ring-shaped silicon rings. If so, it proves that the silicon wafer contains metal impurities.

[0057] The silicon wafer used in this embodiment was tested by ICP-MS, and the metal impurity content of the silicon wafer was found to be as shown in Table 1.

[0058] Table 1

[0059]

[0060]

[0061] In this embodiment, the corrosion layer was observed under a microscope and it was found that a bright ring-shaped silicon ring existed, such as Figure 1 As shown, it can be seen from Table 1 that the Mo content reaches 14.326ppt, indicating that the metal impurity content of the silicon wafer is too high and needs to be removed in advance, and cannot enter the subsequent process.

[0062] Example 2

[0063] This embodiment provides a method for detecting metal impurities in a silicon wafer, the method comprising the following steps:

[0064] The silicon wafer to be tested is subjected to heat treatment at 600°C for 60 minutes. Argon gas is filled during the heat treatment. The flow rate of argon gas during the heat treatment is 3SLM. During the heat treatment, metal impurities react with silicon to generate metal silicide.

[0065] The heat-treated silicon wafer is cooled to 25° C. The cooling time is 55 minutes. Argon gas is filled in the cooling process. The flow rate of argon gas in the cooling process is 8 SLM. The cooling process reduces the solubility of metal silicide and precipitates it in the form of silicon rings.

[0066] The silicon wafer after cooling is first subjected to a first etching to remove the oxide layer. The etching solution used in the first etching is a hydrofluoric acid solution with a mass concentration of 2%. The first etching time is 20 minutes. The thickness of the oxide layer removed by the first etching is Then, the silicon wafer after the first corrosion is subjected to a second corrosion to eat away the silicon layer. The etching liquid used for the second corrosion is a hydrofluoric acid solution with a mass concentration of 10%. The second corrosion time is 180 minutes, and the thickness of the silicon layer eaten away by the second corrosion is 2 μm. The corrosion surfaces after the first corrosion and the second corrosion are observed respectively to see whether there are bright ring-shaped silicon rings. If there are, it proves that the silicon wafer contains metal impurities.

[0067] The silicon wafer used in this embodiment was tested by ICP-MS, and the metal impurity content of the silicon wafer was found to be as shown in Table 2.

[0068] Table 2

[0069]

[0070] In this embodiment, the corrosion layer was observed under a microscope and it was found that a bright ring-shaped silicon ring existed, such as Figure 2 As shown, and from Table 2, it can be seen that the Cr content reaches 12.275ppt and the Cu content reaches 11.213ppt, indicating that the metal impurity content of the silicon wafer is too high and needs to be removed in advance and cannot enter the subsequent process.

[0071] Example 3

[0072] This embodiment provides a method for detecting metal impurities in a silicon wafer, the method comprising the following steps:

[0073] The silicon wafer to be tested is subjected to heat treatment at 900°C for 120 minutes. Argon gas is filled during the heat treatment. The flow rate of argon gas during the heat treatment is 2SLM. During the heat treatment, metal impurities react with silicon to generate metal silicide.

[0074] The heat-treated silicon wafer is cooled to 25° C. The cooling time is 96 minutes. Argon gas is filled in the cooling process. The flow rate of argon gas in the cooling process is 5 SLM. The cooling process reduces the solubility of metal silicide and precipitates it in the form of silicon rings.

[0075] The silicon wafer after cooling is first subjected to a first etching to remove the oxide layer. The etching solution used in the first etching is a hydrofluoric acid solution with a mass concentration of 10%. The first etching time is 1 minute. The thickness of the oxide layer removed by the first etching is The silicon wafer after the first corrosion is then subjected to a second corrosion to eat away the silicon layer. The etching liquid used for the second corrosion is a hydrofluoric acid solution with a mass concentration of 40%. The second corrosion time is 20 minutes, and the thickness of the silicon layer eaten away by the second corrosion is 1.2 μm. The corrosion surfaces after the first corrosion and the second corrosion are observed respectively to see whether there are bright ring-shaped silicon rings. If so, it proves that the silicon wafer contains metal impurities.

[0076] The silicon wafer used in this embodiment was tested by ICP-MS, and the metal impurity content of the silicon wafer was found to be as shown in Table 3.

[0077] Table 3

[0078]

[0079] In this embodiment, the corrosion layer was observed under a microscope and it was found that a bright ring-shaped silicon ring existed, such as Figure 3 As shown, it means that the metal impurity content of the silicon wafer is too high and needs to be removed in advance, and it cannot enter the subsequent process.

[0080] Example 4

[0081] This embodiment provides a method for detecting metal impurities in a silicon wafer. The difference between the method and the embodiment 1 is that a different silicon wafer is selected.

[0082] The silicon wafer used in this embodiment was tested by ICP-MS, and the metal impurity content of the silicon wafer was found to be as shown in Table 4.

[0083] Table 4

[0084]

[0085] In this embodiment, the corrosion layer was observed under a microscope, and no bright ring-shaped silicon ring was found. Figure 4 As shown, it means that the metal impurity content of the silicon wafer meets the requirements for entering the subsequent process after preliminary judgment, and its impurity content can be further tested by ICP-MS and other methods before entering the production stage.

[0086] It can be seen from the data of Examples 1-4 that the method provided by the present invention has a detection threshold of 10 ppt for metal impurities in silicon wafers, that is, it has good detection accuracy for metal impurities with a content of more than 10 ppt, can achieve the effect of initial screening of original wafers, and can concentrate subsequent analysis resources and energy on higher quality wafers, thereby improving the efficiency and output of the production line and maintaining the accuracy and stability of subsequent ICP analysis.

[0087] Comparative Example 1

[0088] This comparative example provides a method for detecting metal impurities in a silicon wafer, the method being different from Example 1 only in that the heat treatment temperature is 550°C.

[0089] The silicon wafer used in this comparative example was tested by ICP-MS, and the metal impurity content of the silicon wafer was found to be as shown in Table 5.

[0090] Table 5

[0091]

[0092]

[0093] In this comparative example, the corrosion layer was observed using a microscope. Figure 5 As shown in the figure, no bright ring-shaped silicon ring is found, but it can be seen from Table 5 that the content of Ni element reaches 16.234ppt, which shows that Comparative Example 1 cannot effectively detect the presence of metal impurities above 10ppt. From the comparison between Example 1 and Comparative Example 1, it can be seen that in the present invention, by controlling the range of heat treatment temperature, the metal impurities therein are promoted to form silicon rings with the silicon wafer, thereby effectively detecting the presence of metal impurities above 10ppt.

[0094] Comparative Example 2

[0095] This comparative example provides a method for detecting metal impurities in a silicon wafer. The method is different from Example 1 only in that no cooling is performed.

[0096] The silicon wafer used in this comparative example was tested by ICP-MS, and the metal impurity content of the silicon wafer was found to be as shown in Table 6.

[0097] Table 6

[0098]

[0099] In this comparative example, the corrosion layer was observed using a microscope. Figure 6 As shown in Table 6, no bright ring-shaped silicon ring is found, but it can be seen from Table 6 that the content of Ti element reaches 13.18ppt, which shows that Comparative Example 2 cannot effectively detect the presence of metal impurities above 10ppt. From the comparison between Example 1 and Comparative Example 2, it can be seen that in the present invention, by first performing a heat treatment to generate a metal silicide reaction, and then cooling the metal silicide to precipitate, it is possible to effectively determine whether there are metal impurities above 10ppt by detecting the silicon ring.

[0100] In summary, the method provided by the present invention determines whether the silicon ring contains metal impurities by detecting the silicon ring, thereby achieving early screening of original wafers and pre-elimination of wafers with high metal impurity content, and has good detection accuracy.

[0101] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for detecting metal impurities in a silicon wafer, characterized in that: The method comprises the following steps: The silicon wafer to be tested is heat treated at 600-1200°C to make the metal impurities react with silicon to form metal silicide; The heat-treated silicon wafer is cooled to reduce the solubility of the metal silicide and precipitate in the form of silicon rings; The cooled silicon wafer is subjected to layered etching treatment to observe whether there is a bright ring-shaped silicon ring on the corrosion surface at different etching depths. If there is, it proves that the silicon wafer contains metal impurities.

2. The method according to claim 1, characterized in that The heat treatment time is 1-120 min.

3. The method according to claim 1 or 2, characterized in that: The cooling time is 5-120 minutes.

4. The method according to any one of claims 1 to 3, characterized in that: Argon gas was filled during the heat treatment.

5. The method according to claim 4, characterized in that The flow rate of argon gas during the heat treatment is less than 5 SLM.

6. The method according to any one of claims 1 to 5, characterized in that: During the cooling process, argon gas is filled; Preferably, the flow rate of argon gas in the temperature reduction cooling is 5-10 SLM.

7. The method according to any one of claims 1 to 6, characterized in that: The layered etching process includes a first etching and a second etching performed sequentially.

8. The method according to claim 7, characterized in that The first etching comprises etching the cooled silicon wafer and eating away the oxide layer; Preferably, the etching solution used in the first etching comprises a hydrofluoric acid solution; Preferably, the mass concentration of the hydrofluoric acid solution used in the first etching is 1-10%; Preferably, the first corrosion time is 1-20 min; Preferably, the first etching eats away the oxide layer.

9. The method according to claim 7, characterized in that: The second etching comprises etching the silicon wafer after the first etching and eating away the silicon layer; Preferably, the etching liquid used in the second etching comprises a hydrofluoric acid solution; Preferably, the mass concentration of the hydrofluoric acid solution used in the second etching is 1-40%; Preferably, the second corrosion time is 20-180 min; Preferably, the second etching eats away a thickness of the silicon layer of ≤3 μm.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: The silicon wafer to be tested is subjected to heat treatment at 600-1200° C. The heat treatment time is 1-120 min. Argon gas is filled in the heat treatment. The flow rate of argon gas in the heat treatment is less than 5 SLM. During the heat treatment, metal impurities react with silicon to generate metal silicide. Cooling the heat-treated silicon wafer, wherein the cooling time is 5-120 minutes, and argon gas is filled in the cooling process, wherein the flow rate of argon gas in the cooling process is 5-10 SLM, and the cooling process reduces the solubility of metal silicide and precipitates it in the form of silicon rings; The cooled silicon wafer is first subjected to a first etching to remove the oxide layer. The etching solution used in the first etching is a hydrofluoric acid solution with a mass concentration of 1-10%. The first etching time is 1-20 minutes. Then, the silicon wafer after the first corrosion is subjected to a second corrosion to eat away the silicon layer. The etching liquid used in the second corrosion is a hydrofluoric acid solution with a mass concentration of 1-40%. The second corrosion time is 20-180 minutes. The thickness of the silicon layer eaten away by the second corrosion is ≤3μm. The corrosion surfaces after the first corrosion and the second corrosion are observed respectively to see whether there are bright ring-shaped silicon rings. If there are, it proves that the silicon wafer contains metal impurities.