Chip, manufacturing method thereof and electronic equipment

By using the electroless gold plating method on the substrate of the chip, the seed layer and the electroplated gold layer are formed on the nickel-containing adhesive layer, the thickness difference between the inside and outside of the through holes of the conductive plating layer is solved, the chip performance and efficiency are improved, and the production cost is reduced.

CN119028923APending Publication Date: 2024-11-26HUAWEI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310610896.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The thickness of the conductive plating layer made on the back of the existing chips has a large difference in the thickness of the inside and outside of the through holes, resulting in uneven performance and affecting the performance of the chip.

Method used

The electroless gold plating method is used to form a seed layer and an electroplated gold layer on the nickel-containing adhesive layer. The replacement reaction between nickel and gold increases the thickness of the seed layer in the through hole, reduces the thickness difference between inside and outside the through hole, avoids the jaw phenomenon, and improves the Uniformity of conductive plating.

Benefits of technology

It effectively reduces the thickness difference between the conductive plating layer inside and outside the through hole, improves the performance of the conductive plating layer and the heat dissipation ability of the chip, and reduces the amount of gold used and production cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028923A_ABST
    Figure CN119028923A_ABST
Patent Text Reader

Abstract

According to the chip, the manufacturing method thereof and the electronic equipment provided by the invention, when the chemical gold-plating layer is manufactured on the nickel-containing adhesion layer by adopting a chemical gold-plating method, because the chemical gold-plating layer is not influenced by an electric field or a magnetic field, gold can easily enter the through hole without being influenced by an incident angle; gold is deposited on the surface of the adhesion layer through the replacement reaction of nickel and gold, and the gold entering the through hole can increase the thickness of the chemical gold-plated layer in the through hole and reduce the thickness difference of the chemical gold-plated layer inside and outside the through hole, so that the thickness difference of the conductive plating layer inside and outside the through hole is reduced, the mouth clamping phenomenon is avoided, and the service life of the through hole is prolonged. The uniformity of the conductive coating inside and outside the through hole is improved, and the performance of the conductive coating and even the chip is improved. Moreover, as the adhesion layer is the nickel-containing film layer, gold can be deposited on the surface of the adhesion layer, and gold cannot be deposited on other positions without the adhesion layer, so that the usage amount of gold is reduced, and the manufacturing cost of the chip is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a chip, a manufacturing method thereof, and an electronic device. Background Art

[0002] The chip includes a substrate and a semiconductor device disposed on the substrate, such as a transistor, a capacitor, etc. The surface on one side where the semiconductor device is disposed can be referred to as the front side of the substrate, and the surface on the other side can be referred to as the back side of the substrate. When a through hole is disposed in the substrate, the power supply terminal or the ground terminal of the semiconductor device can cover the through hole, and when a conductive coating is made on the back side of the substrate, the conductive coating not only covers the back side, but also covers the side wall of the through hole and the surface of the power supply terminal or the ground terminal exposed by the through hole, so that the heat generated by the semiconductor device during operation can be conducted away from the back side, thereby improving the heat dissipation capacity of the chip, and also simplifying the complexity of the front side structure of the substrate, and utilizing the back side space of the substrate to integrate the power supply terminal or the ground terminal of the semiconductor device.

[0003] However, in current technology, the thickness of the conductive coating made on the back of the substrate inside and outside the through hole varies greatly, and clamping phenomenon is prone to occur, which will lead to uneven performance of the conductive coating inside and outside the through hole, and then cause the performance of the conductive coating to decline, thereby affecting the performance of the chip. Summary of the invention

[0004] The present application provides a chip, a manufacturing method thereof and an electronic device, which can reduce the thickness difference of the conductive coating inside and outside the through hole, and improve the performance of the conductive coating and even the chip.

[0005] In the first aspect, an embodiment of the present application provides a chip, which may include a substrate and a conductive structure, wherein the substrate has: a first surface and a second surface arranged opposite to each other, and a through hole penetrating the first surface and the second surface, and the number of the through hole may be one, or two, three or more, and may be set according to actual needs, which is not limited here. The conductive structure may be arranged on the first surface, and the number of the conductive structures may be one, two or more, and the function of each conductive structure includes but is not limited to: being used to transmit power signals, ground signals or other signals, and the functions of each conductive structure may be the same, partially the same or different, and may be set according to actual needs, but no matter how many conductive structures are arranged and how the functions of each conductive structure are arranged, as long as there is a conductive structure covering the through hole, the number of through holes covered by the conductive structure is not limited here.

[0006] The chip may also include a conductive coating, which may be formed on the second surface, the side walls of the through hole and the surface of the conductive structure exposed by the through hole, wherein the portion of the second surface other than the through hole may be referred to as an outer-hole area, the side walls of the through hole may be referred to as hole walls, and the surface of the conductive structure exposed by the through hole may be regarded as a hole bottom, so that the outer-hole area, the hole walls and the hole bottom are all provided with a conductive coating, and the conductive coating is connected to the conductive structure, so that the heat in the conductive structure can be conducted to the second surface through the conductive coating and dissipated through the second surface, and the signal transmitted by the conductive structure can also be transmitted to the conductive coating.

[0007] Wherein, the conductive plating layer may include: an adhesion layer formed in the hole outer area, the hole wall and the hole bottom, a chemical gold plating layer formed on the adhesion layer, and an electroplated gold layer formed on the chemical gold plating layer, so that the adhesion layer, the chemical gold plating layer and the electroplated gold layer are stacked in sequence along the direction from the first surface to the second surface. In this way, when the chemical gold plating method is used to make the chemical gold plating layer (also referred to as the seed layer) on the nickel-containing adhesion layer, since the chemical plating is not affected by the electric field or the magnetic field, there is no problem of the incident angle of the particles, and then the gold will not be affected by the incident angle and can enter the through hole more easily, and the substitution reaction of nickel and gold is used to deposit gold on the surface of the adhesion layer, and the gold entering the through hole can increase the thickness of the seed layer in the through hole, reduce the thickness difference of the seed layer inside and outside the through hole, and then reduce the thickness difference of the electroplated gold layer inside and outside the through hole, thereby reducing the thickness difference of the conductive plating layer inside and outside the through hole, avoiding the clamping phenomenon, improving the uniformity of the conductive plating layer inside and outside the through hole, and improving the performance of the conductive plating layer and even the chip. Moreover, since the adhesion layer is a nickel-containing film layer, a seed layer can be produced on the surface of the adhesion layer, and gold will not be deposited at other locations without the adhesion layer. This solves the problem of gold waste caused by most of the gold being deposited on the inner wall of the equipment cavity in the physical vapor deposition (PVD) method, reduces the amount of gold used, and thus reduces the cost of chip production.

[0008] In some embodiments, for the chemical gold-plated layer, when the ratio of the first thickness located at any point in the through hole to the second thickness located at any point on the second surface can be set to be greater than or equal to 0.5, it means that the thickness difference of the seed layer inside and outside the through hole is small, which effectively reduces the resistance of the seed layer in the through hole. Therefore, when the gold-plated layer is produced by the gold-plating method on the seed layer, the gold-plated layer in the through hole can be made thicker, further reducing the thickness difference inside and outside the through hole during gold-plating, further improving the thickness uniformity of the conductive plating layer, and at the same time reducing the time for gold plating, which can not only save the use of gold, but also improve the production efficiency of the conductive plating layer and even the chip.

[0009] Exemplarily, any location within the through hole mentioned in the above content may include a location at one-third to two-thirds of the depth of the through hole. Exemplarily, for example, it includes a location at one-half the depth of the through hole. The thickness of the chemically plated gold layer at these locations is relatively close to the average thickness of the chemically plated gold layer at each location in the through hole. By selecting the thickness of the chemically plated gold layer at these locations as the first thickness, it is relatively easy to achieve a ratio of the first thickness to the second thickness greater than or equal to 0.5, which is beneficial to reduce the thickness difference of the electroplated gold layer inside and outside the through hole and reduce the time for electroplating gold.

[0010] Furthermore, the second thickness can be set to be greater than or equal to 300nm, which is conducive to achieving a certain thickness of the chemical gold-plated layer in the through hole, avoiding the thickness of the chemical gold-plated layer in the through hole being too thin and resulting in too large resistance, thereby helping to reduce the thickness difference of the electroplated gold layer inside and outside the through hole, and reducing the thickness difference of the conductive plating layer inside and outside the through hole, especially when the ratio of the first thickness to the second thickness is greater than or equal to 0.5, the thickness difference of the conductive plating layer inside and outside the through hole can be further reduced. Furthermore, when the second thickness is greater than or equal to 300nm, the internal stress of the chemical gold-plated layer can be reduced, and the chemical gold-plated layer can be avoided from warping, thereby helping to reduce the thickness difference of the conductive plating layer inside and outside the through hole, and improve the performance of the conductive plating layer and even the chip.

[0011] In some embodiments, for the adhesion layer, the atomic content of nickel can be set to be greater than or equal to 80%, and the corresponding atomic content of other elements is not greater than 20%, so that there is more nickel in the adhesion layer. Since chemical gold plating can be directly plated on the surface of the nickel-containing film layer without using any catalyst, and the nickel content in the adhesion layer has a certain influence on the gold plating effect, the higher the nickel content, the easier the gold plating will be, and the lower the nickel content, the lower the ease of gold plating, so the higher nickel content in the adhesion layer can promote and accelerate the deposition of gold, so that gold can be more easily deposited on the surface of the adhesion layer, and the production efficiency of the chemical gold plating layer is improved.

[0012] Furthermore, the adhesion layer can be made of at least one of elemental nickel and nickel-containing inorganic substances, and the adhesion layer can be a single-layer structure or a multi-layer structure. When the adhesion layer is a multi-layer structure, the materials of each layer can be the same or different, and can be set according to actual needs. Among them, when selecting the nickel-containing inorganic substance, at least one can be selected from nickel-vanadium alloy, nickel phosphide, nickel nitride, nickel boride, nickel-tungsten alloy, nickel-aluminum alloy, nickel-titanium alloy, nickel-thallium alloy and nickel-chromium alloy, so that the selection of materials has a wide range and meets the needs of various application scenarios.

[0013] In addition, when making the adhesion layer, the PVD method can be used, and the thickness of the adhesion layer can be controlled within a range of 0.1 μm to 0.5 μm. This can prevent the adhesion layer from being too thin and affecting the gold plating effect during chemical gold plating, making it easier to form a chemical gold plating layer on the adhesion layer. It can also prevent unnecessary waste when the adhesion layer is too thick, which is beneficial to reducing the production cost on the basis of reducing the thickness difference of the chemical gold plating layer inside and outside the through hole.

[0014] In some embodiments, the substrate may be made of a compound material of group III or group V, such as but not limited to GaP, GaAs, AlAs, AlP, AlSb, InP, InSb, InAs, GaInAs, GaInP, GaAlP, GaAlAs, etc. The conductive structure may be made of a conductive material, such as but not limited to conductive metals, conductive metal oxides, conductive metal alloys, conductive organics, etc.

[0015] In the second aspect, an embodiment of the present application provides a method for manufacturing a chip, which may include: forming a conductive structure on a substrate, the substrate having a first surface and a second surface arranged opposite to each other, and a through hole penetrating the first surface and the second surface, the conductive structure is located on the first surface and covers the through hole; forming an adhesion layer on the second surface, the side wall of the through hole and the surface of the conductive structure exposed by the through hole, the adhesion layer including nickel element; forming a chemical gold-plated layer on the adhesion layer; and forming an electroplated gold layer on the chemical gold-plated layer.

[0016] Thus, when a chemical gold-plating layer (also referred to as a seed layer) is made on a nickel-containing adhesion layer by using a chemical gold-plating method, since chemical plating is not affected by an electric field or a magnetic field, there is no problem of the incident angle of the particles, and thus gold is not affected by the incident angle and can enter the through hole more easily, and the gold is deposited on the surface of the adhesion layer by using the substitution reaction of nickel and gold, and the gold entering the through hole can increase the thickness of the seed layer in the through hole, reduce the thickness difference of the seed layer inside and outside the through hole, and then reduce the thickness difference of the electroplated gold layer inside and outside the through hole, thereby reducing the thickness difference of the conductive coating inside and outside the through hole, avoiding the occurrence of a clamping phenomenon, improving the uniformity of the conductive coating inside and outside the through hole, and improving the performance of the conductive coating and even the chip. In addition, since the adhesion layer is a nickel-containing film layer, a seed layer can be made on the surface of the adhesion layer, and gold will not be deposited at other positions without the adhesion layer, thus solving the problem of gold waste caused by most of the gold being deposited on the inner wall of the equipment cavity in the PVD method, reducing the amount of gold used, and thus reducing the production cost of the chip.

[0017] Since the principle of solving the problem by the manufacturing method is similar to the principle of solving the problem by the aforementioned chip, the embodiments and technical effects of the manufacturing method can refer to the embodiments and technical effects of the aforementioned chip, and the repeated parts will not be repeated.

[0018] In a third aspect, an embodiment of the present application provides an electronic device, which may include: a circuit board and a chip as described in the first aspect, the chip being disposed on the circuit board. Since the uniformity of the thickness of the conductive coating inside and outside the through hole is improved, the performance of the conductive coating and even the chip is improved, and the manufacturing cost and manufacturing efficiency of the conductive coating can be reduced, the electronic device manufactured using the chip can also achieve the purpose of improving performance, reducing manufacturing costs, and improving manufacturing efficiency.

[0019] Since the principle of solving the problem by the electronic device is similar to the principle of solving the problem by the aforementioned chip, the embodiments and technical effects of the electronic device can refer to the embodiments and technical effects of the aforementioned chip, and the repeated parts will not be repeated. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic diagram of the structure of an electronic device provided in an embodiment of the present application;

[0021] Figure 2 A schematic diagram of the structure of a chip provided in an embodiment of the present application;

[0022] Figure 3 A schematic diagram of the chip manufacturing process provided in the embodiment of the present application;

[0023] Figure 4 A cross-sectional view of an adhesion layer and a chemical gold plating layer provided in an embodiment of the present application;

[0024] Figure 5 is a cross-sectional view of an adhesion layer and a gold layer in the prior art;

[0025] Figure 6 is a cross-sectional view of an electroplated gold layer formed on a chemically plated gold layer;

[0026] Figure 7 This is a cross-sectional view of an electroplated gold layer formed on a gold layer formed by a PVD method.

[0027] Reference numerals:

[0028] 10-substrate, 11-through hole, 20-conductive structure, 30-conductive plating layer, 31-adhesion layer, 32-chemical gold plating layer, 33-electroplated gold layer, 100-housing, 200-circuit board, 300-chip, b1-first surface, b2-second surface, b3-hole wall. DETAILED DESCRIPTION

[0029] In order to make the objectives, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings.

[0030] It should be noted that the same reference numerals in the drawings of this application represent the same or similar structures, and thus their repeated description will be omitted. The words expressing positions and directions described in this application are all explained using the drawings as examples, but they can be changed as needed, and the changes are included in the protection scope of this application. The drawings of this application are only used to illustrate the relative position relationship and do not represent the true proportion.

[0031] In order to facilitate understanding of the technical solution provided in the embodiments of the present application, the application scenario is first explained.

[0032] The chip provided in the embodiment of the present application can be widely used in various electronic devices, and the electronic devices may include various terminal devices and electronic devices. Among them, the terminal devices may include but are not limited to smart phones, smart TVs, smart TV set-top boxes, smart watches, personal computers (PCs), wearable devices, smart broadband and other devices. Electronic devices may include but are not limited to wireless networks, fixed networks, servers and other telecommunication equipment, as well as chip modules, memory and other devices, which are not listed here one by one.

[0033] Figure 1 The schematic diagram of the structure of the chip when it is used in an electronic device is shown as an example. Figure 1 As shown, the electronic device includes a housing 100 and a circuit board 200 disposed in the housing 100, and a chip 300 is disposed on the circuit board 200. The chip 300 may include a substrate and a semiconductor device disposed on the substrate, such as a transistor, a capacitor, etc. The surface on one side of the substrate where the semiconductor device is disposed may be referred to as the front side of the substrate, and the surface on the other side may be referred to as the back side of the substrate. A through hole is disposed in the substrate, and the power supply terminal or the ground terminal of the semiconductor device may cover the through hole. When a conductive coating is made on the back side of the substrate, the conductive coating not only covers the back side of the substrate, but also covers the side wall of the through hole and the surface of the power supply terminal or the ground terminal exposed by the through hole, so that the conductive coating is connected to the power supply terminal or the ground terminal, so that the heat generated by the semiconductor device during operation can be conducted away from the back side of the substrate, thereby improving the heat dissipation capacity of the chip 300, and also simplifying the structural complexity of the front side of the substrate, and utilizing the back side space of the substrate to integrate the power line or the ground line required in the circuit.

[0034] At present, when making a conductive coating on the back of a substrate, a titanium layer or a titanium-tungsten layer can be firstly sputtered as an adhesion layer on the back of the substrate, the sidewall of the through hole, and the surface of the power supply terminal or the ground terminal exposed by the through hole by the PVD method, and then a layer of gold is sputtered as a seed layer on the surface of the adhesion layer by the PVD method, and finally, the surface of the seed layer is plated with gold by electroplating to increase the thickness of the conductive coating. Since the PVD method cannot control the incident angle of the particles, it is difficult for particles with large angles to enter the through hole, resulting in a larger thickness of the seed layer outside the through hole, while the thickness of the seed layer inside the through hole is smaller. Based on the principle that the greater the thickness, the smaller the resistance, and the smaller the thickness, the greater the resistance, when electroplating gold, the thickness of the gold inside the through hole will be much smaller than the thickness of the gold outside the through hole, resulting in a large difference in the thickness of the conductive coating inside and outside the hole, which ultimately leads to poor performance of the conductive coating.

[0035] Based on this, the embodiments of the present application provide a chip, a manufacturing method thereof, and an electronic device, which can reduce the thickness difference of the conductive coating inside and outside the through hole, avoid the clamping phenomenon, improve the uniformity of the conductive coating inside and outside the through hole, and improve the performance of the conductive coating and even the chip.

[0036] Figure 2 The schematic diagram of the structure of the chip provided in the embodiment of the present application is exemplarily shown. Figure 2 As shown, the chip may include a substrate 10 and a conductive structure 20, wherein the substrate 10 has: a first surface b1 and a second surface b2 arranged opposite to each other, and a through hole 11 penetrating the first surface b1 and the second surface b2, and the number of the through hole 11 may be one, or two, three or more, and may be set according to actual needs, which is not limited here. The conductive structure 20 may be arranged on the first surface b1, and the number of the conductive structure 20 may be one, two or more, and the function of each conductive structure 20 includes but is not limited to being used for transmitting power signals, ground signals or other signals, and the functions of each conductive structure 20 may be the same, partially the same or different, and may be set according to actual needs, but no matter how many conductive structures 20 are arranged and how the functions of each conductive structure 20 are arranged, as long as there is a conductive structure 20 covering the through hole 11, it is sufficient, and the number of through holes 11 covered by the conductive structure 20 is not limited here.

[0037] Continue to refer to Figure 2As shown, the chip may further include a conductive coating 30, which may be formed on the second surface b2, the side walls of the through hole 11 and the surface of the conductive structure 20 exposed by the through hole 11, wherein the portion of the second surface b2 other than the through hole 11 may be referred to as an outer-hole area, the side walls of the through hole 11 may be referred to as hole walls b3, and the surface of the conductive structure 20 exposed by the through hole 11 may be regarded as a hole bottom, so that the outer-hole area, the hole walls b3 and the hole bottom are all provided with the conductive coating 30, and the conductive coating 30 is connected to the conductive structure 20, so that the heat in the conductive structure 20 may be conducted to the second surface b2 through the conductive coating 30 and dissipated through the second surface b2, and the signal transmitted by the conductive structure 20 may also be transmitted to the conductive coating 30.

[0038] The conductive plating layer 30 may include: an adhesion layer 31 formed on the hole outer area, the hole wall b3 and the hole bottom, a chemical gold plating layer 32 formed on the adhesion layer 31, and an electroplated gold layer 33 formed on the chemical gold plating layer 32, so that the adhesion layer 31, the chemical gold plating layer 32 and the electroplated gold layer 33 are directed along the first surface b1 to the second surface b2 (i.e. Figure 2 The adhesion layer 31 is stacked in sequence (in the F1 direction). The preparation material of the adhesion layer 31 includes nickel element. Exemplarily, the adhesion layer 31 can be made of at least one of elemental nickel and nickel-containing inorganic substances. When selecting the nickel-containing inorganic substance, at least one can be selected from, but not limited to, nickel-vanadium alloy, nickel phosphide, nickel nitride, nickel boride, nickel-tungsten alloy, nickel-aluminum alloy, nickel-titanium alloy, nickel-thallium alloy and nickel-chromium alloy, so that the material selection has a wide range to meet the needs of various application scenarios. In addition, the adhesion layer 31 can be a single-layer structure or a multi-layer structure. When the adhesion layer 31 is a multi-layer structure, the materials for making each layer can be the same or different, and can be specifically set according to actual needs.

[0039] In this way, when a chemical gold plating method is used to make a chemical gold-plated layer (also called a seed layer) 32 on the nickel-containing adhesion layer 31, since chemical plating is not affected by electric fields or magnetic fields, there is no problem of the incident angle of the particles, and gold will not be affected by the incident angle and can easily enter the through hole 11. The gold is deposited on the surface of the adhesion layer 31 by utilizing the substitution reaction between nickel and gold, and the gold that enters the through hole 11 can increase the thickness of the seed layer in the through hole 11, reduce the thickness difference of the seed layer inside and outside the through hole 11, and then reduce the thickness difference of the electroplated gold layer 33 inside and outside the through hole 11, thereby reducing the thickness difference of the conductive plating layer 30 inside and outside the through hole 11, avoiding the clamping phenomenon, improving the uniformity of the conductive plating layer 30 inside and outside the through hole 11, and improving the performance of the conductive plating layer 30 and even the chip.

[0040] Exemplarily, the adhesion layer 31 can be formed by PVD method, so that the produced adhesion layer 31 can be a nickel-containing film layer. In this way, the substitution reaction between nickel and gold can be used to produce a gold layer on the surface of the adhesion layer 31 by chemical gold plating method to obtain a seed layer, while gold will not be deposited at other locations without the adhesion layer 31. In this way, the problem of gold waste caused by most of the gold being deposited on the inner wall of the device cavity in the PVD method is solved, so that the use of gold is reduced, thereby reducing the production cost of the chip.

[0041] It should be understood that the chemical gold plating method is a method based on the principle of redox, which utilizes chemical reactions to deposit gold on the adhesion layer 31. This method does not require external current. The electroplating gold method is a method in which gold ions are discharged under the action of external current to form a gold layer.

[0042] Reference Figure 2 As shown, for the chemical gold-plated layer 32, the ratio of the first thickness d1 located at any point in the through hole 11 to the second thickness d2 located at any point on the second surface b2 can be greater than or equal to 0.5, indicating that the thickness difference of the seed layer inside and outside the through hole 11 is small, which effectively reduces the resistance of the seed layer in the through hole 11. Therefore, when the gold-plated layer 33 is produced on the seed layer by the gold-plating method, the gold-plated layer 33 in the through hole 11 can be made thicker, further reducing the thickness difference inside and outside the through hole 11 during gold-plating, further improving the thickness uniformity of the conductive plating layer 30, and also reducing the time of gold-plating, thereby not only saving the amount of gold used, but also improving the production efficiency of the conductive plating layer 30 and even the chip.

[0043] Reference Figure 2 As shown, for the chemical gold-plated layer 32, the second thickness d2 located at any point of the second surface b2 can be set to be greater than or equal to 300 nm, which is conducive to achieving a certain thickness of the chemical gold-plated layer 32 in the through hole 11, avoiding the thickness of the chemical gold-plated layer 32 in the through hole 11 being too thin and resulting in too large resistance, thereby helping to reduce the thickness difference of the electroplated gold layer 33 inside and outside the through hole 11, and reduce the thickness difference of the conductive plating layer 30 inside and outside the through hole 11, especially when the ratio of the first thickness d1 to the second thickness d2 is greater than or equal to 0.5, the thickness difference of the conductive plating layer 30 inside and outside the through hole 11 can be further reduced.

[0044] Figure 3 The schematic diagram of the process of manufacturing the chip provided in the embodiment of the present application is shown as an example. Figure 3 As shown, the following steps may be included:

[0045] Step 1: Figure 3As shown in (a), in a substrate 10 having a first surface b1 and a second surface b2 disposed opposite to each other, a through hole 11 penetrating the first surface b1 and the second surface b2 is formed;

[0046] like Figure 3 As shown in (a), the first surface b1 and the second surface b2 in the substrate 10 are arranged opposite to each other along the thickness direction of the substrate 10, and the through hole 11 extends along the thickness direction of the substrate 10 and penetrates the first surface b1 and the second surface b2. The size and shape of the through hole 11 can be set according to actual needs. For example, but not limited to, the cross-sectional shape of the through hole 11 parallel to the first surface b1 can be elliptical, circular or irregular. Taking the elliptical shape as an example, the shortest diameter can be, but not limited to, 30 μm, and the longest diameter can be, but not limited to, 60 μm. In addition, when making the through hole 11, the through hole 11 can be etched in the substrate 10 by plasma etching, but not limited to.

[0047] Step 2: If Figure 3 As shown in (b), a conductive structure 20 covering the through hole 11 is formed on the first surface b1;

[0048] like Figure 3 As shown in (b), the figure takes a conductive structure 20 covering a through hole 11 as an example. If the structure in Figure (b) is turned upside down, the surface of the conductive structure 20 exposed by the through hole 11 can be regarded as the bottom of the through hole 11.

[0049] Step 3: Form a conductive plating layer 30 on the second surface b2, the side walls of the through hole 11 and the surface of the conductive structure 20 exposed by the through hole 11; wherein the conductive plating layer 30 includes: an adhesion layer 31, a chemical gold plating layer 32 and an electroplated gold plating layer 33 stacked in sequence along a direction from the first surface b1 to the second surface b2, wherein the adhesion layer 31 includes nickel element.

[0050] The following is a detailed introduction to the manufacturing process of the conductive plating layer 30, which may specifically include the following steps:

[0051] Step 3.1: If Figure 3 As shown in (c), based on the PVD method, a material containing nickel element is used to form an adhesion layer 31 on the second surface b2, the hole wall b3 and the hole bottom, and the thickness d3 of the adhesion layer 31 can be controlled to be 0.1μm to 0.5μm.

[0052] Step 3.2: Cleaning the chip on which the adhesion layer 31 is formed.

[0053] Exemplarily, a plasma with a certain power (for example, but not limited to 400 W) is used, an inert gas (for example, but not limited to argon) is introduced, and the chip formed with the adhesion layer 31 is cleaned for a period of time (for example, but not limited to 90 seconds), and then the cleaned chip is kept in a vacuum for a certain period of time (for example, but not limited to 5 minutes) to remove organic pollutants on the chip surface; thereafter, the chip is cleaned using a sulfuric acid solution of a certain concentration (for example, but not limited to 5%) at room temperature to remove the oxide film on the chip surface.

[0054] Step 3.3: If Figure 3 As shown in (d) in FIG. 1 , a chemical gold plating layer 32 is formed on the adhesion layer 31 by using a chemical gold plating method.

[0055] Among them, the specific production process of the chemical gold-plated layer 32 can include the following two steps: the first step is to use a displacement gold plating solution to cause a replacement reaction between nickel and gold on the surface of the adhesion layer 31, so that the surface of the adhesion layer 31 contains gold (which can be called a displacement gold layer); the second step is to use a chemical gold plating solution to continue gold plating on the surface of the displacement gold layer to thicken the thickness of the gold layer to obtain a chemical gold-plated layer 32, so that the thickness of the chemical gold-plated layer 32 at any point on the second surface b2 is greater than or equal to 300nm, and the ratio of the thickness of the chemical gold-plated layer 32 at one-half of the through hole 11 to the thickness of the chemical gold-plated layer 32 at any point on the second surface b2 is greater than or equal to 0.5.

[0056] Exemplarily, the replacement gold plating solution generally includes multiple components. A certain volume of each component is measured and mixed together, and the volume is supplemented to the target volume (for example, but not limited to 1L) to obtain a mixed solution A. The pH of the mixed solution A is adjusted to a preset value (for example, but not limited to 7.2). After the temperature of the mixed solution A is increased to a preset temperature (for example, but not limited to 74°C), the chip treated in step 3.2 is placed in the heated mixed solution A to allow the nickel and gold on the surface of the adhesion layer 31 to undergo a replacement reaction. After a period of reaction (for example, but not limited to 12 minutes), the chip is taken out and cleaned to obtain a chip containing a replacement gold layer on the surface of the adhesion layer 31.

[0057] Exemplarily, the chemical gold plating solution also generally includes multiple components. A certain volume of each component is measured and mixed together, and the volume is supplemented to a target volume (for example, but not limited to 1L) to obtain a mixed solution B. The pH of the mixed solution B is adjusted to a preset value (for example, but not limited to 7.2). After the temperature of the mixed solution B is increased to a preset temperature (for example, but not limited to 50°C), the chip formed with the replacement gold layer is placed in the heated mixed solution B, so that the gold in the chemical gold plating solution undergoes a reduction reaction, and a reduced gold layer is formed on the surface of the replacement gold layer, thereby increasing the thickness of the gold layer. After a period of reaction (for example, but not limited to 3 minutes), the chip is taken out and cleaned to obtain a chip formed with a chemical gold plating layer 32, wherein the chemical gold plating layer 32 includes a replacement gold layer and a reduced gold layer.

[0058] Of course, when manufacturing the chemical gold-plated layer 32 , it is not limited to the above two-step method. Other methods that can obtain the chemical gold-plated layer 32 can also be used, which are not limited here.

[0059] Step 3.4: Cleaning the chip on which the chemical gold plating layer 32 is formed.

[0060] For the specific cleaning process, please refer to the cleaning process introduced in the above step 3.2.

[0061] Step 3.5: If Figure 3 As shown in (e) in FIG. 1 , an electroplated gold layer 33 is formed on the chemically plated gold layer 32 .

[0062] When forming the electroplated gold layer 33, the chip processed in step 3.4 can be first fixed on the substrate with the chemical gold-plated layer 32 facing upward, and then the substrate with the chip fixed can be transferred to the electroplating machine fixture, and electroplating can be performed step by step using electroplating gold liquid. After the electroplating is completed, it can be cleaned and dried with deionized water to obtain the electroplated gold layer 33.

[0063] Exemplarily, the current used in each electroplating step during step-by-step electroplating can be different, and the current size used in each electroplating step can be increased in sequence according to the electroplating order. For example, taking two-step electroplating as an example, the current used in the first step of electroplating is less than the current used in the second step of electroplating. The advantage of such a setting is that a smaller current is used in the previous electroplating step, the thickness of the gold in the through hole 11 can be thickened, and the thickness difference of the gold inside and outside the through hole 11 can be reduced. In the subsequent steps, a larger current is used to increase the thickness of the gold to reach the designed thickness of the electroplated gold layer 33, so that the thickness difference of the electroplated gold layer 33 inside and outside the through hole 11 can be ensured to be small, and the manufacturing efficiency can also be improved. Of course, step-by-step electroplating can be but not limited to two-step electroplating, which can be determined according to the actual situation and is not limited here.

[0064] The following introduces the conductive plating through specific test results.

[0065] Example: Refer to Figure 4 and Figure 5 As shown, Figure 4 The cross-sectional views of the adhesion layer and the chemical gold plating layer provided in the embodiment of the present application at different positions and different magnifications are as follows: Figure 5 The following are cross-sectional views of the adhesion layer and the gold layer in the prior art at different positions and different magnifications, wherein the adhesion layer in the prior art is made by PVD method and the material is titanium metal, and the gold layer in the prior art is made by PVD method. Figure 4 and Figure 5In the figure, the magnification of (a) is greater than that of (b), and the magnification of (b) is greater than that of (c). Figure 4 and Figure 5 The structure shown is found:

[0066] 1. The second thickness d2 of the chemical gold-plated layer on the second surface provided in the embodiment of the present application is about 592nm to 620nm. Figure 4 As shown in (b) in FIG. 1 , the first thickness d1 of the chemically plated gold layer corresponding to half the depth of the through hole is approximately 324 nm to 374 nm. Figure 4 As shown in (c), the ratio of the first thickness d1 to the second thickness d2 is greater than 0.5. Therefore, the chemical gold plating layer provided in the embodiment of the present application has a large thickness and a flat surface (such as Figure 4 ).

[0067] 2. The second thickness d2 of the gold layer on the second surface in the prior art is about 128nm to 256nm. Figure 5 As shown in (b) in FIG. 1 , the first thickness d1 of the gold layer corresponding to half the depth of the through hole is about 31 nm to 40 nm. Figure 5 As shown in (c), the ratio of the first thickness d1 to the second thickness d2 is less than 0.3. Therefore, the gold layer in the prior art is relatively thin, island-shaped, and has an uneven surface (such as Figure 5 ).

[0068] After analyzing the reasons, it was found that compared with the gold layer made by the PVD method, the chemical gold-plated layer has a larger internal stress than the gold layer deposited by the PVD method. Increasing the thickness of the gold layer may cause the gold layer to warp and the adhesion layer to separate, and even cause the wafer to tear, so the resulting gold layer is island-shaped and has an uneven surface. In addition, most of the gold in the PVD method is deposited on the inner wall of the cavity of the equipment, so that the gold deposited on the adhesion layer is limited, resulting in a thinner thickness of the gold layer. The gold layer made by the chemical gold plating method (i.e., the chemical gold-plated layer) can avoid the above problems, so that the chemical gold-plated layer has a flat surface and a larger thickness.

[0069] Example: Refer to Figure 6 and Figure 7 As shown, Figure 6 The cross-sectional view of the electroplated gold layer made on the chemical gold-plated layer at different positions and different magnifications. Figure 7 The cross-sectional diagram of the electroplated gold layer made on the gold layer made by PVD method at different positions and different magnifications. Figure 6 and Figure 7 In the figure, the magnification of (a) is greater than that of (b), and the magnification of (b) is greater than that of (c). Figure 6 and Figure 7 The structure shown is found:

[0070] 1. The electroplated gold layer made on the gold layer made by PVD method has a larger thickness outside the hole and a smaller thickness at the bottom of the hole, resulting in a clamping phenomenon, such as Figure 7 As shown in the solid circle in (a) of FIG. This is because when the PVD method is used to make the gold layer, the incident angle of the particles makes it difficult for the gold to be effectively sputtered into the through hole, resulting in a smaller thickness and a larger resistance of the gold layer in the through hole. Therefore, during the electroplating process, the current in the through hole is smaller, and the thickness of the electroplated gold layer is thinner, especially at the bottom of the hole. Since the thickness difference of the chemically plated gold layer inside and outside the through hole is small, the resistance of the chemically plated gold layer in the through hole is small, resulting in a larger current in the through hole during the electroplating process, which increases the thickness of the electroplated gold layer in the through hole and avoids the occurrence of the clamping phenomenon, as shown in FIG. Figure 6 As shown in the solid coil in (a).

[0071] 2. For the electroplated gold layer made on the gold layer made by PVD method: the thickness d4 of the electroplated gold layer in the area outside the hole is about 8.51μm, such as Figure 7 As shown in (b) in FIG. 1 , the thickness d5 of the electroplated gold layer at the bottom of the hole is about 3.90 μm. Figure 7 As shown in (c) in FIG. 1 , the ratio of the thickness d5 to the thickness d4 is 45.9%. For the electroplated gold layer formed on the chemically plated gold layer: the thickness d4 of the electroplated gold layer in the area outside the hole is about 7.63 μm, as shown in FIG. Figure 6 As shown in (b) in FIG. 1 , the thickness d5 of the electroplated gold layer at the bottom of the hole is about 4.64 μm. Figure 6 As shown in (c), the ratio of thickness d4 to thickness d5 is 60.8%. It can be seen that the thickness difference between the inside and outside of the through hole of the electroplated gold layer made on the chemical gold-plated layer is smaller, and the thickness of the electroplated gold layer in the through hole is greater. If the thickness of the electroplated gold layer at the bottom of the hole is required to be 4μm, according to the above ratio, when the electroplated gold layer is made on the gold layer made by the PVD method, the electroplated gold layer in the area outside the hole needs to be electroplated to 8.87μm, and when the electroplated gold layer is made on the chemical gold-plated layer, the electroplated gold layer in the area outside the hole only needs to be electroplated to 6.58μm. In comparison, making an electroplated gold layer on a chemical gold-plated layer can save 30% of electroplated gold, which can effectively save the amount of gold used and reduce production costs. From another perspective, when the electroplated gold layer is made on the chemical gold-plated layer, it has a better filling ability for the through hole.

[0072] It should be understood that during gold electroplating, the gold in the through-hole is consumed quickly and cannot be replenished in time, so the thickness of the gold electroplated layer inside and outside the through-hole cannot be equal under the two processes.

[0073] Obviously, those skilled in the art can make various changes and modifications to the embodiments of the present application without departing from the spirit and scope of the embodiments of the present application. Thus, if these modifications and variations of the embodiments of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A chip, characterized in that: include: A substrate having a first surface and a second surface arranged opposite to each other, and a through hole penetrating the first surface and the second surface; a conductive structure, the conductive structure being located on the first surface and covering the through hole; A conductive plating layer, wherein the conductive plating layer is formed on the second surface, the sidewall of the through hole and the surface of the conductive structure exposed by the through hole; wherein the conductive plating layer comprises: an adhesion layer, a chemical gold plating layer and an electroplated gold plating layer, which are sequentially stacked in a direction from the first surface to the second surface, and the adhesion layer comprises nickel element.

2. The chip according to claim 1, characterized in that: The chemical gold-plated layer at any location in the through hole has a first thickness, and the chemical gold-plated layer at any location on the second surface has a second thickness, and a ratio of the first thickness to the second thickness is greater than or equal to 0.

5.

3. The chip according to claim 2, characterized in that: Any location within the through hole includes a location at one-half the depth of the through hole.

4. The chip according to any one of claims 1 to 3, characterized in that: The thickness of the chemically plated gold layer located at any location of the second surface is greater than or equal to 300 nm.

5. The chip according to any one of claims 1 to 4, characterized in that: The atomic content of the nickel element included in the adhesion layer is greater than or equal to 80%.

6. The chip according to any one of claims 1 to 5, characterized in that: The adhesion layer includes at least one of elemental nickel and a nickel-containing inorganic substance.

7. The chip according to any one of claims 1 to 6, characterized in that: The thickness of the adhesive layer is 0.1 μm to 0.5 μm.

8. A method for manufacturing a chip, characterized in that: include: Forming a conductive structure on a substrate, wherein the substrate has a first surface and a second surface that are opposite to each other, and a through hole that penetrates the first surface and the second surface, and the conductive structure is located on the first surface and covers the through hole; forming an adhesion layer on the second surface, the sidewall of the through hole and the surface of the conductive structure exposed by the through hole, wherein the adhesion layer includes nickel element; forming a chemical gold plating layer on the adhesion layer; An electroplated gold layer is formed on the chemically plated gold layer.

9. The method of claim 8, wherein: Forming an adhesion layer, comprising: The adhesion layer is formed by a physical vapor deposition method.

10. The production method according to claim 8 or 9, characterized in that: The chemical gold-plated layer formed at any location in the through hole has a first thickness, the chemical gold-plated layer formed at any location on the second surface has a second thickness, and a ratio of the first thickness to the second thickness is greater than or equal to 0.

5.

11. The production method according to any one of claims 8 to 10, characterized in that: The thickness of the chemical gold plating layer formed at any location of the second surface is greater than or equal to 300 nm.

12. An electronic device, characterized in that: include: A circuit board and a chip as claimed in any one of claims 1 to 7, wherein the chip is arranged on the circuit board.

Citation Information

Cited By

  • Chip and manufacturing method therefor, and electronic device

    EP4708358A1