Cellulose-based composite diaphragm, preparation method thereof and lithium ion battery
By non-covalent crosslinking of sodium alginate and cellulose in a freezing environment, a cellulose-based composite separator is formed, which solves the problem of insufficient mechanical strength and thermal stability of existing separators and improves the electrochemical performance of lithium-ion batteries And reduce production costs.
Patent Information
- Application Number
- CN202411134902.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing cellulose-based lithium-ion battery separators have shortcomings in terms of mechanical strength, thermal stability and electrochemical performance, and are difficult to meet the needs of high-end products.
In a freezing environment, sodium alginate is introduced into the cellulose solution for non-covalent cross-linking to form a cellulose-based composite separator, improve mechanical strength and thermal stability, and enhance the wetting ability of the electrolyte through a 3D mesh porous structure.
It significantly improves the mechanical strength and thermal stability of the diaphragm, reduces the diffusion distance of Li+, enhances the electrochemical performance of the battery, and reduces production costs.
Smart Images

Figure BDA0005002131680000121 
Figure BDA0005002131680000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery diaphragms, and in particular to a cellulose-based composite diaphragm and a preparation method thereof, and a lithium ion battery. Background Art
[0002] With the rapid economic development, my country's total energy consumption ranks second in the world. However, due to the uneven distribution of energy resources and the difficulty of development, the per capita possession of resources such as oil and natural gas is seriously insufficient. In addition, the consumption of traditional energy will have an unignorable impact on the environment in which humans survive. Therefore, it is necessary to find a renewable clean energy to alleviate the crisis of energy shortage and environmental pollution. Lithium-ion batteries, as a new energy technology with high energy density, long cycle life, high operating voltage, strong tolerance, no pollution and fast charge and discharge, have been widely used in the energy storage industry.
[0003] Commercial lithium battery separators are mainly made of polyolefin materials, but they generally have problems such as low safety performance, electrolyte leakage, complex manufacturing process and high cost. In addition, the overall performance of domestically produced separators is unstable and it is difficult to meet the needs of high-end products. Cellulose is a renewable resource. Compared with synthetic polymers, it has the advantages of complete degradation, non-toxicity, non-pollution, easy modification and good biocompatibility. It is recognized as the main raw material for green energy and chemical industry in the world. Due to its abundant sources, low cost, high heat resistance, good mechanical strength, good liquid absorption and wettability, cellulose has become an ideal substitute for polyolefin materials. Therefore, it is of great significance for cellulose-based composite separators to replace commercial lithium-ion battery separators, which will help improve the sustainability and economy of lithium-ion batteries, reduce the impact on the environment, and promote the battery industry to develop in a more sustainable direction.
[0004] The prior art discloses a cellulose separator for lithium batteries, which comprises firstly mixing and stirring a cellulose aqueous dispersion, a sodium lignin sulfonate aqueous solution, a crosslinking agent aqueous solution and an ammonium polyphosphate aqueous solution to form a mixed solution, then freeze-drying the mixed solution to form a film, heating the film and rolling the film to a certain thickness to obtain a cellulose separator for lithium batteries. The above preparation method requires the coordination of multiple raw materials, which not only greatly increases the production cost, but also does not significantly improve the mechanical strength and thermal stability of the prepared cellulose separator.
[0005] The prior art discloses a method for preparing a cellulose / carbon nanotube composite nanofiber membrane, which utilizes high-voltage electrostatic spinning to form a film. Compared with traditional polyolefin membranes, the battery separator has higher electrical activity. However, the separator still has problems in terms of mechanical strength, membrane porosity and liquid absorption rate, resulting in no obvious improvement in overall performance.
[0006] Based on the above-mentioned problems with cellulose-based separators, there is an urgent need to develop a cellulose-based battery separator with a simple preparation process while ensuring that the prepared cellulose-based battery separator has excellent wetting properties, thermal stability and mechanical strength, thereby improving the electrochemical performance of the battery. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a cellulose-based composite diaphragm and a preparation method thereof and a lithium-ion battery. In the present invention, sodium alginate is introduced into a cellulose solution under a freezing environment, and non-covalent cross-linking of multiple hydrogen bonds between molecules is performed, and then solidified, thereby effectively enhancing the mechanical strength of the diaphragm; after sodium alginate and cellulose are composited, the thermal stability of the diaphragm is further improved; the cellulose-based composite diaphragm has a large number of electrolyte-philic groups and a 3D mesh porous structure, which is more conducive to the infiltration of the electrolyte, can effectively inhibit electrochemical polarization, increase the number of active sites, and reduce Li + The diffusion distance can be shortened, thereby improving the electrochemical performance of the battery.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a cellulose-based composite membrane, the preparation method comprising the following steps:
[0010] (1) mixing an alkali metal hydroxide, a urea compound, deionized water, and cellulose uniformly in a freezing environment to obtain a first mixed solution;
[0011] (2) maintaining the freezing environment, mixing sodium alginate with the first mixed solution of step (1) to obtain a second mixed solution;
[0012] (3) The second mixed solution of step (2) is treated to obtain a sheet material, and then cured and regenerated to obtain a cellulose-based composite diaphragm.
[0013] The present invention utilizes a freezing environment, firstly completely dissolves and disperses cellulose in a solution containing urea compounds and alkaline hydroxides, cellulose forms hydrogen bonds with alkaline hydroxides, destroys the hydrogen bond structure inside the cellulose, and then dissolves the cellulose, and at the same time, the presence of the urea compounds enables the dispersed cellulose to continue to maintain a stable dispersed state, and then sodium alginate is added to the mixed solution containing cellulose, and under this low temperature environment and alkaline conditions, the solubility of sodium alginate is further promoted, and sodium alginate contains multiple hydroxyl groups, which form non-covalent crosslinks with cellulose molecules, thereby obtaining a gel-like product.
[0014] As a preferred technical solution of the present invention, the alkali metal hydroxide in step (1) includes sodium hydroxide.
[0015] Preferably, the urea compound in step (1) comprises urea or thiourea.
[0016] Preferably, based on the total mass of the alkali metal hydroxide, the urea compound and deionized water, the mass fraction of the alkali metal hydroxide is 5-10wt%, for example, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%.
[0017] Preferably, based on the total mass of the alkali metal hydroxide, the urea compound and deionized water, the mass fraction of the urea compound is 10-15wt%, for example, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%.
[0018] In the present invention, the mass fractions of the alkali metal hydroxide and the urea compound are adjusted to ensure that the cellulose is fully dissolved in the mixed solution.
[0019] Preferably, the mixing in step (1) includes stirring.
[0020] Preferably, the temperature of the freezing environment is -11 to -15°C, for example, -11.5°C, -12°C, -12.5°C, -13°C, -13.5°C, -14°C, -14.5°C or -15°C.
[0021] In the present invention, the temperature of the freezing environment is regulated and matched with the concentrations of the alkali metal hydroxide and the urea compound to ensure that the cellulose is fully dissolved in the mixed solution.
[0022] As a preferred technical solution of the present invention, based on the total mass of the alkali metal hydroxide, the urea compound and the deionized water, the amount of cellulose added in step (1) is 3-4wt%, for example, 3wt%, 3.1wt%, 3.2wt%, 3.3wt%, 3.4wt%, 3.5wt%, 3.6wt%, 3.7wt%, 3.8wt%, 3.9wt% or 4wt%, etc.
[0023] In the present invention, cellulose is added in small amounts for multiple times to avoid the phenomenon that part of the cellulose fails to dissolve due to direct addition of the entire cellulose.
[0024] Preferably, the mixing method in step (1) includes stirring.
[0025] Preferably, the stirring speed is 500-1000 rpm, for example, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm, 800 rpm, 850 rpm, 900 rpm, 950 rpm or 1000 rpm.
[0026] Preferably, the stirring time is 6 to 10 hours, for example 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.
[0027] As a preferred technical solution of the present invention, in the second mixed solution of step (2), the mass fraction of sodium alginate is 0.5-2wt%, for example, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2wt%, etc.
[0028] In the present invention, if the amount of sodium alginate added is too much, part of the sodium alginate will not dissolve in the solution and will easily agglomerate, which will have a greater impact on the liquid absorption rate and tensile strength of the diaphragm; if the amount of sodium alginate added is too little, the effect of improving the performance of the diaphragm cannot be achieved.
[0029] Preferably, the treatment in step (3) comprises: pouring the second mixed solution on the surface of the glass plate and drying it naturally to obtain a sheet material.
[0030] As a preferred technical solution of the present invention, the curing and regeneration in step (3) comprises: placing the sheet material in a polyvinyl alcohol solution for curing, and then placing it in an acid solution for regeneration.
[0031] As a preferred technical solution of the present invention, the mass concentration of the polyvinyl alcohol solution is 8-12wt%, for example, 8wt%, 9wt%, 10wt%, 11wt% or 12wt%.
[0032] Preferably, the curing time is 10 to 24 hours, for example, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours.
[0033] Preferably, the mass concentration of the acid solution is 1% to 5%, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%.
[0034] Preferably, the regeneration time is 0.5 to 2 h, such as 0.5 h, 1 h, 1.5 h or 2 h.
[0035] As a preferred technical solution of the present invention, after the solidification and regeneration in step (3), pre-freezing and drying are also included.
[0036] Preferably, the pre-freezing is performed in a liquid nitrogen environment.
[0037] Preferably, the pre-freezing time is 2 to 10 min, for example, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0038] Preferably, the drying comprises freeze-drying.
[0039] Preferably, the freeze-drying temperature is -40 to -80°C, for example, -40°C, -45°C, -50°C, -55°C, -60°C, -65°C, -70°C, -75°C or -80°C.
[0040] Preferably, the freeze-drying time is 24 to 48 h, for example, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, 38 h, 40 h, 42 h, 44 h, 46 h or 48 h.
[0041] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0042] (1) fully mixing and stirring an alkali metal hydroxide, a urea compound, deionized water, and cellulose in a freezing environment at -11 to -15°C for 6 to 10 hours to obtain a first mixed solution;
[0043] Wherein, based on the total mass of the alkali metal hydroxide, the urea compound and the deionized water, the mass fraction of the alkali metal hydroxide is 5-10wt%, the mass fraction of the urea compound is 10-15wt%, and the added amount of the cellulose is 3-4wt%; the alkali metal hydroxide includes sodium hydroxide;
[0044] (2) maintaining a freezing environment of -11 to -15°C, stirring the sodium alginate and the first mixed solution in step (1) at 500 to 1000 rpm for 6 to 10 hours to obtain a second mixed solution;
[0045] Wherein, in the second mixed solution, the mass fraction of sodium alginate is 0.5-2wt%;
[0046] (3) The second mixed solution of step (2) is poured onto the surface of a glass plate to obtain a sheet material, and the sheet material is placed in an 8-12 wt% polyvinyl alcohol solution for curing for 10-24 h, and then placed in a 1%-5% acid solution for regeneration for 0.5-2 h. After washing to neutrality, the sheet material is pre-frozen in liquid nitrogen for 2-10 min, and freeze-dried at -40 to -80°C for 24 to 48 h to obtain a cellulose-based composite diaphragm.
[0047] In a second aspect, the present invention further provides a cellulose-based composite diaphragm, wherein the cellulose-based composite diaphragm is prepared by the preparation method described in the first aspect.
[0048] As a preferred technical solution of the present invention, the cellulose-based composite membrane includes sodium alginate and cellulose.
[0049] Preferably, the cellulose-based composite separator has a thickness of 15 to 60 μm, for example, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm.
[0050] In a third aspect, the present invention further provides a lithium ion battery, wherein the lithium ion battery comprises the cellulose-based composite separator described in the second aspect.
[0051] Compared with the prior art, the present invention has at least the following beneficial effects:
[0052] 1) The present invention introduces sodium alginate into the cellulose solution. Sodium alginate has certain electrolyte affinity and can increase the absorption of electrolyte by the battery separator. Sodium alginate itself is rich in functional groups such as hydroxyl and carboxyl groups, which can significantly improve the ionic conductivity of the cellulose-based separator. Sodium alginate contains multiple hydroxyl groups, which can form non-covalent cross-links between cellulose molecules and then be cured to effectively enhance the mechanical properties of the separator. Sodium alginate is compounded with cellulose to further improve the thermal stability of the separator. It can also effectively inhibit electrochemical polarization, increase the number of active sites, and reduce Li + Diffusion distance, thereby improving battery electrochemical performance;
[0053] 2) The preparation method of the present invention is simple in process, low in cost and environmentally friendly, and provides a simple and effective strategy for preparing biodegradable and highly conductive membranes, and has great potential in replacing widely used commercial polypropylene membranes. DETAILED DESCRIPTION
[0054] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0055] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0056] Example 1
[0057] This embodiment provides a method for preparing a cellulose-based composite diaphragm, the preparation method comprising the following steps:
[0058] (1) 7 g of sodium hydroxide, 12 g of urea and 81 g of deionized water were fully mixed and stirred, placed in a -12.3°C environment, maintained at -12.3°C, 4 g of cellulose was added in small amounts several times, and rapidly stirred at a rate of 800 rpm for 8 hours to obtain a first mixed solution;
[0059] (2) maintaining the environment at -12.3°C, adding 1 g of sodium alginate to the first mixed solution, and rapidly stirring at a rate of 800 rpm for 8 h to obtain a second mixed solution;
[0060] (3) The second mixed solution of step (2) is cast on a glass plate to obtain a sheet material, and the thickness of the sheet is controlled by rolling with a glass rod. The sheet is placed in a 10wt% polyvinyl alcohol solution and immersed for 12 hours, then taken out and placed in a 2% HCl aqueous solution for 1 hour to regenerate to obtain a wet film, which is then washed with deionized water until neutral, pre-frozen with liquid nitrogen for 5 minutes, and then freeze-dried at -60°C for 48 hours to obtain a cellulose-based composite diaphragm.
[0061] Example 2
[0062] This embodiment provides a method for preparing a cellulose-based composite diaphragm, the preparation method comprising the following steps:
[0063] (1) 5 g of sodium hydroxide, 15 g of urea and 80 g of deionized water were fully mixed and stirred, placed in a -14.5°C environment, maintained at -14.5°C, 3 g of cellulose was added in small amounts several times, and rapidly stirred at a rate of 500 rpm for 8 hours to obtain a first mixed solution;
[0064] (2) maintaining the environment at -14.5°C, adding 2 g of sodium alginate to the first mixed solution, and rapidly stirring at a rate of 500 rpm for 6 h to obtain a second mixed solution;
[0065] (3) The second mixed solution of step (2) is cast on a glass plate to obtain a sheet material, and the thickness of the sheet is controlled by rolling with a glass rod. The sheet is placed in an 8wt% polyvinyl alcohol solution and immersed for 24 hours, then taken out and placed in a 5% HCl aqueous solution for 0.5 hours to regenerate to obtain a wet film, which is then washed with deionized water until neutral, pre-frozen with liquid nitrogen for 10 minutes, and then freeze-dried at -80°C for 24 hours to obtain a cellulose-based composite diaphragm.
[0066] Example 3
[0067] This embodiment provides a method for preparing a cellulose-based composite diaphragm, the preparation method comprising the following steps:
[0068] (1) 10 g of sodium hydroxide, 10 g of thiourea and 80 g of deionized water were fully mixed and stirred, placed in a -11°C environment, maintained at -11°C, 3.5 g of cellulose was added in small amounts several times, and rapidly stirred at a rate of 1000 rpm for 8 hours to obtain a first mixed solution;
[0069] (2) maintaining the environment at -11°C, adding 0.6 g of sodium alginate to the first mixed solution, and rapidly stirring at a rate of 1000 rpm for 10 h to obtain a second mixed solution;
[0070] (3) The second mixed solution of step (2) is cast on a glass plate to obtain a sheet material, and the thickness of the sheet is controlled by rolling with a glass rod. The sheet is placed in a 12wt% polyvinyl alcohol solution and immersed for 10 hours, then taken out and placed in a 1% HCl aqueous solution for 2 hours to regenerate to obtain a wet film, which is then washed with deionized water until neutral, pre-frozen with liquid nitrogen for 2 minutes, and then freeze-dried at -40°C for 48 hours to obtain a cellulose-based composite diaphragm.
[0071] Example 4
[0072] This embodiment provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (1), 2 g of sodium hydroxide is added, which is fully mixed and stirred with 12 g of urea and 86 g of deionized water. The rest of the preparation method is consistent with Example 1.
[0073] Example 5
[0074] This embodiment provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (1), the amount of sodium hydroxide added is 15 g, which is fully mixed and stirred with 12 g of urea and 73 g of deionized water. The rest of the preparation method is consistent with Example 1.
[0075] Example 6
[0076] This embodiment provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (2), the amount of sodium alginate added is 0.3 g, and the rest of the preparation method is consistent with Example 1.
[0077] Example 7
[0078] This embodiment provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (2), the amount of sodium alginate added is 2.75 g, and the rest of the preparation method is consistent with Example 1.
[0079] Example 8
[0080] This embodiment provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that an environment of -17°C is maintained during the entire preparation process. The rest of the preparation method is consistent with Example 1.
[0081] Example 9
[0082] This embodiment provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that an environment of -9°C is maintained during the entire preparation process. The rest of the preparation method is consistent with Example 1.
[0083] Comparative Example 1
[0084] This comparative example provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (2), sodium alginate is mixed with the first mixed solution in step (1) at room temperature, and the rest of the preparation method remains consistent with Example 1.
[0085] Comparative Example 2
[0086] This comparative example provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (2), sodium alginate is replaced by xanthan gum, and the rest of the preparation method is consistent with Example 1.
[0087] Comparative Example 3
[0088] This comparative example provides a method for preparing a cellulose-based composite diaphragm. The difference between the preparation method and Example 1 is that in step (1), sodium alginate is first mixed with an alkali metal hydroxide, a urea compound, and deionized water, and then cellulose is added in step (2). The rest of the preparation method remains consistent with Example 1.
[0089] Test Method
[0090] 1) Diaphragm performance test:
[0091] The following tests were performed on the cellulose-based composite membranes prepared in Examples 1 to 9 and Comparative Examples 1 to 3:
[0092] Tensile strength test: Cut the diaphragm into samples with a length of 10 cm and a width of 2 cm, and use a universal testing machine with a test speed of 100 mm / min and a tensile force of 1 KN;
[0093] Thermal stability test (heat shrinkage): Cut the diaphragm into samples with a size of 10 cm in length and 10 cm in width, heat them in an oven, test the temperature at 200°C, test the time for 1 hour, and calculate the heat shrinkage;
[0094] Wetting performance test (liquid absorption rate): soak the sample with mass m1 in EL-1 electrolyte, take it out after 30 minutes, wipe the electrolyte on the surface with non-woven cloth, weigh and record m2, then let it stand for another 5 minutes, weigh and record m3; then the liquid absorption rate L = (m2-m1) / m1×100%, the test results are shown in Table 1:
[0095] Table 1
[0096] project Tensile strength(MPa) Thermal shrinkage (%) Liquid absorption rate (%) Example 1 48.9 0.8 68.1 Example 2 46.5 1.0 60.5 Example 3 42.6 1.2 58.2 Example 4 35.2 1.5 50.5 Example 5 34.5 2.0 50.1 Example 6 25.5 6.5 30.5 Example 7 39.6 2.1 40.6 Example 8 30.9 4.2 31.5 Example 9 40.8 3.5 31.6 Comparative Example 1 20.8 6.7 15.5 Comparative Example 2 15.8 3.2 20.5 Comparative Example 3 37.4 2.5 45.5
[0097] 2) Diaphragm electrical performance test:
[0098] Using NMP as solvent, positive electrode active material (LFP): Super P (conductive carbon black): PVDF (polyvinylidene fluoride) = 96:2:2 are mixed evenly, coated on aluminum foil, and dried at 80°C to 100°C to obtain a positive electrode sheet;
[0099] Using deionized water as solvent, negative electrode active material (graphite): Super P: CMC (carboxymethyl cellulose): SBR (polystyrene butadiene copolymer) = 95.5:1:0.5:3 are mixed evenly, coated on copper foil, and dried at 80°C to 100°C to obtain a negative electrode sheet;
[0100] The cellulose-based composite diaphragm, positive electrode sheet, and negative electrode sheet prepared in the above Examples 1 to 9 and Comparative Examples 1 to 3 were assembled into a lithium-ion battery, the electrolyte was a 1.0 mol / L LiPF6 solution (the solvent was EC, DMC, and EMC in a volume ratio of 1:1:1), and the assembled battery was subjected to electrochemical testing, and the testing method was as follows:
[0101] (1) Cycling performance: tested on an electrochemical workstation battery test system at 25°C, with a current density of 0.2C, a charge and discharge voltage window of 2.5-3.65V, and 1000 cycles;
[0102] (2) Rate discharge performance: The test was conducted on an electrochemical workstation battery test system at 25°C. The current densities tested were 0.2C, 1C and 2C, and the charge and discharge voltage window was 2.5-3.65V. The test results are shown in Table 2:
[0103] Table 2
[0104]
[0105]
[0106] The test results show that:
[0107] (1) It can be seen from Examples 1 to 3 that the cellulose-based composite diaphragm prepared by the preparation method of the present application has a tensile strength of not less than 42.6 MPa, a thermal shrinkage rate of not more than 1.2%, and a liquid absorption rate of not less than 58.2%;
[0108] (2) It can be seen from Examples 1 and 4-5 that Example 4 is a case where the mass fraction of sodium hydroxide is relatively low. If it is relatively low, cellulose cannot be fully dissolved in the mixed solution. Example 5 is a case where the mass fraction of sodium hydroxide is relatively high. If it is relatively high, the internal particle structure of the cellulose material will be destroyed. Both high and low values will affect the thermal shrinkage rate of the diaphragm, thereby reducing the overall performance of the diaphragm and the electrochemical performance of the assembled battery.
[0109] (3) It can be seen from Examples 1 and 6-7 that Example 6 is a case where a small amount of sodium alginate is added. If it is too small, the effect of improving the performance of the diaphragm cannot be achieved. Example 7 is a case where a large amount of sodium alginate is added. If it is too large, some of the sodium alginate will not be dissolved in the solution and will easily agglomerate. Both a large amount and a small amount will reduce the overall performance of the diaphragm and the electrochemical performance of the assembled battery.
[0110] (4) It can be seen from Examples 1 and 8 to 9 that Example 8 is a case where the reaction environment temperature is relatively high, while Example 9 is a case where the reaction environment temperature is relatively low. Both relatively high and relatively low temperatures will affect the dissolution process of cellulose and sodium alginate, thereby reducing the overall performance of the diaphragm and the electrochemical performance of the assembled battery.
[0111] (5) It can be seen from Example 1 and Comparative Examples 1 to 3 that in Comparative Example 1, sodium alginate is added at room temperature, which reduces the solubility of sodium alginate and affects the overall performance of the diaphragm; in Comparative Example 2, sodium alginate is replaced by xanthan gum, and the xanthan gum itself has poor electrophilic performance, which will have a great impact on the liquid absorption rate of the diaphragm; in Comparative Example 3, the order of adding sodium alginate and cellulose is exchanged, which will cause cellulose to coat and agglomerate the surface of sodium alginate molecules, so that part of the active channels of the diaphragm material are occupied, which has a great impact on the overall performance of the diaphragm. The diaphragm-assembled batteries of Comparative Examples 1 to 3 will all cause the electrochemical performance of the battery to be significantly reduced.
[0112] In summary, the present invention introduces sodium alginate into a cellulose solution under a freezing environment, and then solidifies it through non-covalent cross-linking of multiple hydrogen bonds between molecules, thereby effectively enhancing the mechanical strength of the diaphragm; after sodium alginate and cellulose are composited, the thermal stability of the diaphragm is further improved; the cellulose-based composite diaphragm has a large number of electrolyte-philic groups and a 3D mesh porous structure, which is more conducive to the infiltration of the electrolyte, can effectively inhibit electrochemical polarization, increase the number of active sites, and reduce Li + The diffusion distance can be shortened, thereby improving the electrochemical performance of the battery.
[0113] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a cellulose-based composite diaphragm, characterized in that: The preparation method comprises the following steps: (1) mixing an alkali metal hydroxide, a urea compound, deionized water, and cellulose uniformly in a freezing environment to obtain a first mixed solution; (2) maintaining the freezing environment, mixing sodium alginate with the first mixed solution of step (1) to obtain a second mixed solution; (3) The second mixed solution of step (2) is treated to obtain a sheet material, and then cured and regenerated to obtain a cellulose-based composite diaphragm.
2. The preparation method according to claim 1, characterized in that: The alkali metal hydroxide in step (1) comprises sodium hydroxide; Preferably, the urea compound in step (1) comprises urea or thiourea; Preferably, based on the total mass of the alkali metal hydroxide, the urea compound and the deionized water, the mass fraction of the alkali metal hydroxide is 5 to 10 wt %; Preferably, based on the total mass of the alkali metal hydroxide, the urea compound and the deionized water, the mass fraction of the urea compound is 10-15wt%; Preferably, the temperature of the freezing environment is -11 to -15°C.
3. The preparation method according to claim 1 or 2, characterized in that: Based on the total mass of the alkali metal hydroxide, the urea compound and the deionized water, the amount of cellulose added in step (1) is 3-4 wt %; Preferably, the mixing method in step (1) includes stirring; Preferably, the stirring speed is 500-1000 rpm; Preferably, the stirring time is 6 to 12 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that In step (2) the mass fraction of the sodium alginate in the second mixed solution is 0.5-2 wt %.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The curing and regeneration in step (3) comprises: placing the sheet material in a polyvinyl alcohol solution for curing, and then placing it in an acid solution for regeneration.
6. The preparation method according to claim 5, characterized in that: The mass concentration of the polyvinyl alcohol solution is 8-12wt%; Preferably, the curing time is 10 to 48 hours; Preferably, the mass concentration of the acid solution is 1% to 5%; Preferably, the regeneration time is 0.5 to 3 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) fully mixing and stirring an alkali metal hydroxide, a urea compound, deionized water, and cellulose in a freezing environment at -11 to -15°C for 6 to 10 hours to obtain a first mixed solution at a temperature of -11 to -15°C; Wherein, based on the total mass of the alkali metal hydroxide, the urea compound and the deionized water, the mass fraction of the alkali metal hydroxide is 5-10wt%, the mass fraction of the urea compound is 10-15wt%, and the added amount of the cellulose is 3-4wt%; the alkali metal hydroxide includes sodium hydroxide; (2) maintaining a freezing environment of -11 to -15°C, stirring the sodium alginate and the first mixed solution in step (1) at 500 to 1000 rpm for 6 to 10 hours to obtain a second mixed solution; Wherein, in the second mixed solution, the mass fraction of sodium alginate is 0.5-2wt%; (3) The second mixed solution of step (2) is poured onto the surface of a glass plate to obtain a sheet material, and the sheet material is placed in an 8-12 wt% polyvinyl alcohol solution for curing for 10-24 h, and then placed in a 1%-5% acid solution for regeneration for 0.5-2 h. After washing to neutrality, the sheet material is pre-frozen in liquid nitrogen for 2-10 min, and freeze-dried at -40 to -80°C for 24 to 48 h to obtain a cellulose-based composite diaphragm.
8. A cellulose-based composite membrane, characterized in that: The cellulose-based composite diaphragm is prepared by the preparation method according to any one of claims 1 to 7.
9. The cellulose-based composite diaphragm according to claim 8, characterized in that: The cellulose-based composite membrane comprises sodium alginate and cellulose; Preferably, the cellulose-based composite separator has a thickness of 15 to 60 μm.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the cellulose-based composite separator according to claim 8 or 9.
Citation Information
Patent Citations
Cellulose and sodium alginate blend membrane and preparation method thereof
CN106496616A
High-temperature-resistant cellulose-based polyvinyl alcohol composite battery diaphragm and preparation method thereof
CN114665223A