Aluminum nitride filter and gallium nitride power amplifier integrated device and preparation method thereof

By integrating aluminum nitride filter and gallium nitride amplifier devices on a chip, using SiO2-SiO2 bonding technology and piezoelectric layer structure, the cost and loss problems caused by separate device production in the existing technology are solved, and the high cost and loss problems are achieved. More efficient and smaller volume RF front-end filters meet the performance and volume requirements of new RF front-end and wireless communication systems.

CN119030488APending Publication Date: 2024-11-26XIDIAN UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411108220.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing GaN high-electron mobility transistors and surface acoustic wave filters are usually made separately, resulting in high device production costs, large chip area, and large system losses, which cannot meet the performance and volume requirements of new RF front-end and wireless communication systems.

Method used

Using aluminum nitride filter and gallium nitride amplifier integrated device, the surface acoustic wave filter and gallium nitride high electron mobility transistor are combined with SiO2-SiO2 bonding technology. Integrate on one chip and achieve efficient integration of devices through technologies such as isolation structure and interdigit transducer.

Benefits of technology

The process is simplified, the production cost and chip area are reduced, energy efficiency is improved, the impact of temperature changes on frequency is reduced, and performance is achieved with higher frequency and wider bandwidth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119030488A_ABST
    Figure CN119030488A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum nitride filter and gallium nitride power amplifier integrated device and a preparation method thereof. The device comprises a substrate, an epitaxial layer and a transducer, a gallium nitride channel layer is arranged on the substrate, and the channel layer is composed of a first channel layer and a second channel layer which are isolated from each other; a buried oxide layer and an aluminum nitride piezoelectric layer are sequentially stacked on the first channel layer to form a first epitaxial layer, and the first epitaxial layer and the substrate form an aluminum nitride filter; a barrier layer is stacked on the second channel layer to form a second epitaxial layer, and the second epitaxial layer and the substrate form a gallium nitride power amplifier; the transducer is arranged on the first epitaxial layer; and a source electrode, a drain electrode and a gate electrode are arranged on the second epitaxial layer. According to the invention, the aluminum nitride filter and the gallium nitride power amplifier are bonded on one chip to simplify the process, so that the manufacturing cost is reduced, the area and energy loss of the chip can be reduced, and the buried oxide layer can be used as a temperature compensation layer to inhibit the expansion or contraction of the piezoelectric material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor devices and relates to a surface acoustic wave filter, and in particular to an aluminum nitride filter and a gallium nitride power amplifier integrated device and a preparation method thereof. Background Art

[0002] As we enter the era of high-speed communications, RF devices are increasingly used. Gallium nitride high electron mobility transistors are widely used in 5G mobile communication systems due to their high power, high efficiency and low cost. Surface acoustic wave filters have also become widely used RF filters due to their good selectivity, wide bandwidth, stable performance and high reliability, and are gradually being widely used in mobile communication systems. The operating frequency bands required for RF front-end filters are getting higher and higher, and they need to have the bandwidth requirements and quality factor (q value) performance of previous filters. Piezoelectric insulating base materials as substrates can better improve the quality factor, coupling coefficient and frequency temperature coefficient of the filter.

[0003] However, with the advancement of technology, new RF front-ends and wireless communication systems require better performance and smaller size. However, in current applications, GaN high electron mobility transistors and surface acoustic wave filters are usually manufactured separately and packaged as independent devices and integrated together. This makes the device manufacturing cost high, the chip area large, and the system loss large. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an aluminum nitride filter and a gallium nitride power amplifier integrated device and a preparation method thereof, so as to reduce the manufacturing cost, chip area and system loss. The structure of the substrate, buried oxide layer and piezoelectric layer is used to improve the performance of the filter such as the quality factor, coupling coefficient and frequency temperature coefficient.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] In a first aspect of the present invention, an aluminum nitride filter and a gallium nitride power amplifier integrated device is provided, comprising a substrate, an epitaxial layer and a transducer; the epitaxial layer is composed of a first epitaxial layer and a second epitaxial layer, and the transducer is composed of an input transducer and an output transducer;

[0007] A channel layer is arranged on the substrate, the channel layer is composed of a first channel layer and a second channel layer isolated from each other, and the material is gallium nitride; a buried oxide layer and a piezoelectric layer are stacked in sequence on the first channel layer to form the first epitaxial layer, the material of the piezoelectric layer is aluminum nitride, and the first epitaxial layer and the substrate constitute an aluminum nitride filter; a barrier layer is stacked on the second channel layer to form the second epitaxial layer, and the second epitaxial layer and the substrate constitute a gallium nitride power amplifier;

[0008] The input transducer and the output transducer are arranged on the first epitaxial layer; the source electrode, the drain electrode and the gate electrode are arranged on the second epitaxial layer.

[0009] In some embodiments of the present invention, the first channel layer and the second channel layer are isolated by an isolation structure, and the isolation structure can be a groove and a Si 3 N 4 Filling, etc.

[0010] In some embodiments of the present invention, the input transducer and the output transducer are both interdigital transducers, which are arranged on the piezoelectric layer along the direction from the first epitaxial layer to the second epitaxial layer.

[0011] In some embodiments of the present invention, the material of the IDT is any one of Ti / Al and Ti / Au.

[0012] In some embodiments of the present invention, the source electrode and the drain electrode are arranged on the second channel layer, respectively located on both sides of the barrier layer, and the gate electrode is arranged on the barrier layer; the material of the source electrode and the drain electrode is four-layer metal, or two-layer metal of Ti / Al, and the material of the gate electrode is two-layer metal of Ni / Au, or two-layer metal of Pt / Au.

[0013] In some embodiments of the present invention, the material of the barrier layer is aluminum gallium nitride.

[0014] In some embodiments of the present invention, the thickness of the channel layer is 1.7 μm to 2 μm, the thickness of the piezoelectric layer is 0.3 μm to 1.0 μm, the thickness of the barrier layer is 20 nm to 30 nm, and the thickness of the buried oxide layer is 0.2 μm to 0.6 μm.

[0015] In some embodiments of the present invention, a gallium nitride buffer layer is provided between the substrate and the channel layer.

[0016] In some embodiments of the present invention, the buried oxide layer is SiO 2 Bonding layer

[0017] A second aspect of the present invention provides an integrated circuit, comprising a wafer and the aluminum nitride filter and gallium nitride power amplifier integrated device described in the first aspect of the present invention, wherein the aluminum nitride filter and gallium nitride power amplifier integrated device are arranged on the wafer.

[0018] The third aspect of the present invention provides a preparation method for preparing the aluminum nitride filter and gallium nitride power amplifier integrated device according to the first aspect of the present invention, comprising the following steps:

[0019] Take a first substrate wafer, form an aluminum nitride film on its surface, and deposit silicon dioxide on the surface of the aluminum nitride film as a first bonding layer; take a second substrate wafer, form a gallium nitride film on its surface, and deposit silicon dioxide on the surface of the gallium nitride film as a second bonding layer;

[0020] Bonding the first bonding layer to the second bonding layer, grinding and thinning the first substrate wafer until the aluminum nitride film is exposed;

[0021] Dividing the aluminum nitride film into a first region and a second region, etching the first region until the gallium nitride film is exposed, the remaining aluminum nitride film is the piezoelectric layer, and the remaining first bonding layer and the second bonding layer constitute the buried oxide layer;

[0022] Dividing the portion of the gallium nitride film in the projection direction of the first region into two portions, and etching a portion close to the piezoelectric layer until the second substrate wafer is exposed, thereby forming two portions of the gallium nitride film isolated from each other, wherein the gallium nitride film in the projection direction of the second region is the first channel layer, and the other portion of the gallium nitride film is the second channel layer;

[0023] growing the barrier layer on the second channel layer;

[0024] Firstly forming a source electrode and a drain electrode on the second epitaxial layer, and then forming a gate electrode;

[0025] The input transducer and the output transducer are formed on the first epitaxial layer.

[0026] In some embodiments of the present invention, the aluminum nitride film is grown by magnetron sputtering, and the gallium nitride film and the barrier layer are grown by metal organic chemical vapor deposition.

[0027] In some embodiments of the present invention, the first bonding layer and the second bonding layer are grown by plasma enhanced chemical vapor deposition, and the first bonding layer and the second bonding layer may be bonded by direct bonding.

[0028] In some embodiments of the present invention, the source electrode, the drain electrode, the gate electrode, the input transducer and the output transducer are all deposited by electron beam evaporation.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. Through SiO 2 -SiO 2 The surface acoustic wave filter (SAW) and the gallium nitride high electron mobility transistor (GaN HEAMT) are integrated on a chip by bonding, which can simplify the process compared with the existing technology to reduce the production cost, and can also reduce the chip area and energy loss.

[0031] 2. Piezoelectric materials may expand or contract when the temperature changes, thus affecting the frequency. The bonding layer oxygen, i.e. the buried oxide layer, can be used as a temperature compensation layer to inhibit the expansion or contraction of the piezoelectric material, thereby reducing the temperature coefficient and the impact of temperature changes on the frequency. The Si substrate can well control the entire piezoelectric layer, and can obtain a higher equivalent wave propagation in the piezoelectric layer, reduce losses and improve the quality factor. And because of the low energy loss, the energy efficiency is high, so the device can achieve higher frequency and wider bandwidth. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a schematic diagram of the structure of an aluminum nitride filter and a gallium nitride power amplifier integrated device of the present invention.

[0033] Figure 2 It is a main flow chart of a method for preparing an aluminum nitride filter and a gallium nitride power amplifier integrated device of the present invention.

[0034] Figure 3 The present invention is a schematic flow chart of a method for preparing an aluminum nitride filter and a gallium nitride power amplifier integrated device. DETAILED DESCRIPTION

[0035] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0036] The present invention is an integrated chip, specifically an aluminum nitride filter and a gallium nitride power amplifier integrated device, such as Figure 1 As shown, it includes a substrate 1, an epitaxial layer and a transducer. The epitaxial layer is composed of a first epitaxial layer and a second epitaxial layer, and the transducer is composed of an input transducer 9 and an output transducer 10, which are arranged on the first epitaxial layer. A source electrode, a drain electrode and a gate electrode are arranged on the second epitaxial layer.

[0037] The channel layer 2 is located on the substrate 1, which may be a Si substrate. The material of the channel layer 2 is gallium nitride, and it is composed of a first channel layer and a second channel layer isolated from each other. The buried oxide layer 3 and the piezoelectric layer 5 are sequentially stacked on the first channel layer, and the first epitaxial layer is composed of the first channel layer, the buried oxide layer 3 and the piezoelectric layer 5, wherein the material of the piezoelectric layer is aluminum nitride. The barrier layer 4 is stacked on the second channel layer, and the second epitaxial layer is composed of the second channel layer and the barrier layer 4.

[0038] Thus, the first epitaxial layer and the substrate constitute an aluminum nitride filter; and the second epitaxial layer and the substrate constitute a gallium nitride power amplifier.

[0039] In the present invention, an isolation mechanism such as a groove can be used to achieve isolation between the first channel layer and the second channel layer, that is, the integration of the aluminum nitride filter and the gallium nitride power amplifier in the same chip is achieved.

[0040] In the present invention, both the input transducer 9 and the output transducer 10 are interdigital transducers, which are arranged on the piezoelectric layer 5 along the direction from the first epitaxial layer to the second epitaxial layer, wherein the material of the interdigital transducer can be Ti / Al or Ti / Au. That is, the interdigital transducer is made of Ti / Al stacking or Ti / Au stacking.

[0041] In the present invention, the source electrode 6 and the drain electrode 7 are arranged on the second channel layer and are respectively located on both sides of the barrier layer 4, and the gate electrode 8 is arranged on the barrier layer 4. The material of the source electrode 6 and the drain electrode 7 is Ti / Al / Ti / Au, or Ti / Al, and the material of the gate electrode 8 is Ni / Au, or Pt / Au.

[0042] In the present invention, the material of the barrier layer 4 is aluminum gallium nitride. The piezoelectric effect of the AlGaN / GaN heterojunction is strong, and the conduction band offset is large, so that a higher two-dimensional electron device concentration and output power can be obtained.

[0043] The present invention provides some typical size parameters, wherein the thickness of the channel layer 2 is about 1.7 μm, and a GaN buffer layer with a thickness of about 250 nm can be grown below the channel layer 2 to solve the lattice mismatch problem between the substrate and the epitaxial layer. The buried oxide layer 3 has a thickness of 0.2 μm to 0.6 μm and can be SiO 2 The bonding layer is used to bond the piezoelectric layer 5 and the channel layer 2, and can also be used as a temperature compensation layer to suppress the expansion or contraction of the piezoelectric material. The piezoelectric layer 5 is located directly above the buried oxide layer 3, and can be an aluminum nitride film with a thickness of 0.3μm to 1.0μm. The film has high chemical stability and good temperature stability and can work in high temperature environments. The barrier layer 4 is above the second channel layer and can be an AlGaN material layer with a thickness of about 20nm; the source electrode 6 and the drain electrode 7 are 22nm / 140nm / 55nm / 45nm Ti / Al / Ti / Au four-layer metal formed by deposition; the gate electrode 8 is a 50nm / 150nm Ni / Au double-layer metal formed by deposition; the input transducer 9 and the output transducer 10 are 20nm / 300nm Ti / Al double-layer metal formed by deposition.

[0044] By arranging the aluminum nitride filter and the gallium nitride power amplifier integrated device of the present invention on a wafer, an integrated circuit with high integration, low loss and low cost can be formed.

[0045] Reference Figure 2 and Figure 3 The method for manufacturing the integrated device of the present invention is explained through the main steps described in the following embodiment.

[0046] Step 1: growing an AlN thin film on a first substrate and growing a GaN thin film on a second substrate.

[0047] Two Si (111) substrate wafers with the same size and thickness of 500 μm were selected for surface cleaning and named as the first substrate wafer and the second substrate wafer. 2 SO 4 :H 2 O 2 :H 2 O(3:1:1) and HF:H 2 O (1:10) to remove oxides and contaminants on the silicon surface, then rinse with deionized water for 10 min and finally spin dry.

[0048] An aluminum nitride film is formed on the surface of the first substrate wafer. The specific implementation method may be: a 0.3 μm thick aluminum nitride film is grown by magnetron sputtering, and the sputtering gas is high-purity N 2 and Ar, the purity of the sputtered Al target was 99.999%. Before starting the sputtering growth, the Al target was pre-sputtered and cleaned for 10 minutes, and then the Si substrate surface was subjected to a short period of Ar + Ion bombardment, the chamber back pressure is 5×10 -7 Torr.

[0049] A gallium nitride film is formed on the surface of the second substrate wafer. The specific implementation method may be: metal organic chemical vapor deposition is used to grow a gallium nitride film with a thickness of 1.7 μm, the epitaxial temperature is 1100°C, the pressure is 100 Torr, and the carrier gas is H 2 , TMGa is the III source, NH 3 It is the source of the five ethnic groups.

[0050] Step 2: Growing SiO on the first substrate AlN film 2 , SiO is grown on the second substrate GaN film 2 .

[0051] Specifically, SiO is deposited on the surface of the AlN film. 2 As the first bonding layer, SiO is deposited on the surface of GaN film. 2 As the second bonding layer. For example, plasma enhanced chemical vapor deposition (PECVD) technology can be used to form SiH 4 and N 2 O is the reaction gas, and SiO is prepared at low temperature 2 film.

[0052] Step 3: SiO 2 Bonding forms a buried oxide layer.

[0053] Specifically, the first bonding layer and the second bonding layer are aligned and directly bonded to obtain a buried oxide layer, the thickness of the buried oxide layer is 0.4 μm, during bonding, the AlN film faces downward and the GaN film faces upward, and the bonding process adopts either surface activated bonding or hot pressing bonding.

[0054] In this step, SiO 2 -SiO 2 By bonding, the surface acoustic wave filter (SAW) and the gallium nitride high electron mobility transistor (GaN HEAMT) can be integrated on a single chip, which not only simplifies the process but also reduces the chip area and energy loss.

[0055] Furthermore, since the piezoelectric material may expand or contract when the temperature changes, thereby affecting the frequency, the bonding layer oxygen, i.e. the buried oxide layer, can serve as a temperature compensation layer to suppress the expansion or contraction of the piezoelectric material.

[0056] Step 4: Grinding and thinning the Si substrate.

[0057] The Si substrate connected to the AlN film, ie, the first substrate wafer, is ground and thinned until the AlN film is exposed.

[0058] Step 5: Dry etching of AlN film and buried oxide layer.

[0059] The aluminum nitride film is divided into a first region and a second region, and the two regions are connected and form a whole. For example, in this embodiment, the first region is the left region, and the second region is the right region. In the first region, the AlN film, the first bonding layer and the second bonding layer are dry-etched until the gallium nitride film is exposed. The remaining aluminum nitride film is the piezoelectric layer 5, and the remaining first bonding layer and the second bonding layer constitute the buried oxide layer 3; CF4 plasma and H 2 Etching: the etching equipment is reactive ion etching.

[0060] Step 6: Etching the isolation structure.

[0061] The part of the GaN film in the projection direction of the first region is divided into two parts, one of which is close to the piezoelectric layer 5 and the other is far from the piezoelectric layer 5. The GaN film is etched through the part close to the piezoelectric layer 5 until the second substrate wafer is exposed to form an isolation structure. The remaining GaN film in the other part is the second channel layer, and the GaN film in the projection direction of the second region is the first channel layer. The two parts of the GaN film are isolated from each other by the isolation structure. The etching can be carried out by using a low-damage Cl 2 / BCl 3 The etching process uses reactive ion etching (RIE) as the etching equipment, with an etching rate of 7.17 nm / s and an etching depth of 1.7 μm.

[0062] Step 7: Deposition and growth of AlGaN thin film.

[0063] In this step, a barrier layer 4 is grown on the second channel layer. Specifically, an Al2O3 layer is grown on the second channel layer on the right side of the isolation structure by metal organic chemical vapor deposition. 0.55 Ga 0.45 N barrier layer, thickness 20nm, epitaxial temperature 1150℃ pressure 76Torr, using TMGa, TMAl and NH 3 As the reaction source, the carrier gas is H 2 .

[0064] Step 8: Deposition of source and drain electrodes.

[0065] This step is mainly to make the source electrode 6 and the drain electrode 7. Specifically, four metal layers can be grown on the second channel layer by electron beam evaporation, which are Ti / Al / Ni / Au in sequence, and the corresponding film thicknesses are 22nm / 150nm / 55nm / 45nm respectively. Then, the N 2 Rapid annealing was performed in a 1000 sccm atmosphere for 30 seconds to form an ohmic contact through alloying. The AZ5214 reverse adhesive process was used in the metal stripping process.

[0066] Step 9: Deposit the gate electrode.

[0067] This step is mainly to make the gate electrode 8. Usually, a metal with a higher work function is selected as the gate electrode metal. In this embodiment, Ni / Au laminated metal is used. In this embodiment, Ni / Au double-layer metal is deposited on the barrier layer 4 using an electron beam evaporation device with a thickness of 50nm / 150nm. After the metal evaporation is completed, the sample is placed in N at 450°C. 2 Rapid annealing for 5 minutes in atmosphere is performed to form a gate electrode Schottky contact, and AZ5214 reverse glue process is used in the metal stripping process.

[0068] Step 10: Depositing the IDT.

[0069] This step mainly manufactures the input transducer 9 and the output transducer 10. In this embodiment, the interdigital transducer is used as the input transducer and the output transducer, and the metal Ti / Al is deposited on the piezoelectric layer 5 by electron beam evaporation equipment, with a thickness of 20nm / 300nm, the width of the interdigital width and the width of the interdigital gap are both 3μm, the aperture length of the interdigital electrode is 200μm, the electrode center distance is 8μm, and the number of electrode interdigit pairs is 100 pairs.

Claims

1. An aluminum nitride filter and gallium nitride power amplifier integrated device, characterized in that: It comprises a substrate, an epitaxial layer and a transducer; the epitaxial layer is composed of a first epitaxial layer and a second epitaxial layer, and the transducer is composed of an input transducer and an output transducer; A channel layer is arranged on the substrate, the channel layer is composed of a first channel layer and a second channel layer isolated from each other, and the material is gallium nitride; a buried oxide layer and a piezoelectric layer are stacked in sequence on the first channel layer to form the first epitaxial layer, the material of the piezoelectric layer is aluminum nitride, and the first epitaxial layer and the substrate constitute an aluminum nitride filter; a barrier layer is stacked on the second channel layer to form the second epitaxial layer, and the second epitaxial layer and the substrate constitute a gallium nitride power amplifier; The input transducer and the output transducer are arranged on the first epitaxial layer; the source electrode, the drain electrode and the gate electrode are arranged on the second epitaxial layer.

2. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 1, characterized in that: The first channel layer and the second channel layer are isolated by an isolation structure, and the isolation structure is a groove or Si3N4 filling.

3. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 1, characterized in that: The input transducer and the output transducer are both interdigital transducers, which are arranged on the piezoelectric layer along the direction from the first epitaxial layer to the second epitaxial layer.

4. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 3, characterized in that: The source electrode and the drain electrode are arranged on the second channel layer, respectively located on both sides of the barrier layer, and the gate electrode is arranged on the barrier layer.

5. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 1, characterized in that: The material of the barrier layer is aluminum gallium nitride.

6. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 1 or 5, characterized in that: The thickness of the channel layer is 1.7 μm to 2 μm, the thickness of the piezoelectric layer is 0.3 μm to 1.0 μm, the thickness of the barrier layer is 20 nm to 30 nm, and the thickness of the buried oxide layer is 0.2 μm to 0.6 μm.

7. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 1, characterized in that: The buried oxide layer is a SiO2 bonding layer.

8. An integrated circuit, characterized in that: It comprises a wafer and an aluminum nitride filter and a gallium nitride power amplifier integrated device as described in any one of claims 1 to 7, wherein the aluminum nitride filter and the gallium nitride power amplifier integrated device are arranged on the wafer.

9. The method for preparing the aluminum nitride filter and gallium nitride power amplifier integrated device according to any one of claims 1 to 7, characterized in that: Includes steps: Take a first substrate wafer, form an aluminum nitride film on its surface, and deposit silicon dioxide on the surface of the aluminum nitride film as a first bonding layer; take a second substrate wafer, form a gallium nitride film on its surface, and deposit silicon dioxide on the surface of the gallium nitride film as a second bonding layer; Bonding the first bonding layer to the second bonding layer, grinding and thinning the first substrate wafer until the aluminum nitride film is exposed; Dividing the aluminum nitride film into a first region and a second region, etching the first region until the gallium nitride film is exposed, the remaining aluminum nitride film is the piezoelectric layer, and the remaining first bonding layer and the second bonding layer constitute the buried oxide layer; Dividing the portion of the gallium nitride film in the projection direction of the first region into two portions, and etching a portion close to the piezoelectric layer until the second substrate wafer is exposed, thereby forming two portions of the gallium nitride film isolated from each other, wherein the gallium nitride film in the projection direction of the second region is the first channel layer, and the other portion of the gallium nitride film is the second channel layer; growing the barrier layer on the second channel layer; Firstly forming a source electrode and a drain electrode on the second epitaxial layer, and then forming a gate electrode; The input transducer and the output transducer are formed on the first epitaxial layer.

10. The aluminum nitride filter and gallium nitride power amplifier integrated device according to claim 1, characterized in that: The aluminum nitride film is grown by magnetron sputtering, and the gallium nitride film and the barrier layer are grown by metal organic chemical vapor deposition; the first bonding layer and the second bonding layer are grown by plasma enhanced chemical vapor deposition, and the first bonding layer is directly bonded to the second bonding layer.

Citation Information

Cited By

  • A gallium nitride SAW resonator with improved electromechanical coupling coefficient and a method of manufacturing the same

    CN122891015A