Electric heating film with composite conductive layer and preparation method thereof

By using a composite structure of a metal grid and a microcrystalline chalcogen compound conductive layer in the electric heating film, the problems of heating uniformity and durability are solved, lower energy consumption and higher light transmittance are achieved, and the electric heating film is extended service life.

CN119031520APending Publication Date: 2024-11-26SHENZHEN SHENGAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411316235.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing electrical heating films have shortcomings in heating uniformity, energy consumption and durability, especially in high temperature environments, which are prone to aging and deformation, affecting service life.

Method used

Using a composite conductive layer structure, including a metal grid conductive layer and a chalcogen compound conductive layer, the metal grid conductive layer is prepared by photolithography technology, and a microcrystalline chalcogen compound conductive layer is formed by microwave heating, and an antioxidant layer is added to improve stability. sex.

Benefits of technology

The heating uniformity, reduced energy consumption and improved durability of the electric heating film are achieved, which extends the service life and improves the reliability and light transmittance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031520A_ABST
    Figure CN119031520A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electric heating films, and discloses an electric heating film with a composite conductive layer and a preparation method of the electric heating film. The electric heating film with the composite conducting layer comprises a base material, and a metal grating conducting layer, a chalcogenide conducting layer and an electrode layer are sequentially overlaid on the base material. The chalcogenide conductive layer is formed of a microcrystalline chalcogenide. The electric heating film is stably improved in the aspects of heating uniformity, durability, structural stability, energy consumption and other properties under the cooperation of the metal grating conducting layer and the chalcogenide conducting layer, and the overall quality is more excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electric heating films, and in particular relates to an electric heating film with a composite conductive layer and a preparation method thereof. Background Art

[0002] The conductive layer of the electric heating film generates heat under the action of an external electric field, completing the process of converting electrical energy into thermal energy. Electric heating films are widely used in flexible electronic devices (such as flexible sensors, wearable devices), biomedical sensors (such as biological monitoring and diagnosis), optoelectronics (optical devices, photovoltaic devices), near-infrared fields (security, sensors, imaging system heating devices) and high-performance energy storage devices (such as supercapacitors and lithium-ion batteries), and have broad market prospects and commercial application potential.

[0003] However, based on the selection and manufacturing process of traditional electric heating film materials, the current electric heating film has many deficiencies in heating uniformity, energy consumption and infrared transmittance. Especially in terms of life, since the electric heating film will generate high temperature when working, long-term high temperature environment will accelerate the aging, deformation and even cracking of the material, thus affecting the service life.

[0004] With the advancement of science and technology, electric heating films are increasingly widely used. Electric heating films face certain challenges in durability, structural stability and energy consumption. Therefore, how to provide a high-quality electric heating film and its preparation method is an urgent problem to be solved by those skilled in the art. Summary of the invention

[0005] In order to solve the deficiencies of the prior art, the present invention provides an electric heating film with a composite conductive layer and a preparation method thereof, and improves the durability, structural stability and electrical conductivity of the electric heating film and improves the overall quality of the electric heating film through structural design of the electric heating film.

[0006] The technical effects to be achieved by the present invention are achieved through the following technical aspects:

[0007] In a first aspect, the present invention provides an electric heating film having a composite conductive layer, comprising

[0008] It comprises a substrate, on which a metal grid conductive layer, a chalcogen compound conductive layer and an electrode layer are sequentially stacked;

[0009] The chalcogenide conductive layer is formed of microcrystalline chalcogenide.

[0010] In some embodiments, the substrate is selected from any one of long-wave bandpass glass, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, polyimide, and polymethyl methacrylate.

[0011] In some embodiments, the metal grid conductive layer includes metal wires, the metal wires cross to form grid units, the grid units are regular hexagonal grooves, the inner diameter of the grid unit diagonal length is 200-400 μm, the grid unit depth is 0.3-2 μm, and the metal wire width is 2-8 μm, which is conducive to further ensuring the uniform distribution of current on the electric heating film and avoiding the common heating unevenness problem of traditional electric heating films; regular hexagonal metal grids usually have a smaller resistance value, so under the same heating effect, the electric heating film of the present invention has lower energy consumption and is more energy-saving and environmentally friendly; the metal grid conductive layer is designed in a regular hexagonal grid shape because it has a higher filling efficiency than other shapes. Under the same area, the hexagonal grid can cover the area more effectively while keeping the spacing between the lines relatively large, which helps to reduce the metal lines from blocking the light, thereby improving the light transmittance. The symmetry of the hexagonal grid also helps to evenly distribute the light, further reduce light scattering and loss, and improve the light transmission performance.

[0012] In some embodiments, an anti-oxidation layer is further disposed on the electrode layer, the material of the anti-oxidation layer includes at least one of silicon dioxide and silicon nitride, and the thickness of the anti-oxidation layer is 10 to 50 nm.

[0013] In a second aspect, the present invention further provides a method for preparing any of the above-mentioned electric heating films having a composite conductive layer, comprising the following steps:

[0014] S1. preparing a photoresist pattern compatible with the metal grid on the substrate, depositing the metal on the substrate having the photoresist pattern, etching to obtain a substrate covered with a metal grid conductive layer, and forming a first composite film;

[0015] S2. mixing a chalcogen compound source with thioacetamide or a chalcogen compound source with selenoacetamide to obtain a chalcogen compound mixed gel, coating the chalcogen compound mixed gel on the metal grid conductive layer to form a chalcogen compound thin film layer, obtaining a substrate having a chalcogen compound thin film layer, and forming a second composite film;

[0016] S3. The two composite films are sequentially dried and microwave heated to convert the chalcogen compound thin film layer into a chalcogen compound conductive layer to obtain a substrate having a chalcogen compound conductive layer to form a third composite film;

[0017] S4. Screen printing electrode slurry on the third composite film to form an electrode layer, thereby obtaining an electric heating film having a composite conductive layer.

[0018] Among them, chalcogenides refer to compounds containing chalcogen elements (sulfur, selenium, and tellurium), mainly including: Metal sulfides: such as zinc sulfide (ZnS), cadmium sulfide (CdS), lead sulfide (PbS), molybdenum disulfide (MoS2), etc. Metal selenides: such as zinc selenide (ZnSe), etc. Metal tellurides: such as cadmium telluride (CdTe), etc.), which can provide good conductivity for the electric heating film.

[0019] In some embodiments, in step S1, the metal deposition adopts magnetron sputtering technology, wherein the magnetron sputtering target source power is 100-200 W, the coating time is 10-30 min, the argon gas flow rate is 20-40 sccm, and the metal layer deposition thickness is about 0.3-2 μm.

[0020] In some embodiments, in step S2, preparing the chalcogen compound mixed gel comprises:

[0021] preparing a 0.01-0.1 mol / L chalcogen compound source solution and a 0.01-0.1 mol / L thioacetamide solution / selenoacetamide solution respectively;

[0022] Mixing the thioacetamide solution / selenoacetamide aqueous solution with the chalcogen compound source solution and stirring to obtain a chalcogen compound mixed solution;

[0023] The pH value of the chalcogen compound mixed solution is adjusted to 8-10, and the solution is allowed to stand to obtain a chalcogen compound mixed gel.

[0024] In some embodiments, in step S2, the thickness of the chalcogenide compound thin film layer formed by coating the mixed gel is 1-10 μm.

[0025] In some embodiments, in step S3, after the substrate B is dried, it is placed in a nitrogen atmosphere at 100-120° C. and simultaneously subjected to microwave heating, with a microwave power of 50 W to 300 W and a heating time of 5 to 30 min.

[0026] In some embodiments, it also includes:

[0027] S5. Prepare an anti-oxidation layer on the electrode layer using atomic layer deposition technology.

[0028] In the process of preparing the anti-oxidation layer, the temperature is 100-150° C., the plasma power is 2000-3000 W, the gas flow rate is 150-200 sccm, and the reaction time is 10-90 min.

[0029] In summary, the present invention has at least the following benefits:

[0030] 1. The electric heating film with a composite conductive layer provided by the present invention improves the overall quality of the electric heating film by superimposing a sulfide compound conductive layer on the metal grid layer. Among them, the metal grid helps to achieve uniform distribution of current on the electric heating film and achieve uniform heating. Sulfide compounds have good electrical conductivity, which can further improve the overall electrical conductivity and reduce energy consumption. They can also provide better chemical stability and protect the metal grid conductive layer from oxidation and corrosion, thereby further improving the durability of the electric heating film, so that the electric heating film can operate stably for a long time in harsh environments and extend its service life. In addition, the sulfide compound conductive layer enhances the adhesion between the metal grid conductive layer and the substrate, and improves the reliability and stability of the device. It should be noted that the metal grid has good bending resistance and can be used to manufacture flexible devices with flexible materials as the substrate. In addition, compared with the metal grid on the traditional electric heating film, the metal grid conductive layer prepared by this method is not prone to turning points or intersections between metal wires, so it has the effect of uniform heating and good light transmittance. At the same time, the diameter of the metal wire forming the grid on the traditional electric heating film is large, and the general diameter is on the order of 10 1 -10 2 micrometers, the diameter of the metal grid conductive layer provided by the present invention is on the order of 10 0 Micron, photolithography and etching preparation for uniform surface.

[0031] Combined with chalcogenides, the electric heating film conductor has better flexibility and is suitable for curved or bent devices. In the present application, the chalcogenide conductive layer is formed by microcrystalline chalcogenides. Compared with the crystal morphology, the grains in the microcrystalline structure are smaller and more evenly distributed, which helps to reduce the scattering and absorption of light and improve the transparency of the material. There are a large number of grain boundaries and defect sites in the microcrystalline structure, which can provide additional carriers, thereby promoting the free movement of electrons and further improving conductivity. With the cooperation of the metal grid conductive layer and the chalcogenide conductive layer, the electric heating film has been steadily improved in terms of heating uniformity, durability, structural stability, energy consumption and other properties, and the overall quality is more excellent.

[0032] 2. The present invention provides a method for preparing an electric heating film with a composite conductive layer, wherein the sulfide compound thin film layer can be transformed into a sulfide compound conductive layer by microwave heating, and the sulfide compound undergoes a morphological transformation during this process to form a microcrystalline sulfide compound. This method can stably form microcrystalline sulfide compounds under low temperature conditions. At the same time, compared with traditional high-temperature crystallization, the present application has no restrictions on the high temperature resistance of the substrate. At the same time, the method prepares an electric heating film having a metal grid conductive layer and a sulfide compound conductive layer, and the overall quality of the electric heating film is improved by the composite of two different conductive layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1The figure is a schematic flow chart of a method for preparing an electric heating film with a composite conductive layer according to the present invention.

[0034] Figure 2 It is a schematic structural diagram of the electric heating film with a composite conductive layer of the present invention.

[0035] Reference numerals:

[0036] 1 substrate, 2 metal grid conductive layer, 3 chalcogenide conductive layer, 4 electrode layer. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them.

[0038] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Embodiment 1:

[0040] The following is an electric heating film with a composite conductive layer prepared using polycarbonate as the substrate 1. It should be noted that the substrate 1 can also be any one of long-wave bandpass glass, polyethylene terephthalate, polyethylene naphthalate, polyimide, and polymethyl methacrylate. These materials can achieve visible light non-transmission, high near-infrared light transmission, and good high temperature resistance and insulation performance.

[0041] First, the substrate 1 is cleaned by ultrasonic cleaning with acetone, deionized water, and anhydrous ethanol for 15 minutes in sequence to remove dust, grease and other pollutants on the surface, and then dried in a vacuum drying oven at 120° C. for 20 minutes for standby use.

[0042] A barrier layer is plated on the surface of the cleaned substrate 1, and a thin layer of silane coupling agent (γ-methacryloxypropyltrimethoxysilane, ethanol solvent, 0.5% concentration, rotation speed 500rpm, 5s, 1000rpm, 3s) is applied by spin coating, and dried in a drying oven at 50°C for 1h. The silane coupling agent can react with the hydroxyl groups on the surface of the polyester film to form a chemical bond, thereby enhancing the adhesion between the primer material and the substrate 1; at the same time, it can improve the flatness of the surface of the substrate 1 and reduce the influence of surface defects and contaminants on the photolithography accuracy. This helps to improve the clarity and resolution of the photolithography pattern.

[0043] Use a coating machine to evenly coat a layer of photoresist on the barrier layer. Place substrate 1 on the central axis of the coating machine, fix substrate 1 with a vacuum suction plate, drop photoresist on the center of substrate 1, and use two gears for spin coating. The low gear is set to 600rpm / min, the spin coating time is 5 to 15s, and the high gear is set to 4000rpm / min, and the spin coating time is 10 to 20s. Photoresist is a light-sensitive material, and its properties will change after exposure.

[0044] After the photoresist is applied, a soft bake is performed to remove the solvent in the photoresist and enhance the adhesion between the photoresist and the substrate 1. The soft bake is performed on a vacuum hot plate, the temperature is set to 90°C, and the time is 30 to 60 seconds. After the soft bake is completed, the photoresist should remain soft, but not completely cured.

[0045] A mask plate matching the metal grid structure is placed on the substrate 1 coated with photoresist, and then aligned and exposed. The photoresist is exposed to an ultraviolet light source with an intensity of 10 mW / cm 2 The exposure time is 5 to 15 seconds, which causes the photosensitizer in the photoresist to undergo a chemical reaction, and the photoresist changes from an initial state to an excited state, ultimately generating an organic acid that reacts with the developer.

[0046] After exposure, the developer that matches the photoresist is used for development. The developer reacts with the photosensitive material in the photoresist, causing the unexposed photoresist to be dissolved and removed. The exposed area becomes less soluble due to the photochemical reaction, and thus remains in the development process. In this way, the pattern on the mask is accurately copied to the photoresist layer.

[0047] After development, hardening treatment is required, and deionized water is used to remove residual developer and other impurities, and to improve the mechanical strength and etching resistance of the photoresist. Hardening is carried out on a hot plate, set at 90°C, and the time is 15 to 30 minutes.

[0048] The substrate 1 with the photoresist pattern is placed in a vacuum coating device, and a metal material is deposited on the developed substrate 1 by physical vapor deposition to form a metal grid structure. The power of the magnetron sputtering target source is adjusted to 100-200W, the coating time is 10-30min, the argon gas flow rate is 20-40sccm, and the thickness of the metal layer deposition is about 0.5μm. Among them, the metal deposit can be a highly conductive or alloy material such as silver, copper, gold, aluminum and silver-copper alloy, so that the resistivity of the subsequently formed metal grid conductive layer 2 is extremely low. In this embodiment, the metal deposit is silver, and the metal grid conductive layer 2 is a silver grid conductive layer.

[0049] Hydrochloric acid is used as an etchant to etch the substrate 1. After etching, the pattern on the photoresist layer is accurately transferred to the substrate 1, and a fine metal grid conductive layer 2 is obtained.

[0050] After the etching is completed, the remaining photoresist is removed with a stripper, and the substrate 1 is cleaned and dried to preliminarily obtain the substrate 1 covered with the metal grid conductive layer 2 to form a first composite film.

[0051] Specifically, the metal grid conductive layer 2 includes metal wires formed by metal deposition, the metal wires cross to form a plurality of grid units, the grid units are regular hexagonal grooves, the inner diameter diagonal length of the grid units is 300 μm, the depth of the grid units is 1 μm, and the metal wire width is 5 μm.

[0052] The metal grid conductive layer 2 of the first composite film is subjected to necessary post-treatment, such as cleaning, drying, annealing, etc., to improve its conductivity and stability.

[0053] Zinc sulfide is used as the chalcogen compound in this embodiment. Specifically, zinc acetate (Zn(CH3COO)2) is dissolved in deionized water to form a zinc acetate aqueous solution with a concentration of 0.05 mol / L. Then, thioacetamide with a concentration of 0.05 mol / L is slowly added to the zinc acetate solution, and the solution is stirred to ensure sufficient mixing. In this embodiment, 200 mL of the zinc acetate aqueous solution and the thioacetamide aqueous solution are mixed in equal volumes. The chalcogen compound source is a reactant that can react with thioacetamide to obtain a chalcogen compound. In the present application, the chalcogen compound source is zinc acetate.

[0054] Use acid or alkali to adjust the pH value of the solution to an appropriate range, between 8 and 10.

[0055] The sol is left to age for 0.5 to 2 hours to promote the formation of gel.

[0056] The gel is converted into a thin film by a coating method, such as blade coating, spin coating, dip coating or spray coating, etc. The gel is uniformly coated on the metal grid conductive layer 2 with a coating thickness of 5 μm to form a chalcogen compound thin film layer, thereby obtaining a substrate 1 having a chalcogen compound thin film layer and forming a second composite film.

[0057] The second composite film is dried at 80°C to remove moisture. Then, it is heat treated in a nitrogen atmosphere at 100-120°C, and microwave-assisted to convert zinc sulfide into microcrystalline zinc sulfide at low temperature. Microwave energy can penetrate the chalcogen compound film layer and produce an in vivo heating effect. The microwave power is 50W-300W, and the heating time is 5-30 minutes, which promotes the conversion of the chalcogen compound film layer into the chalcogen compound conductive layer 3 to obtain the third composite film.

[0058] Silver paste was screen-printed on both sides of the third composite film and dried at 120° C. for 1 h to form an electrode layer 4, thereby preliminarily obtaining an electric heating film with a composite conductive layer.

[0059] The electric heating film formed with the electrode layer 4 is placed in an atomic layer deposition device, and silane and oxygen as precursors are introduced by alternating pulses to grow a silicon dioxide protective layer atomically layer by atomic layer on the surface of the conductive layer. During this period, the temperature is precisely controlled at 100-150°C, the plasma power is 2000-3000W, the gas flow rate is 150-200sccm, and the reaction time is 10-90min to form a uniform anti-oxidation layer with a thickness of 30nm. Finally, the electric heating film with a composite conductive layer of this embodiment is obtained.

[0060] Connect the wire to the part of the silk-screened silver paste electrode that is not covered by the anti-oxidation layer.

[0061] In this embodiment, the electric heating film of the composite conductive layer is composed of a substrate, and a metal grid conductive layer, a chalcogen compound conductive layer, an electrode layer and an anti-oxidation layer sequentially stacked on the substrate.

[0062] Example 2

[0063] Different from Example 1, only a metal grid conductive layer 2, a chalcogen compound conductive layer 3 and an electrode layer 4 are sequentially prepared on a substrate 1, and no anti-oxidation layer is prepared. Among them, the metal grid conductive layer 2 is a silver grid conductive layer, the chalcogen compound used in the chalcogen compound conductive layer 3 is zinc sulfide, and the electrode layer 4 is prepared and formed by silver paste.

[0064] Example 3

[0065] Different from Example 1, this embodiment uses cadmium sulfide as the chalcogen compound in this embodiment, and cadmium acetate (Cd(CH3COO)2) is dissolved in deionized water to form a cadmium acetate aqueous solution with a concentration of 0.05 mol / L. Then, thioacetamide with a concentration of 0.05 mol / L is slowly added to the cadmium acetate solution, and the solution is stirred to ensure sufficient mixing. In this embodiment, 200 mL of each cadmium acetate aqueous solution and thioacetamide aqueous solution are mixed in equal volumes.

[0066] Example 4

[0067] Different from Example 1, this embodiment uses zinc selenide as the chalcogen compound in this embodiment, and zinc acetate (Zn(CH3COO)2) is dissolved in deionized water to form a zinc acetate aqueous solution with a concentration of 0.05 mol / L. Then, selenoacetamide with a concentration of 0.05 mol / L is slowly added to the zinc acetate solution, and the solution is stirred to ensure sufficient mixing. In this embodiment, 200 mL of the zinc acetate aqueous solution and the selenoacetamide aqueous solution are mixed in equal volumes.

[0068] Example 5

[0069] Different from Example 1, this embodiment uses molybdenum disulfide as the chalcogen compound in this embodiment, and dissolves molybdenum acetate (MoO2(CH3COO)2) in deionized water to form a molybdenum acetate aqueous solution with a concentration of 0.05 mol / L. Then, thioacetamide with a concentration of 0.05 mol / L is slowly added to the molybdenum acetate solution, and the solution is stirred to ensure sufficient mixing. In this embodiment, 200 mL of the molybdenum acetate aqueous solution and 400 mL of the thioacetamide aqueous solution are mixed.

[0070] Example 6

[0071] Different from the third embodiment, in this embodiment, when the substrate 1 with the photoresist pattern is placed in the vacuum coating equipment for physical vapor deposition, the metal deposit used is copper.

[0072] Example 7

[0073] Different from the fourth embodiment, in this embodiment, when the substrate 1 with the photoresist pattern is placed in the vacuum coating equipment for physical vapor deposition, the metal deposit used is copper.

[0074] Example 8

[0075] Different from the fifth embodiment, in this embodiment, when the substrate 1 with the photoresist pattern is placed in the vacuum coating equipment for physical vapor deposition, the metal deposit used is copper.

[0076] Example 9

[0077] Different from Example 1, in this embodiment, the deposition thickness of the metal when depositing to form the metal grid is 2 μm, the formed grid unit is a regular hexagonal groove, the diagonal length of the inner diameter of the grid unit is 200 μm, the depth of the grid unit is 2 μm, and the metal line width is 8 μm. In addition, the thickness of the chalcogenide conductive layer 3 in this embodiment is 10 μm, and the thickness of the anti-oxidation layer is 50 nm.

[0078] It should be noted that, in the process of preparing the chalcogen compound mixed gel, this embodiment uses a zinc acetate aqueous solution with a concentration of 0.1 mol / L and a thioacetamide aqueous solution with a concentration of 0.1 mol / L.

[0079] Example 10

[0080] Different from Example 1, in this embodiment, the deposition thickness of the metal when depositing to form the metal grid is 0.3 μm, the formed grid unit is a regular hexagonal groove, the inner diameter diagonal length of the grid unit is 400 μm, the grid unit depth is 0.3 μm, and the metal line width is 2 μm. In addition, the thickness of the chalcogenide conductive layer 3 in this embodiment is 1 μm, and the thickness of the anti-oxidation layer is 10 nm.

[0081] It should be noted that, in the process of preparing the chalcogen compound mixed gel, this embodiment uses a zinc acetate aqueous solution with a concentration of 0.01 mol / L and a thioacetamide aqueous solution with a concentration of 0.01 mol / L.

[0082] Comparative Example 1

[0083] Different from Example 1, only a metal grid conductive layer 2 and an electrode layer 4 are sequentially prepared on a substrate 1, and no chalcogen compound conductive layer 3 and an anti-oxidation layer are prepared. The metal grid conductive layer 2 is a silver grid conductive layer, and the electrode layer 4 is prepared and formed by silver paste.

[0084] Comparative Example 2

[0085] Different from the first embodiment, the grid unit formed by the metal grid conductive layer 2 of the present embodiment is a rectangle, and the diagonal length of the rectangle is consistent with the diagonal length of the regular hexagon, which is 200-400 μm.

[0086] Comparative Example 3

[0087] Different from the first embodiment, the grid unit formed by the metal grid conductive layer 2 of the present embodiment is a triangle, and the side length of the triangle is 200-400 μm.

[0088] Comparative Example 4

[0089] This embodiment uses a conventional electric heating wire heating film.

[0090] Comparative Example 5

[0091] Different from Example 1, the chalcogen compound conductive layer is prepared by conventional methods in this example, and the chalcogen compound in the chalcogen compound conductive layer in this example is non-microcrystalline zinc sulfide.

[0092] The electric heating films obtained in Example 1, Example 2 and Comparative Examples 1-4 were taken to prepare samples, and the in-plane square resistance, light transmittance, time required for setting temperature, maximum temperature difference in the heating surface and reliability test were tested and the test results were recorded:

[0093] Square resistance test: Turn on the four-probe square resistance tester and preheat it for 15 minutes, select the square resistance test mode, and place the film to be tested flat on the test platform of the tester with the surface facing up. Use the four-probe probe to press on the conductive film, and make sure that the four probe heads are in good contact with the film. Be careful to keep the distance from the edge of the probe to the edge of the material greater than the probe spacing (generally more than 10 times). Read the value and record the data.

[0094] Transmittance test: Turn on the spectrophotometer, preheat the device for 15 minutes, calibrate the device, set the measurement wavelength range to 750-1100nm, start measuring, read the data, and record the transmittance value at a wavelength of 950nm.

[0095] Temperature measurement: apply a certain DC voltage to the heating film, use an infrared thermal imager to test the heating temperature of the heating film, record the time when the preset temperature of 70°C is reached, and measure the maximum temperature difference percentage within the heating surface (maximum temperature difference percentage within the surface = (highest temperature within the surface - lowest temperature within the surface) / set temperature);

[0096] Reliability test:

[0097] The electric heating film is placed under 340nm ultraviolet rays for aging, and the UV aging resistance time of the electric heating film is measured when the light transmittance decreases by no more than 5% of the original light transmittance, the resistance value changes by no more than 2 times of the initial value, and there is no obvious physical damage such as discoloration, blistering, cracks, etc. on the surface of the film;

[0098] The electric heating film is subjected to a high and low temperature cycle test, with a test temperature range of -40℃~85℃ (the high and low temperature ranges are set from -40℃ to +85℃, -40℃ is maintained for 0.5h, and 85℃ is maintained for 0.5h), and one cycle is recorded as 1h. The test electric heating film has no significant changes in heating rate and uniformity, and the temperature rise time does not change by more than 2 times the initial value compared with the initial test value. The resistance value does not change by more than 2 times the initial value, and there is no obvious warping, delamination, blistering, etc. The time it can be maintained;

[0099] Expose the electric heating film at 85°C and 85% RH, and measure the resistance value of the electric heating film to be no more than twice the initial value, and the transmittance decreases by no more than 5% of the original transmittance, and the high temperature and high humidity resistance time without blistering, peeling, or discoloration;

[0100] The minimum time that meets the above test requirements is recorded as the reliability test time.

[0101] The test results are shown in Table 1.

[0102] Table 1. Test results of different performance parameters of various embodiments

[0103]

[0104]

[0105] After the chalcogen compound conductive layer 3 is superimposed on the metal grid conductive layer, it basically does not affect the light transmittance of the electric heating film, and at the same time improves the conductivity and conductivity uniformity of the electric heating film. Under the same heating voltage, the heating temperature can be reached faster and the temperature difference of the whole surface heating is smaller. In addition, the superposition of the chalcogen compound conductive layer 3 and the metal grid conductive layer also significantly improves the reliability of the electric heating film. On this basis, adding an anti-oxidation layer can further improve the reliability of the heating film. The heating performance and light transmittance of the heating film tested for 1000h are intact.

[0106] The above contents are merely examples and illustrations of the structure of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these obvious replacement forms all belong to the protection scope of the present invention.

Claims

1. An electric heating film having a composite conductive layer, characterized in that: It comprises a substrate, on which a metal grid conductive layer, a chalcogen compound conductive layer and an electrode layer are sequentially stacked; The chalcogenide conductive layer is formed of microcrystalline chalcogenide.

2. The electric heating film with a composite conductive layer according to claim 1, characterized in that: The substrate is selected from any one of long-wave bandpass glass, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, polyimide, and polymethyl methacrylate.

3. The electric heating film with a composite conductive layer according to claim 1, characterized in that: The metal grid conductive layer includes metal wires, which are crossed to form grid units. The grid units are regular hexagonal grooves. The inner diameter diagonal length of the grid units is 200-400 μm, the depth of the grid units is 0.3-2 μm, and the width of the metal wires is 2-8 μm.

4. The electric heating film with a composite conductive layer according to claim 1, characterized in that: An anti-oxidation layer is also provided on the electrode layer. The material of the anti-oxidation layer includes at least one of silicon dioxide and silicon nitride. The thickness of the anti-oxidation layer is 10-50 nm.

5. A method for preparing an electric heating film with a composite conductive layer according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. preparing a photoresist pattern compatible with the metal grid on the substrate, depositing the metal on the substrate having the photoresist pattern, etching to obtain a substrate covered with a metal grid conductive layer, and forming a first composite film; S2. Mixing a chalcogen compound source with thioacetamide or a chalcogen compound source with selenoacetamide to obtain a chalcogen compound mixed gel, coating the chalcogen compound mixed gel on the metal grid conductive layer to form a chalcogen compound thin film layer, obtaining a substrate having a chalcogen compound thin film layer, and forming a second composite film; S3. The second composite film is sequentially dried and microwave heated to convert the chalcogen compound thin film layer into a chalcogen compound conductive layer to obtain a substrate having a chalcogen compound conductive layer to form a third composite film; S4. Screen printing electrode slurry on the third composite film to form an electrode layer, thereby obtaining an electric heating film having a composite conductive layer.

6. The method for preparing an electric heating film with a composite conductive layer according to claim 5, characterized in that: In step S1, the metal deposition adopts magnetron sputtering technology, wherein the magnetron sputtering target source power is 100-200W, the coating time is 10-30min, the argon gas flow rate is 20-40sccm, and the metal layer deposition thickness is about 0.3-2μm.

7. The method for preparing an electric heating film with a composite conductive layer according to claim 5, characterized in that: In step S2, preparing the chalcogen compound mixed gel comprises: preparing a 0.01-0.1 mol / L chalcogen compound source solution and a 0.01-0.1 mol / L thioacetamide solution / selenoacetamide solution respectively; The thioacetamide solution / selenoacetamide solution is mixed with the chalcogen compound source solution, and stirred to obtain a chalcogen compound mixed solution; The pH value of the chalcogen compound mixed solution is adjusted to 8-10, and the solution is allowed to stand to obtain a chalcogen compound mixed gel.

8. The method for preparing an electric heating film with a composite conductive layer according to claim 5, characterized in that: In step S2, the thickness of the chalcogen compound thin film layer formed by coating the chalcogen compound mixed gel is 1-10 μm.

9. The method for preparing an electric heating film with a composite conductive layer according to claim 5, characterized in that: In step S3, after the substrate B is dried, it is placed in a nitrogen atmosphere at 100-120°C and simultaneously subjected to microwave heating, with a microwave power of 50W-300W and a heating time of 5-30min.

10. The method for preparing an electric heating film with a composite conductive layer according to claim 5, characterized in that: Also includes: S5. Prepare an anti-oxidation layer on the electrode layer using atomic layer deposition technology. In the process of preparing the anti-oxidation layer, the temperature is 100-150° C., the plasma power is 2000-3000 W, the gas flow rate is 150-200 sccm, and the reaction time is 10-90 min.