Flexible electromagnetic shielding film and preparation method and application thereof

By combining a multi-layer structure of two-dimensional film and cellulose film in electromagnetic shielding materials, the shortcomings of traditional electromagnetic shielding materials in lightweight and flexible applications are solved, and efficient electromagnetic shielding effect and material flexibility are achieved.

CN119031684APending Publication Date: 2024-11-26SHENZHEN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411092972.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Due to the shortcomings of high density, poor flexibility, and difficult processing, traditional electromagnetic shielding materials have limited their use in applications that require lightweight and flexible, especially in the context of increasingly prominent electromagnetic interference problems in the development of electronic equipment and communication technology. .

Method used

Using a multi-layer structure flexible electromagnetic shielding film including a two-dimensional film layer, a first cellulose film layer and a second cellulose film layer arranged on both sides of the two-dimensional film layer, the combination of the cellulose film is carried out by electrochemical peeling treatment and a combination of the cellulose film. , form an efficient electromagnetic shielding material.

Benefits of technology

It achieves the improvement of the flexibility and lightweight of the material while ensuring excellent electromagnetic shielding performance. The electromagnetic shielding efficiency reaches a commercial level of more than 20dB. The preparation method is simple, the operation controllability is strong, and the processing cost is low, which is suitable for large-scale manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031684A_ABST
    Figure CN119031684A_ABST
Patent Text Reader

Abstract

The invention discloses a flexible electromagnetic shielding film and a preparation method and application thereof. The flexible electromagnetic shielding film comprises a two-dimensional film layer, a first cellulose film layer and a second cellulose film layer, wherein the first cellulose film layer and the second cellulose film layer are arranged on the two sides of the two-dimensional film layer respectively. The flexible electromagnetic shielding film is obtained by adopting an alternating vacuum filtration method for crystal powder subjected to electrochemical stripping and bacterial cellulose dispersion liquid. The flexible electromagnetic shielding film is composed of multiple layers of materials, the electromagnetic shielding effectiveness of the flexible electromagnetic shielding film is remarkably improved compared with that of an untreated film and reaches the level of a commercial electromagnetic shielding film of 20 dB or above, the preparation method is simple and effective, operation controllability is high, the processing cost is low, and large-scale manufacturing can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electromagnetic shielding composite materials, and in particular to a flexible electromagnetic shielding film and a preparation method and application thereof. Background Art

[0002] With the rapid development of electronic equipment and communication technology, electromagnetic interference (EMI) has become increasingly prominent, affecting the normal operation of electronic equipment and may have adverse effects on human health. Traditional electromagnetic shielding materials are mainly copper, aluminum and other metals. Although they have good shielding effects, these materials have disadvantages such as high density, poor flexibility and difficult processing, which limits their use in certain applications, especially in situations that require lightness and flexibility.

[0003] The emergence of two-dimensional materials has provided a new direction for the research of electromagnetic shielding materials. Two-dimensional materials have a series of significant advantages, making them an ideal choice for new electromagnetic shielding materials. First, two-dimensional materials have ultra-high conductivity, which enables them to effectively reflect and absorb electromagnetic waves and provide efficient electromagnetic shielding effects. Secondly, two-dimensional materials are extremely thin, only a few atomic layers, but have high strength and high toughness, which enables them to be lightweight and flexible while maintaining high shielding effectiveness. This flexibility allows two-dimensional materials to easily adapt to surfaces of various complex shapes, thereby showing excellent adaptability in different applications.

[0004] In addition, two-dimensional materials have excellent thermal conductivity, which can effectively disperse heat and prevent local overheating, thereby improving the reliability and stability of electronic devices. Their high specific surface area also helps to enhance the interaction between the material and the matrix and improve the overall performance of the composite material. Compared with traditional metal materials, two-dimensional materials not only have significant advantages in performance, but also excel in environmental friendliness and sustainability because they can be synthesized through relatively environmentally friendly methods and have good renewability.

[0005] In summary, two-dimensional materials, with their ultra-high conductivity, excellent flexibility, high strength, light weight and good thermal conductivity, overcome many shortcomings of traditional metal materials and become an ideal choice for the development of high-performance, lightweight and flexible electromagnetic shielding materials. Summary of the invention

[0006] The main purpose of the present invention is to propose a flexible electromagnetic shielding film and a preparation method and application thereof, aiming to solve the problem of application of transition metal disulfide compound two-dimensional material films in electromagnetic shielding in the prior art.

[0007] To achieve the above object, the present invention provides a flexible electromagnetic shielding film, comprising a two-dimensional film layer and a first cellulose film layer and a second cellulose film layer respectively arranged on both sides of the two-dimensional film layer.

[0008] Optionally, the material of the two-dimensional thin film layer includes at least one of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2; and / or,

[0009] The material of the first cellulose film layer and the second cellulose film layer includes at least one of bacterial cellulose and cellulose nanofiber.

[0010] Optionally, the thickness of the two-dimensional thin film layer is 60-80 μm; and / or,

[0011] The thickness of the first cellulose film layer and the second cellulose film layer is 10-20 μm; and / or,

[0012] The thickness of the flexible electromagnetic shielding film is 90-100 μm.

[0013] Optionally, the mass ratio of the total mass of the first cellulose film layer and the second cellulose film layer to the two-dimensional film layer is (0.6-0.8):(0.11-0.35); preferably, the mass ratio of the total mass of the first cellulose film layer and the second cellulose film layer to the two-dimensional film layer is (0.6-0.8):0.24.

[0014] The present invention also provides a method for preparing the flexible electromagnetic shielding film, comprising the following steps:

[0015] S1, obtaining a first cellulose film layer;

[0016] S2, performing electrochemical stripping treatment on the two-dimensional material to obtain a dispersion containing the two-dimensional thin film material;

[0017] S3, covering the surface of the first cellulose film layer with the dispersion liquid and filtering it to obtain a two-dimensional film layer formed on the surface of the first cellulose film layer;

[0018] S4. Covering the surface of the two-dimensional film layer with a second cellulose film layer to obtain the flexible electromagnetic shielding film.

[0019] Optionally, step S1 comprises: filtering the cellulose dispersion to obtain a first cellulose film; wherein the concentration of the cellulose dispersion is 8-12 mg / mL.

[0020] Optionally, step S2 includes:

[0021] The crystal powder is pressed into tablets to obtain a two-dimensional material;

[0022] Using the two-dimensional material as a working electrode, performing electrochemical stripping treatment on the two-dimensional material to obtain a dispersion containing the two-dimensional thin film material;

[0023] The dispersion containing the two-dimensional thin film material is washed, filtered and dried.

[0024] Wherein, during the electrochemical stripping process, the voltage is +4.0 to 8.0 V; and / or,

[0025] The electrochemical stripping treatment time is 10-60 minutes; and / or,

[0026] The washing reagent includes dimethylformamide;

[0027] The electrochemical stripping solution used in the electrochemical stripping treatment includes a solute and a solvent;

[0028] The solute includes tetrabutylammonium tetrafluoroborate;

[0029] The solvent includes at least one of propylene carbonate and dimethyl sulfoxide;

[0030] Preferably, the electrochemical stripping solution comprises tetrabutylammonium tetrafluoroborate and propylene carbonate; the concentration of tetrabutylammonium tetrafluoroborate in the electrochemical stripping solution is 0.03-0.075 mol / L; more preferably, the concentration of tetrabutylammonium tetrafluoroborate is 0.05 mol / L.

[0031] Optionally, the specific steps of step S4 are: covering the surface of the two-dimensional film layer with a bacterial cellulose dispersion, and filtering to obtain the flexible electromagnetic shielding film;

[0032] The pore size of the filter membrane used for filtration is 0.20-0.3 μm; preferably, the pore size of the filter membrane is 0.22 μm.

[0033] The present invention also provides application of the flexible electromagnetic shielding film in electronic products, medical equipment, military fields, and household electrical appliances. The flexible electromagnetic shielding film is used for shielding electromagnetic interference.

[0034] The present invention proposes a flexible electromagnetic shielding film and a preparation method and application thereof. The flexible electromagnetic shielding film includes a two-dimensional film layer and a first cellulose film layer and a second cellulose film layer respectively arranged on both sides of the two-dimensional film layer. The flexible electromagnetic shielding film is composed of multiple layers of materials. By optimizing the combination and arrangement of each layer of materials, the flexibility and lightness of the material can be significantly improved while ensuring excellent electromagnetic shielding performance. The electromagnetic shielding efficiency is significantly improved compared with the film that has not been stripped, and both reach the level of commercial electromagnetic shielding films of more than 20dB. The preparation method is simple and effective, the operation is highly controllable, the processing cost is low, and it can be manufactured on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0036] Figure 1 (a) is a physical size diagram of the NbSe2 flexible electromagnetic shielding film provided in Example 1 of the present invention; Figure 1 (b) is a folded view of the NbSe2 flexible electromagnetic shielding film provided in Example 1 of the present invention; Figure 1 (c) is Figure 1 (b) Folding diagram of NbSe2 flexible electromagnetic shielding film;

[0037] Figure 2 A comparison chart of electromagnetic shielding performance between the NbSe2 flexible electromagnetic shielding film provided in Example 1 of the present invention and the film provided in Comparative Example 1 which has not been subjected to electrochemical stripping;

[0038] Figure 3 A comparison chart of electromagnetic shielding performance between the TiSe2 flexible electromagnetic shielding film provided in Example 2 of the present invention and the film provided in Comparative Example 2 without electrochemical stripping;

[0039] Figure 4 This is a comparison chart of the electromagnetic shielding performance of the MoTe2 flexible electromagnetic shielding film provided in Example 3 of the present invention and the film provided in Comparative Example 3 that has not been subjected to electrochemical stripping.

[0040] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0041] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.

[0042] With the rapid development of electronic equipment and communication technology, the problem of electromagnetic interference (EMI) has become increasingly prominent. Electromagnetic interference not only affects the normal operation of electronic equipment, but may also have adverse effects on human health. Traditional electromagnetic shielding materials are mainly metal materials, such as copper and aluminum. Although these metal materials have good shielding effects, they have disadvantages such as high density, poor flexibility, and difficulty in processing, which limits their use in certain applications.

[0043] In the present invention, the flexible electromagnetic shielding film includes a two-dimensional film layer and a first cellulose film layer and a second cellulose film layer respectively arranged on both sides of the two-dimensional film layer. In the technical solution of the present invention, the two-dimensional film layer can respond to changes in the external electromagnetic field more quickly because it has a higher carrier mobility and a higher permittivity. When electromagnetic waves penetrate the material, the carriers can quickly move to the surface of the film material to form currents, which will generate a magnetic field opposite to the incident electromagnetic wave, thereby offsetting or weakening the magnetic field component of the incident wave. The cellulose film has good processing performance and can be easily combined with other electronic components or materials. The design of the multilayer structure helps to form a more effective electromagnetic shielding layer, and the electromagnetic wave will be partially reflected and transmitted at each interface. These multiple reflected and transmitted electromagnetic waves interfere with each other, enhance the absorption and reflection of the electromagnetic wave, and thus improve the shielding effectiveness. In addition, the two-dimensional film layer and the cellulose film layer have different absorption capacities for electromagnetic waves. The multilayer structure can use these differences to make the electromagnetic wave partially absorbed and attenuated when passing through each layer, reducing the electromagnetic energy that finally penetrates.

[0044] The material of the two-dimensional thin film layer includes at least one of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2; and / or,

[0045] The material of the first cellulose film layer and the second cellulose film layer includes at least one of bacterial cellulose and cellulose nanofibers. The material of the two-dimensional film layer includes at least one of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2, that is, the two-dimensional film layer may contain any one of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2, or may contain two or more of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2 at the same time, all of which belong to the protection scope of the present invention. As a representative of new electromagnetic shielding materials, two-dimensional materials have significant advantages over traditional metal materials. Two-dimensional materials not only have the characteristics of light weight, can achieve efficient electromagnetic shielding at a lower filling amount, but also have the characteristics of low density, high flexibility and easy processing. Two-dimensional materials have higher carrier mobility and higher permittivity, so they can respond faster to changes in external electromagnetic fields. When electromagnetic waves penetrate the material, carriers can quickly move to the surface of the film material to form currents, which will generate a magnetic field opposite to the incident electromagnetic wave, thereby offsetting or weakening the magnetic field component of the incident wave. NbSe2, TiSe2, MoTe2, TaSe2 and VSe2 selected in the present invention are not commonly used materials in the field of electromagnetic shielding and are not conventionally used.

[0046] The material of the first cellulose film layer and the second cellulose film layer includes at least one of bacterial cellulose and cellulose nanofibers, that is, the first cellulose film layer can be one of bacterial cellulose or cellulose nanofibers, the second cellulose film layer can be one of bacterial cellulose or cellulose nanofibers, the first cellulose film layer can contain both bacterial cellulose and cellulose nanofibers, and the second cellulose film layer can contain both bacterial cellulose and cellulose nanofibers. Bacterial cellulose film has high strength and toughness and can withstand mechanical loads in electromagnetic shielding components. The nanofiber network structure of bacterial cellulose can enhance the absorption and scattering of electromagnetic waves. Cellulose nanofibers have a high specific surface area, which enables cellulose nanofiber films to more effectively absorb and scatter electromagnetic waves in electromagnetic shielding applications, thereby improving shielding effectiveness.

[0047] It should be noted that the material of the above-mentioned two-dimensional film layer includes at least one of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2, and the material of the first cellulose film layer and the second cellulose film layer includes at least one of bacterial cellulose and cellulose nanofibers, which can be set one by one or at the same time. In this embodiment, the effect of setting them simultaneously is better, and the electromagnetic shielding performance of the flexible electromagnetic shielding film is stronger.

[0048] The thickness of the two-dimensional thin film layer is 60-80 μm; and / or,

[0049] The thickness of the first cellulose film layer and the second cellulose film layer is 10-20 μm; and / or,

[0050] The thickness of the flexible electromagnetic shielding film is 90-100 μm.

[0051] In some embodiments, the mass ratio of the total mass of the first cellulose film layer and the second cellulose film layer to the two-dimensional film layer is (0.6-0.8):(0.11-0.35); preferably, the mass ratio of the total mass of the first cellulose film layer and the second cellulose film layer to the two-dimensional film layer is (0.6-0.8):0.24.

[0052] Based on the flexible electromagnetic shielding film provided by the present invention, the present invention also proposes a method for preparing the flexible electromagnetic shielding film. The preparation method includes all the technical solutions of the flexible electromagnetic shielding film, and therefore also has all the beneficial effects brought by the above-mentioned technical solutions, which will not be described one by one here.

[0053] In this embodiment, the method for preparing the flexible electromagnetic shielding film comprises the following steps:

[0054] S1, obtaining a first cellulose film layer;

[0055] S2, performing electrochemical stripping treatment on the two-dimensional material to obtain a dispersion containing the two-dimensional thin film material;

[0056] S3, covering the surface of the first cellulose film layer with the dispersion liquid and filtering it to obtain a two-dimensional film layer formed on the surface of the first cellulose film layer;

[0057] S4. Covering the surface of the two-dimensional film layer with a second cellulose film layer to obtain the flexible electromagnetic shielding film.

[0058] The electromagnetic shielding performance of the flexible electromagnetic shielding film is improved by forming a three-layer composite film (first cellulose film + two-dimensional film + second cellulose film). The preparation method of the flexible electromagnetic shielding film provided by the present invention has the advantages of simple process and stable performance of the prepared product, and is easy to realize industrial production.

[0059] Specifically, step S1 includes: filtering the cellulose dispersion to obtain a first cellulose film; wherein the concentration of the cellulose dispersion is 8-12 mg / mL.

[0060] Specifically, step S2 includes:

[0061] The crystalline powder is pressed into tablets to obtain a two-dimensional material;

[0062] Using the two-dimensional material as a working electrode, performing electrochemical stripping treatment on the two-dimensional material to obtain a dispersion containing the two-dimensional thin film material;

[0063] The dispersion containing the two-dimensional thin film material is washed, filtered and dried.

[0064] Specifically, during the electrochemical stripping process, the voltage is +4.0 to 8.0 V; and / or,

[0065] The electrochemical stripping treatment time is 10-60 minutes; and / or,

[0066] The washing reagent includes dimethylformamide;

[0067] The electrochemical stripping solution used in the electrochemical stripping treatment includes a solute and a solvent;

[0068] The solute includes tetrabutylammonium tetrafluoroborate;

[0069] The solvent includes at least one of propylene carbonate and dimethyl sulfoxide;

[0070] Preferably, the electrochemical stripping solution comprises tetrabutylammonium tetrafluoroborate and propylene carbonate; the concentration of tetrabutylammonium tetrafluoroborate in the electrochemical stripping solution is 0.03-0.075 mol / L; more preferably, the concentration of tetrabutylammonium tetrafluoroborate is 0.05 mol / L.

[0071] Specifically, the specific steps of step S4 are: covering the surface of the two-dimensional film layer with a bacterial cellulose dispersion, and filtering to obtain the flexible electromagnetic shielding film;

[0072] The pore size of the filter membrane used for filtration is 0.20-0.3 μm; preferably, the pore size of the filter membrane is 0.22 μm.

[0073] The present invention also provides an application, in which the flexible electromagnetic shielding film is used in electronic products, medical equipment, military fields, and household appliances to shield electromagnetic interference. The application includes all technical solutions of the flexible electromagnetic shielding film, and therefore also has all the beneficial effects brought by the above-mentioned technical solutions, which will not be repeated here one by one.

[0074] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0075] Example 1

[0076] This embodiment provides a method for preparing a flexible electromagnetic shielding film, comprising the following steps:

[0077] S1. Weigh 0.6g of bacterial cellulose and dissolve it in 60mL of deionized water. Use an ultrasonic cleaner to ultrasonicate it. The ultrasonic power is 720w and the ultrasonic time is 30min. Divide the dispersed bacterial cellulose dispersion into two portions, each of which is 30mL. Take one portion of bacterial cellulose and filter it using a vacuum-assisted filtration device. The filter membrane has a diameter of 50mm and a pore size of 0.22μm to obtain a first cellulose film layer. The thickness of the obtained first cellulose film layer is 10μm.

[0078] S2. Compress 0.8g of NbSe2 crystal powder into a NbSe2 two-dimensional material with a diameter of 14mm; clamp the NbSe2 two-dimensional material with a platinum electrode clamp and connect it to the negative electrode of the power supply as the working electrode, and the platinum electrode as the corresponding electrode; dissolve tetrabutylammonium tetrafluoroborate in a propylene carbonate solution, and then perform ultrasound for 10 minutes to prepare an electrochemical stripping solution with a concentration of 0.05mol / L and an ultrasound power of 720w. Pour the electrochemical stripping solution into the electrolytic cell and connect it to a DC power supply. The DC power supply has a constant voltage of 5V, and the reaction stops after the material swells and falls off completely, obtaining a dispersion of NbSe2 two-dimensional material after intercalation; use dimethylformamide to wash and centrifuge, wash for 5 minutes, and the speed is 8000rpm, and wash 6 times in total. The instruments for washing and centrifugation are centrifuges, and the washed material is dried to obtain NbSe2 two-dimensional powder after intercalation;

[0079] S3, dispersing 0.35 g of the intercalated NbSe2 two-dimensional powder obtained in step S2 with 50 mL of deionized water, adding the powder to the first cellulose film prepared in step S1, and performing vacuum-assisted filtration;

[0080] S4, adding another portion of bacterial cellulose dispersion to the product after vacuum assisted filtration in step S3, vacuum assisted filtration, and the film obtained after filtration is the NbSe2 flexible electromagnetic shielding film, and the thickness of the prepared NbSe2 flexible electromagnetic shielding film is 120μm. Figure 1 As shown in (a), the prepared NbSe2 flexible electromagnetic shielding film has a uniform texture. Figure 1 (b) and Figure 1 (c) It can be seen that the prepared NbSe2 flexible electromagnetic shielding film has good toughness and can be folded multiple times.

[0081] Example 2

[0082] This embodiment provides a method for preparing a flexible electromagnetic shielding film, comprising the following steps:

[0083] S1. Weigh 0.6g of bacterial cellulose and dissolve it in 60mL of deionized water. Use an ultrasonic cleaner to ultrasonicate it. The ultrasonic power is 720w and the ultrasonic time is 30min. Divide the dispersed bacterial cellulose dispersion into two portions, each of which is 30mL. Take one portion of bacterial cellulose and filter it using a vacuum-assisted filtration device. The filter membrane has a diameter of 50mm and a pore size of 0.22μm to obtain a first cellulose film layer. The thickness of the obtained first cellulose film layer is 10μm.

[0084] S2. Compact 0.8g of TiSe2 crystal powder into a TiSe2 two-dimensional material with a diameter of 14mm; clamp the TiSe2 two-dimensional material with a platinum electrode clamp and connect it to the negative electrode of the power supply as the working electrode, and the platinum electrode as the corresponding electrode; dissolve tetrabutylammonium tetrafluoroborate in a propylene carbonate solution, and then perform ultrasound for 10 minutes to prepare an electrochemical stripping solution with a concentration of 0.05mol / L and an ultrasound power of 720w. Pour the electrochemical stripping solution into the electrolytic cell and connect it to a DC power supply. The DC power supply has a constant voltage of 5V, and the reaction stops after the material swells and falls off completely, to obtain a dispersion of the intercalated TiSe2 two-dimensional material; use dimethylformamide to wash and centrifuge, wash for 5 minutes, and the speed is 8000rpm, and wash 6 times in total. The instruments for washing and centrifuging are centrifuges, and the washed material is dried to obtain the intercalated TiSe2 two-dimensional powder;

[0085] S3, dispersing 0.24 g of the TiSe2 two-dimensional film obtained in step S2 with 50 mL of deionized water, adding the dispersion to the first cellulose film prepared in step S1, and performing vacuum-assisted filtration;

[0086] S4. Add another portion of bacterial cellulose dispersion to the product after vacuum-assisted filtration in step S3, and perform vacuum-assisted filtration. The film obtained after the filtration is the TiSe2 flexible electromagnetic shielding film. The thickness of the prepared TiSe2 flexible electromagnetic shielding film is 100 μm.

[0087] Example 3

[0088] This embodiment provides a method for preparing a flexible electromagnetic shielding film, comprising the following steps:

[0089] S1. Weigh 0.6g of bacterial cellulose and dissolve it in 60mL of deionized water. Use an ultrasonic cleaner to ultrasonicate it. The ultrasonic power is 720w and the ultrasonic time is 30min. Divide the dispersed bacterial cellulose dispersion into two portions, each of which is 30mL. Take one portion of bacterial cellulose and filter it using a vacuum-assisted filtration device. The filter membrane has a diameter of 50mm and a pore size of 0.22μm to obtain a first cellulose film layer. The thickness of the obtained first cellulose film layer is 10μm.

[0090] S2. Compress 0.8g of MoTe2 crystal powder into a MoTe2 two-dimensional material with a diameter of 14mm; clamp the MoTe2 two-dimensional material with a platinum electrode clamp and connect it to the negative electrode of the power supply as the working electrode, and the platinum electrode as the corresponding electrode; dissolve tetrabutylammonium tetrafluoroborate in a propylene carbonate solution, and then perform ultrasound for 10 minutes to prepare an electrochemical stripping solution with a concentration of 0.05mol / L and an ultrasound power of 720w. Pour the electrochemical stripping solution into the electrolytic cell and connect it to a DC power supply. The DC power supply has a constant voltage of 5V, and the reaction stops after the material swells and falls off completely, obtaining a dispersion of the intercalated MoTe2 two-dimensional material; use dimethylformamide to wash and centrifuge, wash for 5 minutes, and the speed is 8000rpm, and wash 6 times in total. The instruments for washing and centrifuging are both centrifuges, and the washed material is dried to obtain the intercalated MoTe2 two-dimensional powder;

[0091] S3, dispersing 0.24 g of the intercalated MoTe2 two-dimensional film obtained in step S2 with 50 mL of deionized water, adding the film to the first cellulose film prepared in step S1, and performing vacuum-assisted filtration;

[0092] S4. Add another portion of bacterial cellulose dispersion to the product after vacuum-assisted filtration in step S3, and perform vacuum-assisted filtration. The film obtained after filtration is the MoTe2 flexible electromagnetic shielding film. The thickness of the prepared MoTe2 flexible electromagnetic shielding film is 95 μm.

[0093] Example 4

[0094] This embodiment provides a method for preparing a flexible electromagnetic shielding film, comprising the following steps:

[0095] S1. Weigh 0.6g of bacterial cellulose and dissolve it in 60mL of deionized water. Use an ultrasonic cleaner to ultrasonicate it. The ultrasonic power is 720w and the ultrasonic time is 30min. Divide the dispersed bacterial cellulose dispersion into two portions, each of which is 30mL. Take one portion of bacterial cellulose and filter it using a vacuum-assisted filtration device. The filter membrane has a diameter of 50mm and a pore size of 0.22μm to obtain a first cellulose film layer. The thickness of the obtained first cellulose film layer is 10μm.

[0096] S2. Compact 0.8g of NbSe2 crystal powder into a NbSe2 two-dimensional material with a diameter of 14mm; clamp the NbSe2 two-dimensional material with a platinum electrode clamp and connect it to the negative electrode of the power supply as the working electrode, and the platinum electrode as the corresponding electrode; dissolve tetrabutylammonium tetrafluoroborate in a propylene carbonate solution, and then perform ultrasound for 10 minutes to prepare an electrochemical stripping solution with a concentration of 0.05mol / L and an ultrasound power of 720w. Pour the electrochemical stripping solution into the electrolytic cell and connect it to a DC power supply. The DC power supply has a constant voltage of 5V, and the reaction stops after the material swells and falls off completely, obtaining a dispersion of MoTe2 two-dimensional material after intercalation; use dimethylformamide to wash and centrifuge, wash for 5 minutes, and the speed is 8000rpm, and wash 6 times in total. The instruments for washing and centrifugation are centrifuges, and the washed material is dried to obtain NbSe2 two-dimensional powder after intercalation;

[0097] S3, dispersing 0.24 g of the intercalated NbSe2 two-dimensional film obtained in step S2 with 50 mL of deionized water, adding the film to the first cellulose film prepared in step S1, and performing vacuum-assisted filtration;

[0098] S4. Add another portion of bacterial cellulose dispersion to the product after vacuum-assisted filtration in step S3, and perform vacuum-assisted filtration. The film obtained after the filtration is MoTe2 flexible electromagnetic shielding film. The prepared NbSe2 flexible electromagnetic shielding film has a thickness of 100 μm.

[0099] Example 5

[0100] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is substantially the same as that of Embodiment 4, except that in step S3, 0.18 g of the intercalated NbSe2 two-dimensional film obtained in step S2 is dispersed with 50 mL of deionized water.

[0101] Example 6

[0102] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is substantially the same as that of Embodiment 1, except that in step S1, 0.6 g of bacterial cellulose is weighed and dissolved in 60 mL of deionized water for ultrasonic dispersion, and the dispersed bacterial cellulose dispersion is divided into two portions, one portion is 20 mL and the other portion is 40 mL.

[0103] Example 7

[0104] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is different from Embodiment 1 in that, in step S1, 0.6 g of cellulose nanofibers are weighed and dissolved in 60 mL of deionized water for ultrasonic dispersion.

[0105] Example 8

[0106] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is different from Embodiment 1 in that in step S1, 0.8 g of bacterial cellulose is weighed and dissolved in 60 mL of deionized water for ultrasonic dispersion.

[0107] Example 9

[0108] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is different from Embodiment 1 in that the constant voltage of the DC power supply in step S2 is 4V.

[0109] Example 10

[0110] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is different from Embodiment 1 in that the constant voltage of the DC power supply in step S2 is 8V.

[0111] Embodiment 11

[0112] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is different from Embodiment 1 in that the concentration of the electrochemical stripping solution in step S2 is 0.03 mol / L.

[0113] Example 12

[0114] This embodiment provides a method for preparing a flexible electromagnetic shielding film, which is different from Embodiment 1 in that the concentration of the electrochemical stripping solution in step S2 is 0.075 mol / L.

[0115] Comparative Example 1

[0116] Compared with Example 1, the NbSe2 crystal powder has not been subjected to tableting or electrochemical stripping.

[0117] 0.35g of NbSe2 powder that has not been electrochemically stripped was dissolved in 50mL of deionized water for dispersion, and ultrasonic cleaning was performed using an ultrasonic cleaning machine with an ultrasonic power of 720w and an ultrasonic time of 30min. The dispersed solution was filtered using a vacuum assisted filtration device with a filter membrane diameter of 50mm and a pore size of 0.22μm.

[0118] Comparative Example 2

[0119] Compared with Example 2, the TiSe2 crystal powder has not been subjected to tableting or electrochemical stripping.

[0120] 0.24 g of TiSe2 powder that has not been electrochemically stripped was dissolved in 50 mL of deionized water for dispersion, and ultrasonic cleaning was performed using an ultrasonic cleaning machine with an ultrasonic power of 720 W and an ultrasonic time of 30 min. The dispersed solution was filtered using a vacuum-assisted filtration device with a filter membrane diameter of 50 mm and a pore size of 0.22 μm.

[0121] Comparative Example 3

[0122] Compared with Example 3, the MoTe2 crystal powder has not been subjected to tableting or electrochemical exfoliation.

[0123] 0.24 g of MoTe2 powder that has not been electrochemically stripped was dissolved in 50 mL of deionized water for dispersion, and ultrasonic cleaning was performed using an ultrasonic cleaning machine with an ultrasonic power of 720 W and an ultrasonic time of 30 min. The dispersed solution was filtered using a vacuum-assisted filtration device with a filter membrane diameter of 50 mm and a pore size of 0.22 μm.

[0124] Comparative Example 4

[0125] Weigh 0.6g of bacterial cellulose and dissolve it in 60mL of deionized water, and use an ultrasonic cleaning machine to ultrasonicate it, with an ultrasonic power of 720w and an ultrasonic time of 30min. The dispersed bacterial cellulose is filtered using a vacuum-assisted filtration device, with a filter membrane diameter of 50mm and a pore size of 0.22μm.

[0126] Performance Testing

[0127] The waveguide method is used to test the electromagnetic shielding performance of the film. The method of testing the electromagnetic shielding performance of the film by the waveguide method is to prepare a waveguide device of appropriate size and corresponding electromagnetic band, connect it to the vector network analyzer to ensure the generation and measurement of stable electromagnetic waves and calibration; then place a flat and defect-free film sample cut to suitable waveguide size in the middle of the waveguide to ensure that the sample completely covers the waveguide cross-section and there is no air gap; finally, based on the baseline measurement and the measurement results of the S parameters after inserting the sample, the shielding effectiveness (SE) is calculated using the vector network analyzer to evaluate the electromagnetic shielding performance of the film material.

[0128] The electromagnetic shielding effectiveness of the flexible electromagnetic shielding films prepared in Examples 1-5 and the films prepared in Comparative Examples 1-3 was measured, and the results are as follows:

[0129] Table 1 Electromagnetic shielding performance test

[0130]

[0131] It can be seen intuitively from Table 1 that the electromagnetic shielding performance of the electromagnetic shielding film processed by this method is significantly improved compared with the unprocessed film. Figures 2 to 4As shown, compared with comparative example 1, the electromagnetic shielding performance of embodiment 1 is improved from an average of 9.7 dB to 27.0 dB, compared with comparative example 2, the electromagnetic shielding performance of embodiment 2 is improved from an average of 17.0 dB to 24.1 dB, and compared with comparative example 3, the electromagnetic shielding performance of embodiment 3 is improved from an average of 12.0 dB to 23.7 dB. The layered structure formed after the stripping treatment helps to form a more effective electromagnetic shielding layer, and electromagnetic waves will be partially reflected and transmitted at each interface. These multiple reflected and transmitted electromagnetic waves interfere with each other, enhance the absorption and reflection of electromagnetic waves, and thus improve the shielding effectiveness.

[0132] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A flexible electromagnetic shielding film, characterized in that: The invention comprises a two-dimensional film layer and a first cellulose film layer and a second cellulose film layer respectively arranged on both sides of the two-dimensional film layer.

2. The flexible electromagnetic shielding film according to claim 1, characterized in that: The material of the two-dimensional thin film layer includes at least one of NbSe2, TiSe2, MoTe2, TaSe2 and VSe2; and / or, The material of the first cellulose film layer and the second cellulose film layer includes at least one of bacterial cellulose and cellulose nanofiber.

3. The flexible electromagnetic shielding film according to claim 1, characterized in that: The thickness of the two-dimensional thin film layer is 60-80 μm; and / or, The thickness of the first cellulose film layer and the second cellulose film layer is 10-20 μm; and / or, The thickness of the flexible electromagnetic shielding film is 90-100 μm.

4. The flexible electromagnetic shielding film according to claim 1, characterized in that: The mass ratio of the total mass of the first cellulose film layer and the second cellulose film layer to the mass of the two-dimensional film layer is (0.6-0.8):(0.11-0.35); preferably, the mass ratio of the total mass of the first cellulose film layer and the second cellulose film layer to the mass of the two-dimensional film layer is (0.6-0.8):0.

24.

5. A method for preparing the flexible electromagnetic shielding film according to claim 1, characterized in that: The following steps are involved: S1, obtaining a first cellulose film layer; S2, performing electrochemical stripping treatment on the two-dimensional material to obtain a dispersion containing the two-dimensional thin film material; S3, covering the surface of the first cellulose film layer with the dispersion liquid and filtering it to obtain a two-dimensional film layer formed on the surface of the first cellulose film layer; S4. Covering the surface of the two-dimensional film layer with a second cellulose film layer to obtain the flexible electromagnetic shielding film.

6. The method for preparing the flexible electromagnetic shielding film according to claim 5, characterized in that: Step S1 includes: filtering the cellulose dispersion to obtain a first cellulose film; wherein the concentration of the cellulose dispersion is 8-12 mg / mL.

7. The method for preparing the flexible electromagnetic shielding film according to claim 5, characterized in that: Step S2 includes: The crystalline powder is pressed into tablets to obtain a two-dimensional material; Using the two-dimensional material as a working electrode, performing electrochemical stripping treatment on the two-dimensional material to obtain a dispersion containing the two-dimensional thin film material; The dispersion containing the two-dimensional thin film material is washed, filtered and dried.

8. The method for preparing the flexible electromagnetic shielding film according to claim 7, characterized in that: In the electrochemical stripping process, the voltage is +4.0 to 8.0 V; and / or, The electrochemical stripping treatment lasts for 10-60 minutes; and / or, The washing reagent includes dimethylformamide; The electrochemical stripping solution used in the electrochemical stripping treatment includes a solute and a solvent; the solute includes tetrabutylammonium tetrafluoroborate; the solvent includes at least one of propylene carbonate and dimethyl sulfoxide; Preferably, the electrochemical stripping solution comprises tetrabutylammonium tetrafluoroborate and propylene carbonate; the concentration of tetrabutylammonium tetrafluoroborate in the electrochemical stripping solution is 0.03-0.075 mol / L; more preferably, the concentration of tetrabutylammonium tetrafluoroborate is 0.05 mol / L.

9. The method for preparing the flexible electromagnetic shielding film according to claim 5, characterized in that: The specific steps of step S4 are: covering the surface of the two-dimensional film layer with a bacterial cellulose dispersion, and filtering to obtain the flexible electromagnetic shielding film; The pore size of the filter membrane used for filtration is 0.20-0.3 μm; preferably, the pore size of the filter membrane is 0.22 μm.

10. An application, characterized in that: The flexible electromagnetic shielding film described in any one of claims 1 to 4 is used in electronic products, medical equipment, military fields, and household appliances to shield electromagnetic interference.

Citation Information

Cited By

  • Transition metal thiocarbide composite film with electromagnetic shielding effectiveness as well as preparation method and application of transition metal thiocarbide composite film

    CN122002773A