Solar cell module, preparation method thereof and solar cell
Through ion beam-assisted deposition and thermal evaporation, perovskite solar cell modules with high transmittance, low surface resistance and high mechanical flexibility were prepared, solving the transparency and bending resistance of flexible perovskite solar cells. Inadequate, it improves the photoelectric conversion efficiency and is suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202411150908.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
Existing flexible perovskite solar cells have not yet met the needs of various applications in terms of transparency, bending resistance and photoelectric conversion efficiency.
The dense metal layer was prepared by ion beam-assisted deposition technology, and the arranged oxide-metal-oxide electrode structure was laminated, and the photoactive layer was prepared in combination with thermal evaporation method to form high transmittance, low surface resistance and high mechanical flexibility. solar cell modules.
It realizes transparent, bending-resistant and high photoelectric conversion efficiency solar cell modules, meeting a variety of application needs, such as BIPV, CIPV and wearable devices.
Smart Images

Figure CN119031806A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of energy storage technology, and in particular to a solar cell assembly and a preparation method thereof, and a solar cell. Background Art
[0002] Solar cells, such as perovskite solar cells (PSCs), are increasingly used in scenarios such as building integrated photovoltaics (BIPV), car integrated photovoltaics (CIPV), and wearable electronic devices, and the demand for transparent and flexible PSCs is increasing. However, due to the limitations of related technologies, current flexible perovskite solar cells still cannot meet the requirements. Summary of the invention
[0003] In view of this, embodiments of the present application provide a solar cell assembly, a method for preparing the same, and a solar cell.
[0004] The first aspect of the present application provides a method for preparing a solar cell module, the method comprising:
[0005] providing a substrate;
[0006] forming a first oxide layer on one side of the substrate;
[0007] A first metal layer is prepared on a side of the first oxide layer away from the substrate by ion beam assisted deposition;
[0008] Prepare a second metal layer on a side of the first metal layer away from the substrate;
[0009] forming a second oxide layer on a side of the second metal layer away from the substrate;
[0010] forming a photoactive layer on a side of the second oxide layer away from the substrate;
[0011] A second electrode layer is formed on the side of the photoactive layer away from the substrate.
[0012] In one embodiment, preparing the first metal layer on the side of the first oxide layer away from the substrate by ion beam assisted deposition includes: preparing the first metal layer on the side of the first oxide layer away from the substrate by magnetron sputtering under ion beam assisted conditions;
[0013] Preferably, the preparation of the first metal layer on the side of the first oxide layer away from the substrate by magnetron sputtering under ion beam assistance conditions includes one or more of the following conditions:
[0014] The ion source discharge current is 0.1A~3A;
[0015] DC voltage is 110V~130V;
[0016] The ion source for ion beam assistance includes argon ions; the vacuum before deposition is 10 -3 Pa~10 -6 Pa;
[0017] The raw materials include one or more of silver, gold and copper;
[0018] Sputtering pressure is 0.1Pa~2Pa;
[0019] The deposition rate of the first metal layer is and,
[0020] The thickness of the first metal layer is 0.5nm to 3nm;
[0021] Preferably, a first oxide layer is prepared on one side of the substrate, a first metal layer is prepared on the side of the first oxide layer away from the substrate by ion beam assisted deposition, a second metal layer is prepared on the side of the first metal layer away from the substrate, a second oxide layer is prepared on the side of the second metal layer away from the substrate, a photoactive layer is prepared on the side of the second oxide layer away from the substrate, and a second electrode layer is prepared on the side of the photoactive layer away from the substrate, all using a plating process.
[0022] In one embodiment, preparing the second metal layer on the side of the first metal layer away from the substrate comprises: preparing the second metal layer on the side of the first metal layer away from the substrate by magnetron sputtering;
[0023] Preferably, the preparation of the second metal layer on the side of the first metal layer away from the substrate by magnetron sputtering includes one or more of the following conditions:
[0024] The vacuum degree before deposition was 10 -3 Pa~10 -6 Pa;
[0025] Sputtering gases include argon;
[0026] Sputtering pressure is 0.1Pa~2Pa;
[0027] The raw materials include silver; and,
[0028] The thickness of the second metal layer is 1nm to 10nm;
[0029] Preferably, the preparation of the first metal layer on the side of the first oxide layer away from the substrate and the preparation of the second metal layer on the side of the first metal layer away from the substrate are performed in the same device by ion beam assisted deposition.
[0030] In one embodiment, preparing a photoactive layer on a side of the second oxide layer away from the substrate comprises:
[0031] On the side of the second oxide layer away from the substrate, a plurality of photoactive material layers are stacked and arranged, wherein the material of each photoactive material layer is a single material;
[0032] Annealing the multi-layer photoactive material layer to obtain a photoactive layer;
[0033] Preferably, preparing a stacked multilayer photoactive material layer on a side of the second oxide layer away from the substrate comprises: using one or more of cesium iodide, methylamine iodide and formamidine iodide and lead iodide as raw materials, and preparing a stacked multilayer photoactive material layer on a side of the second oxide layer away from the substrate by thermal evaporation;
[0034] Preferably, the following conditions are met when the multilayer photoactive material layer is stacked on the side of the second oxide layer away from the substrate by thermal evaporation: the vacuum degree before evaporation is 10 -4 Pa~10 -5 Pa;
[0035] Preferably, each photoactive material layer is prepared by single-source evaporation, the thickness of each photoactive material layer is 0.5 nm to 30 nm, and the thickness of the photoactive layer is 200 nm to 800 nm;
[0036] Preferably, the conditions for annealing the multi-layer photoactive material layer include: an annealing temperature of 100° C. to 300° C., and an annealing time of 2 minutes to 30 minutes.
[0037] In one embodiment, preparing the first oxide layer on one side of the substrate includes: preparing the first oxide layer on one side of the substrate by electron beam evaporation;
[0038] Preferably, preparing the first oxide layer on one side of the substrate by electron beam evaporation includes one or more of the following conditions:
[0039] The vacuum degree before evaporation is 10 -3 Pa~10 -4 Pa;
[0040] The raw materials include one or more of zinc oxide, tungsten oxide and molybdenum oxide;
[0041] The evaporation rate is controlled as and,
[0042] The thickness of the first oxide layer is 5nm to 50nm;
[0043] Preferably, preparing the second oxide layer on the side of the second metal layer away from the substrate comprises: preparing the second oxide layer on the side of the second metal layer away from the substrate by electron beam evaporation;
[0044] Preferably, preparing the second oxide layer on the side of the second metal layer away from the substrate by electron beam evaporation includes one or more of the following conditions:
[0045] The vacuum degree before deposition was 10 -3 Pa~10 -4 Pa;
[0046] The raw materials include one or more of zinc oxide, tungsten oxide and molybdenum oxide;
[0047] The evaporation rate is controlled as and,
[0048] The thickness of the second oxide layer is 5nm to 50nm;
[0049] Preferably, after preparing the second oxide layer on the side of the second metal layer away from the substrate and before preparing the photoactive layer on the side of the second oxide layer away from the substrate, the method further comprises: preparing a first transmission layer on the side of the second oxide layer away from the substrate;
[0050] Preferably, preparing the first transmission layer on the side of the second oxide layer away from the substrate comprises: preparing the first transmission layer on the side of the second oxide layer away from the substrate by magnetron sputtering;
[0051] Preferably, preparing the first transmission layer on the side of the second oxide layer away from the substrate by magnetron sputtering includes one or more of the following conditions:
[0052] The atmosphere is a mixture of inert gas and oxygen, with oxygen accounting for 0.01% to 2%;
[0053] The gas pressure is 1mTorr~8mTorr;
[0054] The deposition rate of the first transport layer is and,
[0055] Thickness: 5nm~40nm;
[0056] Preferably, after preparing the photoactive layer on the side of the second oxide layer away from the substrate and before preparing the second electrode layer on the side of the photoactive layer away from the substrate, the method further comprises:
[0057] A second transmission layer is formed on a side of the photoactive layer away from the substrate;
[0058] Preferably, preparing the second transmission layer on the side of the photoactive layer away from the substrate comprises: preparing the second transmission layer on the side of the photoactive layer away from the substrate by thermal evaporation;
[0059] Preferably, the conditions for preparing the second transmission layer on the side of the photoactive layer away from the substrate by thermal evaporation include: the evaporation rate is
[0060] Preferably, preparing the second electrode layer on the side of the photoactive layer away from the substrate comprises: preparing the second electrode layer on the side of the photoactive layer away from the substrate by thermal evaporation;
[0061] Preferably, forming a photoactive layer on a side of the second oxide layer away from the substrate, forming a second transport layer on a side of the photoactive layer away from the substrate, and forming a second electrode layer on a side of the photoactive layer away from the substrate are performed in the same device.
[0062] A second aspect of the present application provides a method for preparing a solar cell module, comprising:
[0063] providing a substrate;
[0064] preparing a first electrode layer on one side of the substrate;
[0065] A plurality of photoactive material layers are stacked on one side of the first electrode layer away from the substrate, wherein the material of each photoactive material layer is a single material;
[0066] Annealing the multi-layer photoactive material layer to obtain a photoactive layer;
[0067] A second electrode layer is formed on the side of the photoactive layer away from the substrate.
[0068] In one embodiment, preparing a stacked multi-layer photoactive material layer on a side of the first electrode layer away from the substrate comprises: using one or more of cesium iodide, methylamine iodide and formamidine iodide and lead iodide as raw materials, and using a thermal evaporation method to prepare a stacked multi-layer photoactive material layer on a side of the first electrode layer away from the substrate;
[0069] Preferably, the multi-layer photoactive material layer stacked on the side of the first electrode layer away from the substrate by thermal evaporation satisfies the following conditions: the vacuum degree before evaporation is 10 -4 Pa~10 -5 Pa;
[0070] Preferably, each photoactive material layer is prepared by single-source evaporation, the thickness of each photoactive material layer is 0.5 nm to 30 nm, and the thickness of the photoactive layer is 200 nm to 800 nm;
[0071] Preferably, the conditions for annealing the multi-layer photoactive material layer include: an annealing temperature of 100° C. to 300° C., and an annealing time of 2 minutes to 30 minutes.
[0072] The third aspect of the present application provides a solar cell assembly, comprising:
[0073] substrate;
[0074] a first electrode layer, located on one side of the substrate, the first electrode layer comprising a first oxide layer, a first metal layer, a second metal layer and a second oxide layer, the first oxide layer being located on a side of the first metal layer close to the substrate;
[0075] A photoactive layer is located on a side of the first electrode layer away from the substrate;
[0076] A second electrode layer is located on a side of the photoactive layer away from the substrate;
[0077] The surface resistance of the first electrode layer is 5Ω to 35Ω.
[0078] In one embodiment, the surface resistance of the first electrode layer is 5Ω to 10Ω;
[0079] Preferably, the thickness of the first metal layer is 0.5 nm to 3 nm;
[0080] Preferably, the thickness of the second metal layer is 1 nm to 10 nm;
[0081] Preferably, the first metal layer comprises one or more of silver, gold and copper;
[0082] Preferably, the second metal layer comprises silver;
[0083] Preferably, the transmittance of the first electrode layer to light with a wavelength of 400 to 800 nm is 70 to 90%.
[0084] A fourth aspect of the present application provides a solar cell, including the solar cell module prepared by the above-mentioned preparation method, or including the above-mentioned solar cell module.
[0085] A fourth aspect of the present application provides a solar cell, comprising the above-mentioned solar cell assembly.
[0086] In the preparation method of the solar cell module of the embodiment of the present application, ion beam assisted deposition is utilized, and the ion beam has a certain bombardment effect on the first metal layer, so that the first metal layer is relatively dense, which is beneficial to the subsequent growth of the second metal layer, and is beneficial to obtaining a dense, complete and thin second metal layer, thereby making the electrode layer formed by the stacked first oxide layer, first metal layer, second metal layer and second oxide layer have a higher transmittance, lower surface resistance and stronger mechanical flexibility, thereby facilitating the acquisition of a solar cell module that is resistant to bending, has high transparency and has a high photoelectric conversion efficiency (Power Conversion Efficiency, referred to as PCE). BRIEF DESCRIPTION OF THE DRAWINGS
[0087] Figure 1 This is a schematic diagram of a process for preparing a solar cell module in one embodiment of the present application.
[0088] Figure 2 This is a schematic flow chart of a method for preparing a solar cell module in another embodiment of the present application.
[0089] Figure 3 This is a schematic diagram of the process for preparing a photoactive layer in one embodiment of the present application.
[0090] Figure 4 This is a schematic flow chart of a method for preparing a solar cell module in another embodiment of the present application.
[0091] Figures 5 to 12 This is a schematic diagram of the preparation process of a solar cell module in one embodiment of the present application.
[0092] Fig.13 This is a schematic flow chart of a method for preparing a solar cell module in another embodiment of the present application. DETAILED DESCRIPTION
[0093] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0094] In addition, in order to better illustrate the present application, numerous specific details are given in the following specific embodiments. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In some examples, methods and means well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present application.
[0095] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0096] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.
[0097] The first aspect of the present application provides a method for preparing a solar cell module, referring to Figure 1 A schematic diagram of a method for preparing a solar cell module is shown, and Figures 5 to 12 The schematic diagram of the preparation process of the solar cell assembly shown is a schematic diagram of the preparation process of the solar cell assembly, and the preparation method includes the following steps.
[0098] S110: providing a substrate.
[0099] It can be understood that the substrate may be a flexible substrate, or a transparent substrate. For example, the material of the substrate may be transparent polyimide (CPI) or the like.
[0100] S120: Prepare a first oxide layer on one side of the substrate, see Figure 5 .
[0101] In one embodiment, preparing the first oxide layer on one side of the substrate includes: preparing the first oxide layer on one side of the substrate by electron beam evaporation. Thus, the electron beam evaporation method can avoid preparing the first oxide layer in an exposed environment, avoid the first oxide layer from being corroded by water and oxygen in the exposed environment, and help improve the reliability of the first oxide layer; and the obtained first oxide layer has strong bending resistance.
[0102] In one embodiment, the first oxide layer is prepared on one side of the substrate by electron beam evaporation, which includes one or more of the following conditions: the vacuum degree before evaporation is 10 -3 Pa~10 -4 Pa (for example, it can be 10 -3 Pa, 10 -3.5 Pa and 10 - 4 Pa, etc.); the raw materials include one or more of zinc oxide, tungsten oxide and molybdenum oxide; the evaporation rate is controlled to be (For example, or etc.); and, the thickness of the first oxide layer is 5nm to 50nm (for example, it can be 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm, etc.). Therefore, the above-mentioned electron beam evaporation conditions can further avoid preparing the first oxide layer in an exposed environment, avoid the first oxide layer from being corroded by water and oxygen in the exposed environment, and help improve the reliability of the first oxide layer; the evaporation rate is appropriate, and the obtained first oxide layer is relatively flat and dense, and has a strong bending resistance; the thickness of the first oxide layer is thin, and the light transmittance is high, which is conducive to improving the PCE efficiency of the solar cell module.
[0103] S130: Prepare a first metal layer on a side of the first oxide layer away from the substrate by ion beam assisted deposition. Figure 6 .
[0104] In one embodiment, preparing the first metal layer on the side of the first oxide layer away from the substrate by ion beam assisted deposition includes: preparing the first metal layer on the side of the first oxide layer away from the substrate by magnetron sputtering under ion beam assisted conditions. It can be understood that when the first metal layer is prepared by magnetron sputtering, ion beam assistance is used, and the high-speed ion beam has a certain bombardment effect on the first metal layer, making the first metal layer more dense.
[0105] Exemplarily, the ion source of the ion beam assistance includes argon ions, etc. During the process of bombarding the first metal layer, the argon ions will be converted into argon gas, which will hardly affect the composition of the first metal layer.
[0106] In one embodiment, under ion beam assisted conditions, the first metal layer is prepared on the side of the first oxide layer away from the substrate by magnetron sputtering, including one or more of the following conditions: the ion source discharge current is 0.1A to 3A (for example, it can be 0.1A, 0.5A, 1A, 1.5A, 2A, 2.5A or 3A, etc.); the DC voltage is 110V to 130V (for example, it can be 110V, 115V, 120V, 125V or 130V, etc.); the vacuum degree before deposition is 10 -3 Pa~10 -6 Pa (for example, it can be 10 -3 Pa, 10 -4 Pa, 10 -5 Pa or 10 -6 Pa, etc.); the sputtering pressure is 0.1Pa~2Pa (for example, it can be 0.1Pa, 0.5Pa, 1Pa, 1.5Pa or 2Pa, etc.); the raw materials include one or more of silver, gold and copper; and the thickness of the first metal layer is 0.5nm~3nm (for example, it can be 0.5nm, 1nm, 1.5nm, 2nm, 2.5nm or 3nm, etc.). Therefore, the above-mentioned ion beam assisted deposition conditions make the first metal layer denser, more conducive to obtaining a complete first metal layer on the entire surface, and conducive to the subsequent growth of the second metal layer. The process of preparing the first metal layer is not disturbed by the exposure environment, so that the first metal layer has higher reliability and stronger mechanical flexibility.
[0107] S140: Prepare a second metal layer on a side of the first metal layer away from the substrate, see Figure 7 .
[0108] In one embodiment, preparing the second metal layer on the side of the first metal layer away from the substrate includes: preparing the second metal layer on the side of the first metal layer away from the substrate by magnetron sputtering. Thus, the magnetron sputtering method can avoid preparing the second metal layer in the air, avoid the second metal layer from being corroded by water and oxygen, and help improve the reliability of the second metal layer.
[0109] In one embodiment, the second metal layer is prepared on the side of the first metal layer away from the substrate by magnetron sputtering, which includes one or more of the following conditions: the vacuum degree before deposition is 10 -3 Pa~10 -6 Pa (for example, it can be 10 -3 Pa, 10 -4 Pa, 10 -5 Pa or 10 -6 Pa, etc.); the sputtering gas includes argon; the sputtering pressure is 0.1Pa~2Pa (for example, it can be 0.1Pa, 0.5Pa, 1Pa, 1.5Pa or 2Pa, etc.); the raw material includes silver; and the thickness of the second metal layer is 1nm~10nm (for example, it can be 1nm, 3nm, 5nm, 7nm, 9nm or 10nm, etc.). Therefore, the above-mentioned magnetron sputtering method can further prevent the second metal layer from being corroded by water and oxygen, and improve the reliability of the second metal layer; the sputtering pressure is appropriate, which is conducive to obtaining a dense and complete second metal layer, the thickness of the second metal layer is appropriate, the light transmittance is high, and the flexibility is strong.
[0110] It can be understood that when the raw material of the first metal layer is silver, the seed silver obtained by magnetron sputtering deposition under the assistance of ion beam is complete on the entire surface, and the seed silver layer is conducive to the growth of the second metal layer; illustratively, when the raw material of the second metal layer is silver, the seed silver layer can induce the metal silver layer to grow continuously to obtain a complete metal silver layer on the entire surface, and the metal silver layer is thin, has a low surface resistance, a high light transmittance, and strong flexibility.
[0111] In one embodiment, the preparation of the first metal layer on the side of the first oxide layer away from the substrate and the preparation of the second metal layer on the side of the first metal layer away from the substrate are performed in the same device by ion beam assisted deposition. This facilitates the growth of the second metal layer on the surface of the first metal layer, and can avoid the erosion of the first metal layer and the second metal layer by water and oxygen in the external environment. Exemplarily, the first metal layer and the second metal layer are prepared in a combined magnetron sputtering and ion beam device. Exemplarily, in a combined magnetron sputtering and ion beam device, the first metal layer is prepared by magnetron sputtering under ion beam assisted conditions. After the preparation of the first metal layer is completed, the ion beam assistance is stopped, and the second metal layer is continued to be prepared by magnetron sputtering.
[0112] S150: Prepare a second oxide layer on the side of the second metal layer away from the substrate, see Figure 8 .
[0113] In one embodiment, preparing the second oxide layer on the side of the second metal layer away from the substrate includes: preparing the second oxide layer on the side of the second metal layer away from the substrate by electron beam evaporation. Thus, the electron beam evaporation method can avoid preparing the second oxide layer in an exposed environment, avoid the second oxide layer from being corroded by water and oxygen in the exposed environment, and help improve the reliability of the second oxide layer; and the obtained second oxide layer has strong bending resistance.
[0114] In one embodiment, the second oxide layer is prepared on the side of the second metal layer away from the substrate by electron beam evaporation, which includes one or more of the following conditions: the vacuum degree before evaporation is 10 -3 Pa~10 -4 Pa (for example, it can be 10 - 3 Pa, 10 -3.5 Pa and 10 -4 Pa, etc.); the raw materials include one or more of zinc oxide, tungsten oxide and molybdenum oxide; the evaporation rate is controlled to be (For example, or etc.); and, the thickness of the second oxide layer is 5nm to 50nm (for example, it can be 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm, etc.). Therefore, the above-mentioned electron beam evaporation conditions can further avoid preparing the second oxide layer in an exposed environment, avoid the second oxide layer from being corroded by water and oxygen in the exposed environment, and help improve the reliability of the second oxide layer; the evaporation rate is appropriate, and the obtained second oxide layer is relatively flat and dense, and has a strong bending resistance; the thickness of the second oxide layer is thin, and the light transmittance is high, which is conducive to improving the PCE efficiency of the solar cell module.
[0115] It can be understood that the electrode formed by the above-mentioned stacked first oxide layer, first metal layer, second metal layer and second oxide layer is an oxide-metal-oxide (OMO) electrode, and the electrode layer has an overall thin thickness, strong flexibility, low surface resistance, high light transmittance and strong stability, so that the solar cell module has higher stability and longer life.
[0116] In one embodiment, after forming a second oxide layer on a side of the second metal layer away from the substrate, and before forming a photoactive layer on a side of the second oxide layer away from the substrate, Figure 2 The schematic flow chart of the preparation method of the solar cell assembly shown in the figure further includes the following steps.
[0117] S180: Prepare a first transmission layer on the side of the second oxide layer away from the substrate, see Fig. 9 .
[0118] In one embodiment, preparing the first transmission layer on the side of the second oxide layer away from the substrate includes: preparing the first transmission layer on the side of the second oxide layer away from the substrate by magnetron sputtering.
[0119] In one embodiment, the first transport layer is prepared on the side of the second oxide layer away from the substrate by magnetron sputtering, including one or more of the following conditions: the atmosphere is a mixture of an inert gas and oxygen, the oxygen ratio is 0.01% to 2% (for example, it can be 0.01%, 0.1%, 0.5%, 1%, 1.5% or 2%, etc., and the oxygen ratio is the volume ratio of oxygen to the inert gas); the gas pressure is 1mTorr to 8mTorr (for example, it can be 1mTorr, 2mTorr, 4mTorr, 6mTorr or 8mTorr, etc.); the deposition rate of the first transport layer is (For example, The magnetron sputtering conditions are conducive to obtaining a first transmission layer with high flatness and density, and are conducive to improving the performance of the solar cell module.
[0120] S160: Prepare a photoactive layer on the side of the second oxide layer away from the substrate, see Fig.10 .
[0121] Exemplarily, the photoactive layer is located on a side of the first transmission layer away from the substrate.
[0122] In one embodiment, referring to Figure 3 The schematic flow chart of the method for preparing the photoactive layer is shown. Preparing the photoactive layer on the side of the second oxide layer away from the substrate includes the following steps.
[0123] S161: preparing a stacked multi-layer photoactive material layer on a side of the second oxide layer away from the substrate, wherein the material of each photoactive material layer is a single material.
[0124] Exemplarily, the photoactive material layers are all located on a side of the first transmission layer away from the substrate.
[0125] In one embodiment, preparing a stacked multilayer photoactive material layer on the side of the first transmission layer away from the substrate includes: using one or more of cesium iodide, methylamine iodide and formamidine iodide and lead iodide as raw materials, and using thermal evaporation to prepare a stacked multilayer photoactive material layer on the side of the second oxide layer away from the substrate. Thus, using thermal evaporation to prepare a stacked single-material photoactive material layer can avoid the use of solvents, which is environmentally friendly, and the photoactive material layer will hardly be corroded by water and oxygen during the preparation process, ensuring the reliability of the photoactive material layer; moreover, by controlling the thickness of each layer of the photoactive material layer, the proportion and composition of the perovskite are controlled, and there is no need to accurately control the evaporation speed of different materials, reducing the difficulty of preparing the perovskite.
[0126] It can be understood that when the photoactive material layer is prepared using methylamine iodide and / or formamidine iodide as raw materials, since methylamine iodide and formamidine iodide contain organic ligands, the obtained photoactive material layer is smoother and more flexible, thereby making the photoactive layer have higher flatness and flexibility, and making the PCE efficiency of the solar cell module higher.
[0127] In one embodiment, each photoactive material layer is prepared by single-source evaporation, and the thickness of each photoactive material layer is 0.5nm to 30nm (for example, it can be 0.5nm, 1nm, 5nm, 10nm, 15nm, 20nm, 25nm or 30nm, etc.), and the thickness of the photoactive layer is 200nm to 800nm (for example, it can be 200nm, 300nm, 400nm, 500nm, 600nm, 700nm or 800nm, etc.). Thus, by controlling the thickness of each photoactive material layer, the proportion and composition of perovskite in the photoactive layer can be regulated, and the overall thickness of the photoactive layer is easy to control; the single-source evaporation method reduces the equipment cost requirements and can successfully prepare high-quality perovskite films.
[0128] For example, before preparing a stacked multi-layer photoactive material layer on the side of the second oxide layer away from the substrate by thermal evaporation, the vacuum degree in the device is adjusted to 10 -4 Pa~10 -5 Pa (for example, it can be 10 -4 Pa, 10 -4.5 Pa and 10 -5 Pa, etc.), thereby being more conducive to obtaining a photoactive layer with higher flatness and higher quality.
[0129] S162: performing annealing treatment on the multiple photoactive material layers to obtain a photoactive layer.
[0130] In one embodiment, the conditions for annealing the multi-layer photoactive material layer include: an annealing temperature of 100° C. to 300° C. (e.g., 100° C., 200° C., or 300° C.), and an annealing time of 2 minutes to 30 minutes (e.g., 2 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, or 30 minutes). Thus, the annealing conditions are suitable, which is conducive to obtaining a perovskite with uniform composition.
[0131] Exemplarily, the photoactive layer is prepared in a thermal evaporation device. It is understood that the annealing process can be performed in the thermal evaporation device or in other devices.
[0132] In one embodiment, referring to Figure 4 The schematic flow chart of the preparation method of the solar cell assembly shown in the figure further includes the following steps after preparing the photoactive layer on the side of the second oxide layer away from the substrate and before preparing the second electrode layer on the side of the photoactive layer away from the substrate.
[0133] S190: Prepare a second transmission layer on the side of the photoactive layer away from the substrate, see Fig.11 .
[0134] In one embodiment, preparing the second transmission layer on the side of the photoactive layer away from the substrate includes: preparing the second transmission layer on the side of the photoactive layer away from the substrate by thermal evaporation.
[0135] In one embodiment, the conditions for preparing the second transmission layer on the side of the photoactive layer away from the substrate by thermal evaporation include: the evaporation rate is (For example, or Thus, the evaporation rate is appropriate, which is conducive to obtaining a dense second transmission layer, and the second transmission layer has strong mechanical flexibility.
[0136] In one embodiment, one of the first transmission layer and the second transmission layer includes one or more of nickel oxide, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly(3-hexylthiophene) (P3HT) and poly-3,4-ethylenedioxythiophene (PEDOT), and the other of the first transmission layer and the second transmission layer includes one or more of C60, fullerene, a fullerene derivative and 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline.
[0137] Exemplarily, the first transport layer is an electron transport layer, and the second transport layer is a hole transport layer; or, the first transport layer is a hole transport layer, and the second transport layer is an electron transport layer.
[0138] S170: Prepare a second electrode layer on the side of the photoactive layer away from the substrate, see Fig.12 .
[0139] Exemplarily, the second electrode layer is located on a side of the second transmission layer away from the substrate.
[0140] In one embodiment, preparing the second electrode layer on the side of the photoactive layer away from the substrate includes: preparing the second electrode layer on the side of the photoactive layer away from the substrate by thermal evaporation.
[0141] In one embodiment, the preparation of the photoactive layer on the side of the second oxide layer away from the substrate, the preparation of the second transport layer on the side of the photoactive layer away from the substrate, and the preparation of the second electrode layer on the side of the photoactive layer away from the substrate are performed in the same device, illustratively, in the same thermal evaporation device. Thus, the photoactive layer, the second transport layer, and the second electrode layer are prevented from being exposed to air and water during the preparation process, thereby improving the reliability of the film layer.
[0142] In a specific embodiment, a first oxide layer is prepared on one side of the substrate, a first metal layer is prepared on the side of the first oxide layer away from the substrate by ion beam assisted deposition, a second metal layer is prepared on the side of the first metal layer away from the substrate, a second oxide layer is prepared on the side of the second metal layer away from the substrate, a photoactive layer is prepared on the side of the second oxide layer away from the substrate, and a second electrode layer is prepared on the side of the photoactive layer away from the substrate. All of them adopt a coating process, which can avoid contact with water and oxygen in the air during the preparation process, avoid device degradation caused by water absorption and oxidation of each film layer, and avoid the use of solvents, which is environmentally friendly.
[0143] In a specific embodiment, after preparing the first oxide layer in the electron beam evaporation equipment, the product is transferred to the magnetron sputtering and ion beam combined equipment to prepare the first metal layer and the second metal layer; after the second metal layer is prepared, the product is transferred to the electron beam evaporation equipment to prepare the second oxide layer; after the second oxide layer is prepared, the product is transferred to the magnetron sputtering equipment to prepare the first transmission layer; after the first transmission layer is prepared, the product is transferred to the thermal evaporation equipment to prepare the photoactive layer, the second transmission layer and the second electrode layer. The electron beam evaporation equipment, the magnetron sputtering and ion beam combined equipment, the magnetron sputtering equipment and the evaporation equipment are interconnected, which can ensure that the entire solar cell module is prevented from contacting with the outside air during the preparation process, reduce the erosion of water and oxygen on the film layers of the solar cell module, and facilitate the acquisition of a solar cell module with higher performance.
[0144] In the preparation method of the solar cell module of the embodiment of the present application, the ion beam has a certain bombardment effect on the first metal layer through auxiliary deposition, so that the first metal layer is relatively dense, which is beneficial to the subsequent growth of the second metal layer, and is beneficial to obtaining a dense, complete and thin second metal layer, thereby making the electrode layer formed by the stacked first oxide layer, the first metal layer, the second metal layer and the second oxide layer have a higher transmittance, lower surface resistance and stronger mechanical flexibility, thereby facilitating the acquisition of a solar cell module that is resistant to bending, has high transparency and high photoelectric conversion efficiency (Power Conversion Efficiency, referred to as PCE).
[0145] In a specific embodiment, the method for preparing a solar cell assembly comprises the following steps:
[0146] S1. Select colorless polyimide (CPI) with a side length of 1 cm to 10 cm (for example, 1 cm, 5 cm or 10 cm) as a flexible substrate, ultrasonically clean it with acetone for 30 min, ultrasonically clean it with ethanol for 30 min, ultrasonically clean it with deionized water for 30 min, and dry it in an oven at 70°C.
[0147] S2. Place the cleaned substrate into the electron beam evaporation chamber and evacuate to 10 -3 pa~10 -4 pa, evaporate one of the three zinc oxide (ZnO), tungsten oxide (WO3), and molybdenum oxide (MoO3), and the rate is controlled at The single layer film thickness is 5nm to 50nm and is used to prepare the first oxide layer.
[0148] S3, the substrate coated with the first oxide layer is moved into the combined magnetron sputtering and ion beam equipment, and the vacuum chamber pressure is 10 -3 ~10 -6 pa, the sputtering gas is argon, and the sputtering pressure is 0.1-2 Pa. The ion source discharge current is 0.1-3A, the DC voltage is 120V, and a 0.5-3nm thin silver first metal layer is deposited under the assistance of the ion beam. Subsequently, the ion beam assistance is cancelled and the thickness of the sputtered silver is 1-10nm to prepare the second metal layer.
[0149] S4, move the substrate coated with the second metal layer into the electron beam evaporation chamber, and adjust the vacuum degree to 10- 3 pa~10 -4 pa, evaporate one of the three zinc oxide (ZnO), tungsten oxide (WO3), and molybdenum oxide (MoO3), and the rate is controlled at The single-layer film has a thickness of 5nm to 50nm and is used to prepare the second oxide layer. The first oxide layer / first metal layer / second metal layer / second oxide layer together constitute the OMO flexible electrode.
[0150] S5. Move the substrate coated with the OMO flexible electrode into the magnetron sputtering equipment, inject argon and oxygen, the oxygen ratio is 0.01% to 2%, the gas pressure is controlled at 1 to 8 mTorr, the power is 100 to 500 W, and the thickness of the sputtered nickel oxide is 5 to 40 nm, so as to prepare a hole transport layer.
[0151] S6, move the substrate coated with the hole transport layer into a thermal evaporation device, adopt single-source evaporation, and the evaporation material is at least two of the four types of lead iodide (PbI2), cesium iodide (CsI), methylamine iodide (MAI), and formamidine iodide (FAI), among which lead iodide must be present, and the evaporation rate is controlled at The perovskite components are regulated by controlling the thickness of the film layer. Lead iodide, cesium iodide, methylamine iodide, and formamidine iodide are sequentially vapor-deposited on the substrate. The thickness of a single layer of material is 0.5 to 30 nm, and there are 2 to 10 groups in total (each group includes at least one layer of lead iodide material layer). The total film thickness is 200 to 800 nm. After the vapor deposition is completed, annealing is performed at 100 to 300°C in a chamber for 2 to 30 minutes to prepare a perovskite active layer.
[0152] S7, evaporate one or more of C60, PCBM, and BCP on the surface of the perovskite active layer away from the substrate, and control the evaporation rate to In this way, an electron transport layer is prepared.
[0153] S8. Replace the mask and evaporate any one of gold, silver, copper and aluminum as the second electrode layer to obtain a solar cell module.
[0154] The second aspect of the present application provides a method for preparing a solar cell module, referring to Fig.13 The schematic flow chart of the preparation method of the solar cell assembly shown is a schematic flow chart of the preparation method of the solar cell assembly, and the preparation method comprises the following steps.
[0155] S210: providing a substrate.
[0156] It should be noted that the substrate is consistent with the previous description and will not be elaborated here.
[0157] S220: preparing a first electrode layer on one side of the substrate.
[0158] It should be noted that the first electrode layer includes a first oxide layer, a first metal layer, a second metal layer and a second oxide layer which are stacked. The first oxide layer, the first metal layer, the second metal layer and the second oxide layer and their preparation methods are consistent with the previous description and will not be elaborated here.
[0159] S230: preparing a plurality of stacked photoactive material layers on a side of the first electrode layer away from the substrate, wherein the material of each photoactive material layer is a single material.
[0160] It should be noted that the photoactive material layer is consistent with the above description and will not be described in detail here.
[0161] S240: performing annealing treatment on the multiple photoactive material layers to obtain a photoactive layer.
[0162] It should be noted that the annealing treatment and the photoactive layer are consistent with the previous description and will not be elaborated herein.
[0163] S250: preparing a second electrode layer on a side of the photoactive layer away from the substrate.
[0164] It should be noted that the second electrode layer is consistent with the above description and will not be elaborated herein.
[0165] In one embodiment, preparing a stacked multi-layer photoactive material layer on a side of the first electrode layer away from the substrate includes: using one or more of cesium iodide, methylamine iodide and formamidine iodide and lead iodide as raw materials, and using a thermal evaporation method to prepare a stacked multi-layer photoactive material layer on a side of the first electrode layer away from the substrate. Thus, using a thermal evaporation method to prepare a stacked single-material photoactive material layer can avoid the use of solvents, which is environmentally friendly, and the photoactive material layer will hardly be corroded by water and oxygen during the preparation process, thereby ensuring the reliability of the photoactive material layer; moreover, by controlling the thickness of each layer of the photoactive material layer, the proportion and composition of the perovskite are controlled, and there is no need to accurately control the evaporation speed of different materials, thereby reducing the difficulty of preparing the perovskite.
[0166] It can be understood that when the photoactive material layer is prepared using methylamine iodide and / or formamidine iodide as raw materials, since methylamine iodide and formamidine iodide contain organic ligands, the obtained photoactive material layer is smoother and more flexible, thereby making the photoactive layer have higher flatness and flexibility, and making the PCE efficiency of the solar cell module higher.
[0167] In one embodiment, each photoactive material layer is prepared by single-source evaporation, and the thickness of each photoactive material layer is 0.5nm to 30nm (for example, it can be 0.5nm, 1nm, 5nm, 10nm, 15nm, 20nm, 25nm or 30nm, etc.), and the thickness of the photoactive layer is 200nm to 800nm (for example, it can be 200nm, 300nm, 400nm, 500nm, 600nm, 700nm or 800nm, etc.). Thus, by controlling the thickness of each photoactive material layer, the proportion and composition of perovskite in the photoactive layer can be regulated, and the overall thickness of the photoactive layer is easy to control; the single-source evaporation method reduces the equipment cost requirements and can successfully prepare high-quality perovskite films.
[0168] For example, before preparing the stacked multi-layer photoactive material layer on the side of the first electrode layer away from the substrate by thermal evaporation, the vacuum degree in the device is adjusted to 10 -4 Pa~10 -5 Pa (for example, it can be 10 -4 Pa, 10 - 4.5 Pa and 10 -5 Pa, etc.), thereby being more conducive to obtaining a photoactive layer with higher flatness and higher quality.
[0169] In one embodiment, the conditions for annealing the multi-layer photoactive material layer include: an annealing temperature of 100° C. to 300° C. (e.g., 100° C., 200° C., or 300° C.), and an annealing time of 2 minutes to 30 minutes (e.g., 2 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, or 30 minutes). Thus, the annealing conditions are suitable, which is conducive to obtaining a perovskite with uniform composition.
[0170] Exemplarily, the photoactive layer is produced in a thermal evaporation apparatus.
[0171] The third aspect of the present application provides a solar cell assembly, comprising: a substrate; a first electrode layer, located on one side of the substrate, the first electrode layer comprising a first oxide layer, a first metal layer, a second metal layer and a second oxide layer, the first oxide layer being located on a side of the first metal layer close to the substrate; a photoactive layer, located on a side of the first electrode layer away from the substrate; a second electrode layer, located on a side of the photoactive layer away from the substrate; the surface resistance of the first electrode layer is 5Ω to 35Ω (for example, it can be 5Ω, 10Ω, 15Ω, 20Ω, 25Ω, etc.);
[0172] Ω, 30Ω, etc.). As a result, the first electrode layer has a smaller surface resistance, a thinner thickness, and a higher light transmittance, which is conducive to obtaining a solar cell module with higher efficiency.
[0173] In one embodiment, the surface resistance of the first electrode layer is 5Ω to 10Ω. Therefore, the first electrode layer has a smaller surface resistance, a thinner thickness, and a higher light transmittance, which is conducive to obtaining a solar cell module with higher efficiency.
[0174] In one embodiment, the thickness of the first metal layer is 0.5 nm to 3 nm (for example, 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm or 3 nm, etc.). Thus, the thickness of the first metal layer is relatively thin, which is conducive to controlling costs, and the light transmittance is relatively high. At the same time, the subsequent second metal layer can be continuously grown on the surface of the first metal layer, which is conducive to obtaining a first electrode layer with low surface resistance.
[0175] In one embodiment, the thickness of the second metal layer is 1 nm to 10 nm (for example, 1 nm, 3 nm, 5 nm, 7 nm, 9 nm or 10 nm, etc.) Thus, the thickness of the second metal layer is relatively thin, which is conducive to obtaining a first electrode layer with a higher light transmittance, thereby facilitating the improvement of the PCE efficiency of the solar cell module.
[0176] In one embodiment, the first metal layer includes one or more of silver, gold and copper; and the second metal layer includes silver.
[0177] In one embodiment, the transmittance of the first electrode layer to light with a wavelength of 400 to 800 nm is 70 to 90% (for example, it may be 70%, 80% or 90%, etc.). Thus, the light transmittance of the first electrode layer is relatively high, which is beneficial to improving the utilization rate of the perovskite solar cell module to the wavelength of 400 to 800 nm and improving the PCE efficiency of the solar cell module.
[0178] A fourth aspect of the present application provides a solar cell, including the solar cell module prepared by the above-mentioned preparation method, or including the above-mentioned solar cell module.
[0179] It is understandable that the solar cell mentioned above, in addition to the solar cell assembly mentioned above, may also include structures that a conventional solar cell should have, such as a packaging structure, a housing, etc., which will not be elaborated herein.
[0180] For example, the above-mentioned solar cells can be applied to scenarios such as BIPV, CIPV and wearable devices.
[0181] The solar cell assembly of the present application is further described below in conjunction with specific embodiments. It should be noted that the following embodiments are only used to explain the present application and cannot be understood as limiting the present application.
[0182] Example 1
[0183] The method for preparing a solar cell module comprises the following steps:
[0184] S1. Select colorless polyimide (CPI) with a side length of 5 cm as a flexible substrate, ultrasonically clean it with acetone for 30 min, ultrasonically clean it with ethanol for 30 min, ultrasonically clean it with deionized water for 30 min, and dry it in an oven at 70°C.
[0185] S2. Place the cleaned substrate into the electron beam evaporation chamber and evacuate to 10 -4 pa, evaporation of zinc oxide (ZnO), the rate is controlled at The film thickness is 30nm and is used to prepare the first oxide layer.
[0186] S3, the substrate coated with the first oxide layer is moved into the combined magnetron sputtering and ion beam equipment, and the vacuum chamber pressure is 10 -6 pa, the sputtering gas is argon, and the sputtering pressure is 1 pa. The ion source discharge current is 2A, the DC voltage is 120V, and a 2nm thin silver first metal layer is deposited under the assistance of the ion beam. Subsequently, the ion beam assistance is cancelled and the thickness of the sputtered silver is 10nm to prepare the second metal layer.
[0187] S4, move the substrate coated with the second metal layer into the electron beam evaporation chamber, and adjust the vacuum degree to 10- 4 pa, evaporation of molybdenum oxide (MoO3), the rate is controlled at The single-layer film has a thickness of 30 nm and is used to prepare the second oxide layer. The first oxide layer / first metal layer / second metal layer / second oxide layer together constitute the OMO flexible electrode.
[0188] S5. Move the substrate coated with the OMO flexible electrode into the magnetron sputtering equipment, inject argon and oxygen, the oxygen ratio is 2%, the gas pressure is controlled at 4mTorr, the power is 300W, and the thickness of the sputtered nickel oxide is 20nm, so as to prepare the hole transport layer.
[0189] S6, the substrate coated with the hole transport layer is moved into the thermal evaporation equipment, and lead iodide (PbI2), cesium iodide (CsI) and formamidine iodide (FAI) are alternately evaporated in sequence by single-source evaporation, and the evaporation rate is controlled at The thickness of the single-layer material is 20 nm, and the total film thickness is 600 nm. After the evaporation is completed, annealing is performed at 200° C. in a chamber for 20 minutes to prepare a perovskite active layer.
[0190] S7, evaporate BCP on the surface of the perovskite active layer away from the substrate, and control the evaporation rate to In this way, an electron transport layer is prepared.
[0191] S8, replacing the mask, vapor-depositing aluminum as the second electrode layer, and obtaining a solar cell module.
[0192] Example 2
[0193] The method for preparing the solar cell assembly in this embodiment is basically the same as that in Embodiment 1, except that the thickness of the second metal layer is 7 nm.
[0194] Example 3
[0195] The method for preparing the solar cell assembly in this embodiment is basically the same as that in Embodiment 1, except that the thickness of the second metal layer is 4 nm.
[0196] Example 4
[0197] The method for preparing the solar cell assembly in this embodiment is basically the same as that in Embodiment 1, except that the thickness of the second metal layer is 1 nm.
[0198] Example 5
[0199] The method for preparing the solar cell assembly in this embodiment is basically the same as that in Embodiment 1, except that the raw material of the first metal layer is gold.
[0200] Example 6
[0201] The preparation method of the solar cell assembly in this embodiment is basically the same as that in Embodiment 1, except that the raw material of the second metal layer is copper.
[0202] Comparative Example 1
[0203] The preparation method of the solar cell assembly in this comparative example is basically the same as that in Example 1, except that the first metal layer is not prepared, and the thickness of the second metal layer is 12 nm.
[0204] Comparative Example 2
[0205] The preparation method of the solar cell assembly in this comparative example is basically the same as that in Example 2, except that the first metal layer is not prepared and the thickness of the second metal layer is 9 nm.
[0206] Comparative Example 3
[0207] The preparation method of the solar cell assembly in this comparative example is basically the same as that in Example 3, except that the first metal layer is not prepared and the thickness of the second metal layer is 6 nm.
[0208] Comparative Example 4
[0209] The preparation method of the solar cell assembly in this comparative example is basically the same as that in Example 4, except that the first metal layer is not prepared and the thickness of the second metal layer is 3 nm.
[0210] Comparative Example 5
[0211] The preparation method of the solar cell module in this comparative example is basically the same as that in Example 1, except that steps S2 to S4 are not performed, and the OMO flexible electrode is replaced by an ITO electrode.
[0212] The anti-bending effect test is as follows: use a force of 300N to bend the solar cell module back and forth 90°, and measure the PCE efficiency of the solar cell module after being bent 1000 times.
[0213] The surface resistance of the OMO flexible electrode in Examples 1 to 6 and Comparative Examples 1 to 5, the light transmittance of the OMO flexible electrode (the average transmittance of light with a wavelength of 400 to 800 nm), the initial PCE efficiency of the solar cell module, and the anti-bending effect (PCE efficiency after bending 1000 times) are shown in Table 1 below:
[0214] Table 1
[0215]
[0216] It can be seen from the data of Examples 1 to 4 and Comparative Examples 1 to 4 that the presence of the first metal layer is more conducive to reducing the surface resistance of the OMO flexible electrode and makes the surface resistance of the OMO flexible electrode more resistant to bending.
[0217] It can be seen from the data of Example 1 and Example 6 that when the second metal layer is silver, the surface resistance of the OMO flexible electrode is lower and the PCE efficiency of the solar cell module is higher.
[0218] It can be seen from the data of Example 1 and Example 5 that when the second metal layer is silver, the performance of the solar cell module is equivalent when the first metal layer is gold and silver respectively, proving that the presence of the first metal layer enables the silver second metal layer to grow continuously, which is beneficial to reducing the surface resistance of the OMO flexible electrode.
[0219] The basic principles of the present application are described above in conjunction with specific embodiments. However, it should be noted that the advantages, strengths, effects, etc. mentioned in the present application are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. are required by each embodiment of the present application. In addition, the specific details disclosed above are only for the purpose of illustration and ease of understanding, not for limitation, and the above details do not limit the present application to being implemented by adopting the above specific details.
[0220] The above description has been given for the purpose of illustration and description. In addition, this description is not intended to limit the embodiments of the present application to the forms disclosed herein. Although multiple example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, changes, additions and sub-combinations thereof.
Claims
1. A method for preparing a solar cell module, It is characterized in that include: providing a substrate; forming a first oxide layer on one side of the substrate; preparing a first metal layer on a side of the first oxide layer away from the substrate by ion beam assisted deposition; preparing a second metal layer on a side of the first metal layer away from the substrate; forming a second oxide layer on a side of the second metal layer away from the substrate; preparing a photoactive layer on a side of the second oxide layer away from the substrate; A second electrode layer is formed on a side of the photoactive layer away from the substrate.
2. The preparation method according to claim 1, It is characterized in that The step of preparing the first metal layer on the side of the first oxide layer away from the substrate by ion beam assisted deposition comprises: preparing the first metal layer on the side of the first oxide layer away from the substrate by magnetron sputtering under ion beam assisted conditions; Preferably, the step of preparing the first metal layer on the side of the first oxide layer away from the substrate by magnetron sputtering under ion beam assistance includes one or more of the following conditions: The ion source discharge current is 0.1A~3A; DC voltage is 110V~130V; The ion beam assisted ion source includes argon ions; the vacuum degree before deposition is 10 -3 Pa~10 -6 Pa; The raw materials include one or more of silver, gold and copper; Sputtering pressure is 0.1pa~2pa; The deposition rate of the first metal layer is and, The thickness of the first metal layer is 0.5nm to 3nm; Preferably, a first oxide layer is prepared on one side of the substrate, a first metal layer is prepared on the side of the first oxide layer away from the substrate by ion beam assisted deposition, a second metal layer is prepared on the side of the first metal layer away from the substrate, a second oxide layer is prepared on the side of the second metal layer away from the substrate, a photoactive layer is prepared on the side of the second oxide layer away from the substrate, and a second electrode layer is prepared on the side of the photoactive layer away from the substrate, all using a plating process.
3. The preparation method according to claim 1, It is characterized in that Preparing a second metal layer on a side of the first metal layer away from the substrate comprises: preparing the second metal layer on a side of the first metal layer away from the substrate by magnetron sputtering; Preferably, preparing the second metal layer on the side of the first metal layer away from the substrate by magnetron sputtering includes one or more of the following conditions: The vacuum degree before deposition was 10 -3 Pa~10 -6 Pa; Sputtering gases include argon; Sputtering pressure is 0.1Pa~2Pa; The raw materials include silver; and, The thickness of the second metal layer is 1nm to 10nm; Preferably, the preparation of the first metal layer on the side of the first oxide layer away from the substrate and the preparation of the second metal layer on the side of the first metal layer away from the substrate are performed in the same device by ion beam assisted deposition.
4. The preparation method according to claim 1, It is characterized in that Preparing a photoactive layer on a side of the second oxide layer away from the substrate comprises: On the side of the second oxide layer away from the substrate, a plurality of photoactive material layers are stacked, wherein the material of each photoactive material layer is a single material; Annealing the multiple photoactive material layers to obtain the photoactive layer; Preferably, preparing a stacked multi-layer photoactive material layer on a side of the second oxide layer away from the substrate comprises: using one or more of cesium iodide, methylamine iodide and formamidine iodide and lead iodide as raw materials, and preparing a stacked multi-layer photoactive material layer on a side of the second oxide layer away from the substrate by thermal evaporation; Preferably, the multi-layer photoactive material layer stacked on the side of the second oxide layer away from the substrate by thermal evaporation satisfies the following conditions: the vacuum degree before evaporation is 10 -4 Pa~10 -5 Pa; Preferably, each photoactive material layer is prepared by single-source evaporation, the thickness of each photoactive material layer is 0.5 nm to 30 nm, and the thickness of the photoactive layer is 200 nm to 800 nm; Preferably, the conditions for annealing the multiple photoactive material layers include: an annealing temperature of 100° C. to 300° C., and an annealing time of 2 minutes to 30 minutes.
5. The preparation method according to claim 1, It is characterized in that Preparing a first oxide layer on one side of the substrate includes: preparing the first oxide layer on one side of the substrate by electron beam evaporation; Preferably, preparing the first oxide layer on one side of the substrate by electron beam evaporation includes one or more of the following conditions: The vacuum degree before evaporation is 10 -3 Pa~10 -4 Pa; The raw materials include one or more of zinc oxide, tungsten oxide and molybdenum oxide; The evaporation rate is controlled as and, The thickness of the first oxide layer is 5nm to 50nm; Preferably, preparing the second oxide layer on the side of the second metal layer away from the substrate comprises: preparing the second oxide layer on the side of the second metal layer away from the substrate by electron beam evaporation; Preferably, preparing the second oxide layer on the side of the second metal layer away from the substrate by electron beam evaporation includes one or more of the following conditions: The vacuum degree before deposition was 10 -3 Pa~10 -4 Pa; The raw materials include one or more of zinc oxide, tungsten oxide and molybdenum oxide; The evaporation rate is controlled as and, The thickness of the second oxide layer is 5nm to 50nm; Preferably, after preparing a second oxide layer on a side of the second metal layer away from the substrate and before preparing a photoactive layer on a side of the second oxide layer away from the substrate, the method further comprises: preparing a first transmission layer on a side of the second oxide layer away from the substrate; Preferably, preparing the first transmission layer on the side of the second oxide layer away from the substrate comprises: preparing the first transmission layer on the side of the second oxide layer away from the substrate by magnetron sputtering; Preferably, preparing the first transmission layer on the side of the second oxide layer away from the substrate by magnetron sputtering includes one or more of the following conditions: The atmosphere is a mixture of inert gas and oxygen, with oxygen accounting for 0.01% to 2%; The air pressure is 1mTorr~8mTorr; The deposition rate of the first transport layer is and, Thickness is 5nm~40nm; Preferably, after preparing a photoactive layer on a side of the second oxide layer away from the substrate and before preparing a second electrode layer on a side of the photoactive layer away from the substrate, the method further comprises: Prepare a second transmission layer on a side of the photoactive layer away from the substrate; Preferably, preparing the second transmission layer on the side of the photoactive layer away from the substrate comprises: preparing the second transmission layer on the side of the photoactive layer away from the substrate by thermal evaporation; Preferably, the conditions for preparing the second transmission layer on the side of the photoactive layer away from the substrate by thermal evaporation include: the evaporation rate is Preferably, preparing the second electrode layer on the side of the photoactive layer away from the substrate comprises: preparing the second electrode layer on the side of the photoactive layer away from the substrate by thermal evaporation; Preferably, preparing a photoactive layer on a side of the second oxide layer away from the substrate, preparing a second transport layer on a side of the photoactive layer away from the substrate, and preparing a second electrode layer on a side of the photoactive layer away from the substrate are carried out in the same device.
6. A method for preparing a solar cell module, It is characterized in that include: providing a substrate; preparing a first electrode layer on one side of the substrate; Preparing a stacked arrangement of multiple photoactive material layers on a side of the first electrode layer away from the substrate, wherein the material of each photoactive material layer is a single material; Annealing the multiple photoactive material layers to obtain a photoactive layer; A second electrode layer is formed on a side of the photoactive layer away from the substrate.
7. The preparation method according to claim 6, It is characterized in that Preparing a stacked multilayer photoactive material layer on a side of the first electrode layer away from the substrate comprises: using one or more of cesium iodide, methylamine iodide and formamidine iodide and lead iodide as raw materials, and using a thermal evaporation method to prepare a stacked multilayer photoactive material layer on a side of the first electrode layer away from the substrate; Preferably, the multi-layer photoactive material layer stacked on the side of the first electrode layer away from the substrate by thermal evaporation satisfies the following conditions: the vacuum degree before evaporation is 10 -4 Pa~10 -5 Pa; Preferably, each photoactive material layer is prepared by single-source evaporation, the thickness of each photoactive material layer is 0.5 nm to 30 nm, and the thickness of the photoactive layer is 200 nm to 800 nm; Preferably, the conditions for annealing the multiple photoactive material layers include: an annealing temperature of 100° C. to 300° C., and an annealing time of 2 minutes to 30 minutes.
8. A solar cell module, It is characterized in that include: substrate; a first electrode layer, located on one side of the substrate, the first electrode layer comprising a first oxide layer, a first metal layer, a second metal layer and a second oxide layer, the first oxide layer being located on a side of the first metal layer close to the substrate; A photoactive layer, located on a side of the first electrode layer away from the substrate; A second electrode layer is located on a side of the photoactive layer away from the substrate; The surface resistance of the first electrode layer is 5Ω to 35Ω.
9. The solar cell module according to claim 8, It is characterized in that The surface resistance of the first electrode layer is 5Ω to 10Ω; Preferably, the thickness of the first metal layer is 0.5 nm to 3 nm; Preferably, the thickness of the second metal layer is 1 nm to 10 nm; Preferably, the first metal layer comprises one or more of silver, gold and copper; Preferably, the second metal layer comprises silver; Preferably, the transmittance of the first electrode layer to light with a wavelength of 400 to 800 nm is 70 to 90%.
10. A solar cell, It is characterized in that The invention comprises a solar cell module prepared by the preparation method according to any one of claims 1 to 7, or comprises a solar cell module according to claim 8 or 9.