Solar cell, solar cell module and electric device
The light absorption layer of perovskite photovoltaic cells is prepared by contactless sealed annealing container, which solves the problems of grain size and grain boundary defects caused by perovskite photovoltaic cells due to heat inhomogeneity, and improves energy conversion efficiency and open circuits. Voltage.
Patent Information
- Application Number
- CN202310587850.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
During the annealing process, existing perovskite photovoltaic cells have different grain sizes due to heat inhomogeneity, which increases grain boundary defects and reduces energy conversion efficiency and open circuit voltage.
The light absorption layer is prepared by contactless sealed annealing container, and the overall particle size of perovskite-type compound grains is controlled from 1 μm to 6 μm, reducing the number of grain boundaries, using polar aprotic solvent annealing atmosphere and regulating the annealing temperature and time to improve the Crystallization mass.
It improves light capture capability and carrier transport capability, reduces interface defects, and improves the energy conversion efficiency and open circuit voltage of solar cells.
Smart Images

Figure CN119031811A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cell devices, and in particular to a solar cell, a solar cell assembly and an electrical device. Background Art
[0002] Green and environmentally friendly recycling and renewable energy is the key direction of future energy technology development. Solar cells based on perovskite photovoltaic cells can directly convert solar energy into electrical energy under sunlight, and are a new energy technology that is receiving more and more attention.
[0003] For perovskite photovoltaic cells, how to improve the overall performance is the key research direction. Summary of the invention
[0004] The purpose of the present application is to provide a solar cell that can improve the internal electric field strength of the solar cell, increase the open circuit voltage, and improve its energy conversion efficiency; the purpose of the present application is also to provide a solar cell module and an electrical device comprising the solar cell, so that it can obtain improved internal electric field strength, open circuit voltage, and improve its energy conversion efficiency.
[0005] In a first aspect, an embodiment of the present application provides a solar cell, comprising a light absorbing layer,
[0006] The light absorbing layer comprises a plurality of perovskite compound grains, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is ≥90%.
[0007] According to the technical solution of the embodiment of the present application, the light absorbing layer contains perovskite compound grains with a grain length of 1 μm to 6 microns in at least one cross section perpendicular to the layer thickness direction, and the cumulative distribution rate of the number of perovskite compound grains is ≥90%, thereby improving the crystallization quality of the perovskite compound grains in the light absorbing layer, including the overall particle size, and obtaining properties such as efficient light capture capability, ultrafast carrier transport capability, and inhibition of ion migration. During the power generation process of the solar cell, the overall particle size of the perovskite compound grains is relatively large, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and promotes charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including the energy conversion efficiency.
[0008] In addition, the open circuit voltage is affected by the minimum energy required to excite electrons and the energy gap of the semiconductor material itself. When the energy gap is higher, the open circuit voltage will increase, and the number of photons required will also decrease. In the process of power generation of solar cells, the larger the particle size of the perovskite compound grains, the more favorable it is for having a suitable energy gap, improving the light capture ability, and reducing the number of photons required, which is conducive to increasing the open circuit voltage.
[0009] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.0 μm to 5.0 μm is ≥ 75%.
[0010] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.0 μm to 3.5 μm is ≥50%.
[0011] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D greater than or equal to 3.5 μm is 5%-30%.
[0012] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.5 μm to 3.0 μm is ≥ 60%.
[0013] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 1.0 μm to 2.5 μm is 20%-40%.
[0014] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm is ≤8%. According to the embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm is within the above range, indicating that the proportion of perovskite compound grains of the above particle size in the entire cross section is within a suitable range, and the proportion of smaller grains is small, which improves the uniformity of the grain size of the entire light absorbing layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the operation of the solar cell.
[0015] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 6 μm are polygonal. The contact between the grains of the above shape is good, the porosity is small, which is conducive to improving the transmission efficiency of carriers and reducing defects between grains; when the solar cell is generating electricity, it is conducive to the stability of the operation of the solar cell and the energy conversion efficiency.
[0016] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 4 μm are N-polygons, where N is a positive integer and N is greater than 5; it can be selected from 6 to 9. According to the embodiment of the present application, the above-mentioned polygonal perovskite compound grains are closely connected to each other, which is conducive to improving the transmission efficiency of carriers and reducing the influence of grain boundary defects; during the power generation process of the solar cell, it is conducive to the stability of the operation of the solar cell and the energy conversion efficiency.
[0017] In any embodiment of the present application, the light absorbing layer contains perovskite compound grains running through the light absorbing layer in at least one cross section in the layer thickness direction. The perovskite compound grains running through the light absorbing layer can be in direct contact with the first carrier transport layer and the second carrier transport layer, which can reduce interface defects between the light absorbing layer and the first carrier transport layer and the second carrier transport layer, respectively, reduce non-radiative recombination losses between interfaces, reduce or avoid current transmission limitations, and improve the current intensity and energy conversion efficiency of the battery.
[0018] In any embodiment of the present application, the ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is 50% to 90%, and can be 60% to 85%. The ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is within the above range, which can further reduce the interface defects between the light absorbing layer and the first carrier transport layer and the second carrier transport layer, respectively, reduce the non-radiative recombination loss between the interfaces, reduce or avoid the limitation of current transmission, and improve the current intensity and energy conversion efficiency of the battery.
[0019] In any embodiment of the present application, the perovskite compound grains include primary grains and secondary grains, and the number of the secondary grains accounts for 80%-100% of the total number of the perovskite compound grains, and can be optionally 65%-95%.
[0020] In any embodiment of the present application, the solar cell includes a first carrier transport layer and a second carrier transport layer, and the solar cell includes:
[0021] A passivation layer between the light absorption layer and the first carrier transport layer and / or a passivation layer between the light absorption layer and the second carrier transport layer; wherein the passivation layer is used to reduce defects when the two interfaces are in contact. The passivation layer is conducive to the ohmic transport of carriers, reduces the interface charge transport barrier caused by the poor interface contact caused by the polarity difference between the light absorption layer and the carrier transport layer, reduces the defect density, optimizes the energy level, promotes internal charge transfer, and is conducive to improving the energy conversion efficiency of perovskite solar cells.
[0022] In a second aspect, an embodiment of the present application provides a method for preparing a solar cell, the method comprising:
[0023] The light absorbing layer of the first aspect comprising a plurality of perovskite compound grains is prepared by a contactless sealed annealing container, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm is ≥90%.
[0024] According to the embodiment of the present application, the above-mentioned light absorption layer prepared by a contactless closed annealing container improves the crystallization quality of the perovskite compound grains in the light absorption layer, including the overall particle size, and can obtain high-efficiency light capture capability, ultrafast carrier transport capability, and ion migration inhibition and other performances; during the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and can promote charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including the energy conversion efficiency.
[0025] In any embodiment of the present application, the method includes at least one of the following conditions:
[0026] 1) The sealed annealing container contains an annealing atmosphere, wherein the annealing atmosphere includes a polar aprotic solvent; optionally, the polar aprotic solvent includes at least one of N,N-dimethylformamide, 1-methyl-2-pyrrolidone, dimethyl sulfoxide, and dimethylacetamide;
[0027] 2) The annealing temperature in the closed annealing container is 100-180°C, and can be optionally 120-160°C;
[0028] 3) The annealing time in the closed annealing container is 8 to 30 minutes, and can be optionally 10 to 20 minutes.
[0029] According to the embodiments of the present application, by regulating the annealing atmosphere, annealing temperature and annealing time in the closed annealing container, the crystal quality of the perovskite compound grains including the overall particle size is comprehensively controlled, thereby improving the comprehensive performance of the solar cell including the energy conversion efficiency.
[0030] In a third aspect, an embodiment of the present application provides a solar cell assembly, comprising the solar cell of the second aspect.
[0031] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising a solar cell assembly in any one of the embodiments of the third aspect of the present application, wherein the solar cell assembly is used to provide electrical energy.
[0032] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] By reading the detailed description of the preferred embodiment below, various other advantages and benefits will become clear to those of ordinary skill in the art. The accompanying drawings are only used for the purpose of illustrating the preferred embodiment and are not to be considered as limitations of the present application. In addition, the same reference numerals are used throughout the drawings to represent the same components.
[0034] In the attached picture:
[0035] Figure 1 A schematic diagram showing the measurement of the major diameter, minor diameter and height in the cross section of the light absorbing layer in the embodiment of the present application is shown;
[0036] Figure 2 A schematic diagram of the cross-sectional structure of a solar cell provided in an embodiment of the present application is shown;
[0037] Figure 3 A schematic diagram of the cross-sectional structure of a solar cell provided in an embodiment of the present application is shown;
[0038] Figure 4 A microscopic image showing the long diameter of a perovskite compound grain in a solar cell light absorption layer provided in one embodiment of the present application is shown;
[0039] Figure 5 A microscopic image showing the long diameter of perovskite compound grains in a solar cell light absorption layer provided in another embodiment of the present application is shown;
[0040] Figure 6 A microscopic image showing the long diameter of perovskite compound grains in a solar cell light absorption layer provided in another embodiment of the present application is shown;
[0041] Figure 7 A microscopic image showing the height of perovskite compound grains in a solar cell light absorption layer provided in an embodiment of the present application is shown.
[0042] The drawings in this application are not necessarily drawn to scale. DETAILED DESCRIPTION
[0043] The following embodiments of the technical solution of the present application will be described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0045] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0046] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0047] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0048] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0049] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0050] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0051] A solar cell is a device that directly converts light energy into electrical energy through the photoelectric effect or photochemical reaction. Examples of solar cells include perovskite solar cells, which are solar cells that use perovskite compound semiconductors as light-absorbing materials and belong to the third generation of solar cells.
[0052] The perovskite compounds in perovskite solar cells absorb photons with a certain energy, causing their valence band electrons to be excited and transition to the conduction band, while leaving holes in the valence band to form bound electron-hole pairs. Such electron-hole pairs can separate into free carriers and be transmitted to the corresponding electrodes to achieve photoelectric conversion. The crystallization quality of perovskite compounds directly affects the initial efficiency and stability of perovskite solar cells, and the crystallization quality is largely affected by the annealing process. In the process of engineering mass production of perovskite solar cells, how to ensure the consistency of annealing temperature for perovskite compounds and the uniformity of the heated area is the key issue to ensure the crystallization quality.
[0053] At present, the widely used annealing process is mainly contact hot plate annealing, and the annealing mechanism is mainly heat conduction or heat radiation, that is, the surface of the hot plate is heated by the electric heating wire, and then the heat is transferred to the substrate material of the perovskite solar cell (mainly glass substrate or flexible substrate) through the hot plate surface, and finally the heat is transferred upward to the perovskite. This process will cause the following problems: First, the uniformity of heating over a large area of the perovskite layer. Traditional annealing is mainly based on hot plate annealing. The uniformity of heating of perovskite is restricted in multiple directions. One is the uniformity of the hot plate. The larger the heating area, the more difficult it is to control the temperature between different areas. Another difficult-to-control factor is that the base material of the perovskite solar cell, especially glass, deforms during the heating process. The deformation will directly lead to a large difference in the heating rate of different areas of the perovskite layer. Due to uneven heating and large temperature differences in biological organisms, the perovskite compound grains are often of different sizes and uneven size distribution, which further brings about grain boundary defects. When a solar cell containing perovskite compound grains of different sizes and uneven size distribution is used, it affects the transmission of carriers, and the grain boundary defects with more water are added, which reduces the energy conversion efficiency of the solar cell. Second, the perovskite grains prepared by the above annealing process are small (generally less than 500nm). Smaller perovskite crystals will inevitably produce a large number of grain boundaries. There are often unavoidable defects at the grain boundaries, which directly cause the open circuit voltage of the perovskite solar cell to drop, and the energy conversion efficiency is low, which seriously affects the performance of the perovskite solar cell.
[0054] In the related art, a fluctuating thermal annealing process is used to strictly control the annealing temperature and annealing cycle of the perovskite photoactive layer. The growth time of the crystallization is controlled through a short heating process, so that the grains of the perovskite active layer grow relatively orderly, and in the slow growth stage, the perovskite grains can self-assemble, making the contact between the grains denser and more uniform. However, it solves the problem of large differences in perovskite grain size or uniformity. Based on the traditional contact hot plate annealing preparation, the perovskite grains produced are small (generally less than 500nm), and a large number of grain boundaries will still be produced, which inevitably brings many defects, resulting in low efficiency and poor stability of perovskite solar cells.
[0055] In view of this, the technical solution of the embodiment of the present application provides a solar cell, which can at least improve the adverse effects of a large number of grain boundaries and grain boundary defects caused by the grain size of perovskite compound grains during the solar cell power generation process, thereby improving the energy conversion efficiency of the solar cell.
[0056] Solar Cells
[0057] In a first aspect, an embodiment of the present application provides a solar cell, comprising a light absorbing layer,
[0058] The light absorbing layer comprises a plurality of perovskite compound grains, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is ≥90%.
[0059] According to the embodiment of the present application, the long diameter D of the perovskite compound grains is measured on a cross section perpendicular to the layer thickness direction of the light absorbing layer, and the short diameter b of the perovskite compound grains can be measured optionally. The thickness h of the perovskite compound grains can be measured in the cross section in the layer thickness direction of the light absorbing layer, so the long diameter D reflects the actual long diameter of the perovskite compound grains. The long diameter can be understood as the longest particle diameter measured of the perovskite compound grains. Figure 1 shown.
[0060] According to the embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains represents the percentage of perovskite compound grains with a specific particle size in the total number of perovskite compound grains in the cross section. The percentage is calculated on a number basis. The cumulative distribution rate of the number of perovskite compound grains = the number of perovskite grains within the size range in the corresponding SEM image / the total number of perovskite grains in the corresponding SEM image × 100%.
[0061] According to the technical solution of the embodiment of the present application, the crystal defects of the perovskite compound grains themselves in the light absorption layer of the solar cell will cause non-radiative recombination of carriers, thereby causing a certain amount of energy loss and reducing the photoelectric conversion efficiency of the solar cell. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm in the present application is within the above range, which improves the crystal quality of the perovskite compound grains in the light absorption layer, including the overall particle size, and can obtain high-efficiency light capture ability, ultra-fast carrier transport ability and ion migration inhibition performance; during the power generation process of the solar cell, the overall particle size of the perovskite compound grains is large, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and can promote charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including energy conversion efficiency.
[0062] In addition, the open circuit voltage is affected by the minimum energy required to excite electrons and the energy gap of the semiconductor material itself. When the energy gap is higher, the open circuit voltage will increase, and the number of photons required will also decrease. In the process of power generation of solar cells, the larger the particle size of the perovskite compound grains, the more favorable it is for having a suitable energy gap, improving the light capture ability, and reducing the number of photons required, which is conducive to increasing the open circuit voltage.
[0063] Optionally, the long diameter D of the perovskite compound grains may be any value or range of its composition in 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm, 4.6 μm, 4.7 μm, 4.8 μm, 4.9 μm, 5.0 μm, 5.1 μm, 5.2 μm, 5.3 μm, 5.4 μm, 5.5 μm, 5.6 μm, 5.7 μm, 5.8 μm, 5.9 μm, 6.0 μm. The cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 microns may be any value or range of its composition in 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%. The long diameter D of the perovskite compound grains is within the above range, which further increases the overall particle size of the perovskite compound grains in the light absorption layer. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is within the above range. During the power generation process of the solar cell, the overall particle size of the perovskite compound grains is relatively large, which further reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and improves the energy conversion efficiency.
[0064] In some embodiments, at least one cross section of the light absorbing layer perpendicular to the layer thickness direction may be a cross section in the thickness direction of the light absorbing layer and close to its surface layer. Optionally, the cross section may be a cross section of an end face in the thickness direction of the light absorbing layer. The thickness range of the surface layer is ≤100nm, and may be ≤50nm.
[0065] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm is ≥ 75%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm can be any value or a range composed of 75%, 76%, 77%, 78%, 79%, 80%, 85%, 90%, 95%. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm is within the above range, which increases the overall particle size of the perovskite compound grains; the long diameter D of 2.0 μm to 5.0 μm increases the uniformity of the perovskite compound grain size; during the power generation process of the solar cell, the number of grain boundaries between the perovskite compound grains is reduced, the interference of interface defects is reduced or avoided, and the energy conversion efficiency is improved.
[0066] The perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm have a suitable energy gap. When the cumulative distribution rate of the number of perovskite compound grains is within the above range, the light capture capability can be improved and the open circuit voltage of the solar cell can be increased.
[0067] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 3.5 μm is ≥ 50%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 3.5 μm can be any value or a range of its composition of 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 65%, 70%, 75%, 80%, 90%, 95%.
[0068] According to the embodiments of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 3.5 μm is within the above range, thereby improving the uniformity of the grain size and the overall particle size of the perovskite compound; during the power generation process of the solar cell, the number of grain boundaries between the perovskite compound grains is reduced, the interference of interface defects is reduced or avoided, and the energy conversion efficiency is improved.
[0069] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D greater than or equal to 3.5 μm is 5%-30%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D greater than or equal to 3.5 μm can be any value or a range composed of 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 26%, 27%, 28%, 29%, 30%. According to the embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D greater than or equal to 3.5 μm is within the above range, indicating that the proportion of perovskite compound grains of the above particle size in the entire cross section is within a suitable range, and the proportion of larger grains is small, which improves the uniformity of the grain size of the entire light absorbing layer; during the power generation process of the solar cell, due to the uniformity of the grain size, it is beneficial to the stability of the operation of the solar cell.
[0070] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.5 μm to 3.0 μm is ≥ 60%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.5 μm to 3.0 μm can be any value or a range composed of 60%, 61%, 62%, 63%, 64%, 65%, 70%, 75%, 80%, 81%, 82%, 83%, 84%, 90%, 95%. According to an embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.5 μm to 3.0 μm is within the above range, which improves the uniformity of the grain size of the perovskite compound and the overall particle size; during the power generation process of the solar cell, the number of grain boundaries between the perovskite compound grains is reduced, the interference of interface defects is reduced or avoided, and the energy conversion efficiency is improved.
[0071] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm is 20%-40%. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm can be any value or a range of their composition in 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 32%, 35%, 36%, 37%, 38%, 39%, 40%. According to the embodiments of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm is within the above range, which means that the proportion of perovskite compound grains with the above particle size in the entire cross-section is within a suitable range, and the proportion of smaller grains is relatively small, thereby improving the uniformity of the grain size of the entire light absorption layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the operation of the solar cell.
[0072] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm is ≤8%. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm can be any value of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or a range composed thereof. According to an embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm is within the above range, indicating that the proportion of perovskite compound grains of the above particle size in the entire cross section is within a suitable range, and the proportion of smaller grains is relatively small, which improves the uniformity of the grain size of the entire light absorbing layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the operation of the solar cell.
[0073] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 6 μm are polygonal.
[0074] According to the embodiments of the present application, the defects in porosity or close contact between the perovskite compound grains in the light absorption layer of the solar cell will cause non-radiative recombination of carriers, thereby causing certain energy losses and reducing the photoelectric conversion efficiency of the solar cell. The contact between the grains of the above shape is better and the porosity is smaller, which is conducive to improving the transmission efficiency of carriers and reducing defects between grains; when the solar cell is generating electricity, it is beneficial to the stability of the solar cell operation and the energy conversion efficiency.
[0075] As an example, the perovskite compound grains with a long diameter D of 1 μm to 6 μm are polygonal. Figure 4-6 shown.
[0076] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 4 μm are N-gonal, where N is a positive integer and N is greater than 5; it can be optionally 6-9.
[0077] According to the embodiments of the present application, the above-mentioned polygonal perovskite compound grains are closely connected to each other, which is beneficial to improving the carrier transmission efficiency and reducing the influence of grain boundary defects; during the power generation process of the solar cell, it is beneficial to the stability of the operation of the solar cell and the energy conversion efficiency.
[0078] In some optional embodiments of the present application, the light absorbing layer contains perovskite compound grains running through the light absorbing layer in at least one cross section in the layer thickness direction.
[0079] In the embodiment of the present application, the perovskite compound grains penetrating the light absorbing layer can be measured from a cross section parallel to the thickness direction of the light absorbing layer, that is, the height h of the perovskite compound grains can be measured, such as Figure 1 As an example, the perovskite compound grains throughout the light absorbing layer are as shown in Figure 7 shown.
[0080] The carriers formed by the light excitation of the perovskite compound in the solar cell diffuse in the light absorption layer. When reaching the interface between the electron transport layer / hole transport layer and the light absorption layer, if the energy levels of the two functional layers are matched, free electrons and holes are formed under the action of the interface barrier. The defects inside the perovskite compound and at the interface of the two transport layers will cause non-radiative recombination of carriers, thereby causing a certain amount of energy loss and reducing the photoelectric conversion efficiency of the perovskite solar cell. Therefore, the perovskite compound grains running through the light absorption layer can directly contact the first carrier transport layer and the second carrier transport layer, which can reduce the interface defects between the light absorption layer and the first carrier transport layer and the second carrier transport layer, reduce the non-radiative recombination loss between the interfaces, reduce or avoid the limitation of current transmission, and improve the current intensity and energy conversion efficiency of the battery.
[0081] In some optional embodiments of the present application, the ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is 50% to 90%, and optionally 60% to 85%. The ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is within the above range, further reducing the interface defects between the light absorbing layer and the first carrier transport layer and the second carrier transport layer, further reducing or avoiding the limitation of current transmission, and improving the current intensity and energy conversion efficiency of the battery.
[0082] In some optional embodiments of the present application, the perovskite compound grains include primary grains and secondary grains, and the number of the secondary grains accounts for 80%-100% of the total number of the perovskite compound grains, and can be optionally 65%-95%.
[0083] According to the embodiments of the present application, primary grains refer to the dense, small and uniform grains obtained at the initial stage of annealing of the perovskite compound. Secondary grains refer to the primary grains that continue to anneal in a trace solvent atmosphere. According to the Oswald ripening effect, small grains are continuously dissolved to form a solute atmosphere that is absorbed by slightly larger grains due to chemical kinetics, gradually forming a large grain structure, that is, large grains with small surface energy swallow up small grains with large surface energy. Such grown grains are called secondary grains. Generally speaking, the major diameter of the primary grains ranges from about 100nm to 800nm, and the volume of the secondary grains can reach 1μm to 6μm.
[0084] In some alternative embodiments of the present application, the perovskite compound grains contain an organic-inorganic perovskite compound represented by the general formula ABX3, where A is an organic cation, B is a metal cation, and X is a halogen anion or SCN. - . In some embodiments of the present application, the halogen X includes at least one of chlorine, bromine, and iodine.
[0085] It can be understood that perovskite materials with different halogen ions have different bandgaps. The perovskite material with the halogen ion being I - has the smallest bandgap (generally about 1.5 electron volts), and the perovskite material with the halogen ion being Cl - has the largest bandgap (generally about 3 electron volts). Moreover, the perovskite material can contain two mixed halogen ions, and the mixing ratio can be continuously adjusted. Therefore, the bandgap of the perovskite material can be continuously adjusted within the range of 1.5 - 3 electron volts, corresponding to a wavelength range of the light that can be absorbed of about 414 - 820 nanometers, basically covering the entire visible light spectrum. Carriers are generated in the light absorption layer.
[0086] For example: A in ABX3 can include at least one of CH3NH 3+ and HC(NH2) 2+ ; in other words, A can be CH3NH 3 + , HC(NH2) 2+ or a mixture of the two in any proportion. It can be understood that A can also include metal ions, such as Cs + , Rb + and K + at least one of them.
[0087] For example: B in ABX3 can be at least one of Pb 2+ , Sn 2+ and Ge 2+ .
[0088] For example, ABX3 can be CH3NH3PbI3; CH3NH3SnI3; CH3NH3PbI2Cl; CH3NH3PbI2Br; CH3NH3Pb(I 1-x Br x )3 (where 0 < x < 1), and so on.
[0089] In some embodiments, the organic cation A includes at least one of an amino group and an amino group derivative. In some examples, the amino group can be an alkylamino group.
[0090] In some embodiments, the amino group includes at least one of methylamino, ethylamino, propylamino, butylamino, pentylamino, hexylamino, and formamidinyl. The amino group derivative can include an imidazolyl group.
[0091] In some embodiments, the metal in the metal cation B includes at least one of lead (Pb), cesium (Cs), tin (Sn), zinc (Zn), titanium (Ti), antimony (Sb), bismuth (Bi), nickel (Ni), iron (Fe), cobalt (Co), silver (Ag), copper (Cu), gallium (Ga), germanium (Ge), magnesium (Mg), calcium (Ca), indium (In), aluminum (Al), manganese (Mn), chromium (Cr), molybdenum (Mo) and europium (Eu). B in the general formula ABX3 is selected from the above metal cations, which can help improve the photoelectric conversion efficiency of the light absorbing layer.
[0092] Figure 2 FIG. 2 shows a schematic cross-sectional structure diagram of a solar cell according to an embodiment of the present application. Figure 2 As shown, the solar cell 10 includes the following structures stacked in sequence: a first electrode layer 11 ; a first carrier transport layer 13 ; a light absorption layer 15 ; a second carrier transport layer 14 ; and a second electrode layer 12 .
[0093] In some embodiments of the present application, the first electrode layer 11 may be made of a conductor, and the conductor has a high work function to facilitate hole injection. Exemplarily, the conductor may be a metal, a metal oxide and / or a conductive polymer.
[0094] Exemplarily, the first electrode layer 11 may be made of metal, for example, the material of the first electrode 11 includes at least one of nickel (Ni), platinum (Pt), vanadium (V), chromium (Cr), copper (Cu), zinc (Zn), gold (Au), silver (Ag) or alloys thereof. The first electrode 131 may also be made of metal oxide, for example, the material of the first electrode 131 includes at least one of zinc oxide (ZnO), indium oxide (In2O3), fluorine-doped tin oxide (FTO), indium tin oxide (ITO), nickel oxide (NiO), aluminum zinc oxide (AZO), indium zinc oxide (IZO) and gallium zinc oxide (GZO). The first electrode 131 may also be made of a conductive polymer, for example, the material of the first electrode 131 includes at least one of poly (3-methylthiophene), poly (3, 4- (ethylene-1, 2-dioxy) thiophene) (PEDOT), polypyrrole and polyaniline.
[0095] In an embodiment of the present application, the second electrode layer 12 may also be made of a conductor, and the conductor has a lower work function to facilitate the injection of electrons. Exemplarily, the material of the second electrode 12 includes at least one of copper (Cu), magnesium (Mg), aluminum (Al), nickel (Ni), silver (Ag), tin (Sn), chromium (Cr), bismuth (Bi), platinum (Pt), molybdenum (Mo), tungsten (W) or their alloys, carbon (C), graphene, carbon nanotubes, fluorine-doped tin oxide (FTO), indium tin oxide (ITO), aluminum zinc oxide (AZO), indium zinc oxide (IZO) and gallium zinc oxide (GZO).
[0096] In some embodiments, the solar cell includes a first carrier transport layer 13 and a second carrier transport layer 14 disposed on both sides of the light absorbing layer 15. The first carrier transport layer 13 and the second carrier transport layer 14 are disposed in a related manner.
[0097] The carrier selectivity corresponding to the first carrier transport layer 13 and the second carrier transport layer 14 is opposite. If the first carrier transport layer 13 has electron selectivity and the second carrier transport layer 14 has hole selectivity, after the light absorption layer 15 absorbs sunlight and generates carriers, the electrons in the carriers are selected by the first carrier transport layer 13 and transported to the first electrode layer 11, and then collected by the first electrode layer 11, and the holes after losing the electrons are selected by the second carrier transport layer 15 and their electrical properties are transmitted to the second electrode layer 12, and then collected by the second electrode layer 12, thereby realizing the separation of carriers in the perovskite compound in the light absorption layer 15.
[0098] If the first carrier transport layer 13 has hole selectivity and the second carrier transport layer 14 has electron selectivity, then after the light absorption layer 15 absorbs sunlight and generates carriers, the holes that lose electrons are selected by the first carrier transport layer 13 and their electrical properties are transmitted to the first electrode layer 11, and then collected by the first electrode layer 11, and the electrons in the carriers are selected by the second carrier transport layer 30 and transmitted to the second electrode layer 12, and then collected by the second electrode layer 12, thereby realizing the separation of carriers in the light absorption layer 15.
[0099] Furthermore, the first carrier transport layer 13 is arranged on the light-facing surface of the light absorption layer 15, and the second carrier transport layer 14 is arranged on the backlight surface of the light absorption layer 15, and the carrier selectivities corresponding to the first carrier transport layer 13 and the second carrier transport layer 15 are opposite, and the first electrode layer 11 is arranged on the side of the first carrier transport layer 13 away from the light absorption layer 15, and the second electrode layer 12 is arranged on the side of the second carrier transport layer 14 away from the light absorption layer 15, and the second electrode layer 12 and the second carrier transport layer 14 are electrically connected.
[0100] According to the embodiment of the present application, the first carrier transport layer 13 and the second carrier transport layer 14 may be a single-layer structure or a multi-layer structure, respectively.
[0101] In some embodiments of the present application, the hole-selective material includes at least one of thiophene, phthalocyanine, porphyrin, 2,2',7,7'-tetrakis(N,N-dimethoxyaniline)-9,9'-spirobifluorene, molybdenum oxide (MoO3), vanadium oxide (V2O5), tungsten oxide (WO3 and / or WO2), nickel oxide (NiO), copper oxide (CuO), tin oxide (SnO2), molybdenum sulfide (MoS2), tungsten sulfide (WS2), copper sulfide (CuS), tin sulfide (SnS), cuprous thiocyanate (CuSCN), copper iodide (CuI), fluorine-containing phosphonic acid, carbonyl-containing phosphonic acid, carbon nanotubes and graphene.
[0102] In some embodiments of the present application, the material with electron selectivity includes [6,6]-phenyl-C61-butyric acid isomethyl ester, C60, cyano-containing polyphenylene vinylene, boron-containing polymer, bathocuproine, bathophenanthroline, hydroxyquinoline aluminum, oxadiazole compounds, benzimidazole compounds, naphthalenetetracarboxylic acid compounds, perylene derivatives, phosphine oxide compounds, phosphorus sulfide compounds, fluorine-containing phthalocyanine, titanium oxide (TiO2), zinc oxide (ZnO), tin oxide (SnO2), indium oxide (In2O3), gallium oxide (Ga2O3), tin sulfide (SnS), indium sulfide (In2O3), lithium fluoride (LiF), sodium fluoride (NaF), magnesium fluoride (MgF2) and zinc sulfide (ZnS) at least one.
[0103] In some optional embodiments of the present application, the solar cell includes a first carrier transport layer and a second carrier transport layer, and the solar cell includes:
[0104] A passivation layer located between the light absorbing layer and the first carrier transport layer and / or a passivation layer located between the light absorbing layer and the second carrier transport layer. The passivation layer is used to reduce defects when the two interfaces are in contact.
[0105] Figure 3 FIG. 2 shows a schematic cross-sectional structure diagram of a solar cell according to an embodiment of the present application. Figure 3 As shown, the solar cell 10 includes the following structures stacked in sequence: a first electrode layer 11 ; a first carrier transport layer 13 ; a first passivation layer 16 ; a light absorption layer 15 ; a second passivation layer 17 ; a second carrier transport layer 14 ; and a second electrode layer 12 .
[0106] According to the embodiment of the present application, the material of the passivation layer can be commonly used in the art. As an example, the material can be methyl substituted carbazole molecules (Me-4PACz). Methyl substituted carbazole molecules (Me-4PACz) can be understood as a self-assembled molecular layer. The thickness can be 1 to 5 nm.
[0107] The light absorption layer in the solar cell absorbs energy and releases carriers to diffuse in the perovskite. When it reaches the interface between the electron transport layer / hole transport layer and the light absorption layer, the defects at the interface between the perovskite compound and the two transport layers will cause non-radiative recombination of the carriers, resulting in a certain amount of energy loss and reducing the photoelectric conversion efficiency of the perovskite solar cell. The above passivation layer is conducive to the ohmic transmission of carriers, reduces the interface charge transport barrier caused by the poor interface contact caused by the polarity difference between the light absorption layer and the carrier transport layer, reduces the defect density, optimizes the energy level, promotes internal charge transfer, and is conducive to improving the energy conversion efficiency of perovskite solar cells.
[0108] In some embodiments, the solar cell includes a substrate disposed on a side of the first electrode layer away from the second electrode layer. The substrate is made of glass or a mixture of one or more transparent organic polymers: the organic polymer includes one or more of PET (polyethylene terephthalate) and PI (polyimide).
[0109] [ Method for preparing solar cell ]
[0110] In the embodiment of the present application, the solar cell 10 may be manufactured by a method known in the art.
[0111] In some embodiments of the present application, a method for preparing a solar cell includes:
[0112] S10: providing a first electrode layer;
[0113] S20: forming a first carrier transport layer on one side of the first electrode layer;
[0114] S30: forming a light absorption layer on a side of the first carrier transport layer away from the first electrode layer;
[0115] S40: forming a second carrier transport layer on a side of the light absorbing layer away from the first carrier transport layer;
[0116] S50: forming a second electrode layer on a side of the second carrier transport layer away from the light absorption layer.
[0117] Exemplarily, the manufacturing method of the solar cell device 10 may include: forming a first carrier transport layer 13, a light absorption layer 15, a second carrier transport layer 14 and a second electrode layer 12 in order from bottom to top on a transparent or opaque first electrode layer 11. The light absorption layer 15 may be formed by known film forming methods such as evaporation, sputtering, spin coating, dipping, ion plating, etc.
[0118] The preparation process of the light absorbing layer includes three steps: wet film coating, solvent quenching and annealing.
[0119] Wet film coating includes: in the wet film coating state, the perovskite is in a colloidal state, and ABX3 is distributed in a precursor solvent and coated on a substrate.
[0120] Solvent quenching includes: quickly taking away a large amount of organic solvent in the perovskite precursor solution, leaving only a small amount of organic solvent to complex with the perovskite components. At this time, the perovskite is in an intermediate state, and the general formula is generally AX·BX2·organic solvent. The above process is the process of partial solute forming seed crystals.
[0121] Annealing includes: AX·BX2·Organic solvent will gradually lose solvent molecules to form a complete ABX3. During the annealing process, the seed crystal will absorb the residual solute that has lost the solvent molecules, thereby growing into perovskite grains. Usually, due to the constant solute content, the number of seed crystals is inversely proportional to the grain size.
[0122] In a second aspect, an embodiment of the present application provides a method for preparing a solar cell, the method comprising:
[0123] The light absorbing layer of the first aspect comprising a plurality of perovskite compound grains is prepared by a contactless sealed annealing container, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm is ≥90%.
[0124] In the related technology, contact hot plate annealing is an annealing process achieved through heat conduction. When the perovskite layer is prepared on a large scale, the temperature rises unevenly due to the warping of the glass, resulting in inconsistent growth rates of the seed crystals and different grain sizes. In addition, the number of seed crystals is large and irreversible, resulting in smaller grains (the maximum width of the grains is less than 500nm).
[0125] According to the embodiment of the present application, the above-mentioned light absorption layer prepared by a contactless closed annealing container improves the crystallization quality of the perovskite compound grains in the light absorption layer, including the overall particle size, and can obtain high-efficiency light capture capability, ultrafast carrier transport capability, and ion migration inhibition and other performances; during the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and can promote charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including the energy conversion efficiency.
[0126] In the embodiment of the present application, the contactless closed annealing container leukemia adopts a contactless closed oven for annealing to achieve uniform temperature rise of the seed crystals, and the volatile organic solvent molecules will accumulate in the annealing atmosphere to form a specific solvent annealing atmosphere, gradually dissolving the small grains, and through the Ostwald ripening effect, the large grains absorb these dissolved small grains and gradually grow into larger perovskite compound grains, with a reduced number of grain boundaries and defects. The Ostwald ripening effect is a phenomenon that can be observed in solid solutions or liquid sols, which describes the changes that occur in a non-uniform structure over time: smaller crystals or sol particles in the solute dissolve and redeposit on larger crystals or sol particles. It relies on the reduction of the specific interface energy per unit mass, the reduction of the total free energy of the system, and the spontaneous reaction.
[0127] In any embodiment of the present application, the method includes at least one of the following conditions:
[0128] 1) The sealed annealing container contains an annealing atmosphere, wherein the annealing atmosphere includes a polar aprotic solvent; optionally, the polar aprotic solvent includes at least one of N,N-dimethylformamide, 1-methyl-2-pyrrolidone, dimethyl sulfoxide, and dimethylacetamide;
[0129] 2) The annealing temperature in the closed annealing container is 100-180°C, and can be optionally 120-160°C;
[0130] 3) The annealing time in the closed annealing container is 8 to 30 minutes, and can be optionally 10 to 20 minutes.
[0131] According to the embodiments of the present application, by regulating the annealing atmosphere, annealing temperature and annealing time in the closed annealing container, the crystal quality of the perovskite compound grains including the overall particle size is comprehensively controlled, thereby improving the comprehensive performance of the solar cell including the energy conversion efficiency.
[0132] In some embodiments, the closed oven has a first heating source and a second heating source. In some embodiments, the first heating source and the second heating source can be arranged oppositely, and the space in the middle is used to accommodate the structure to be prepared. The structure to be prepared can be a stacked first electrode layer, a first carrier layer and a mixture coated on the first carrier layer, and the mixture is used to prepare a light absorption layer. The first heating source and the second heating source can themselves heat the closed oven, and can also conduct the heat of the heat source. In some embodiments, the closed oven includes a carrier, the carrier contacts the edge of the structure to be prepared, and the middle of the structure to be prepared is suspended. The position where the carrier contacts the structure to be prepared is ≤5mm from the edge of the prepared structure. In some embodiments, along the direction of the first heating source and the second heating source arranged oppositely, the width of the cross section of the first heating substrate and the second heating substrate can be 5 to 100mm, preferably 20 to 80mm. In some embodiments, the surfaces of the first heating source and the second heating source are 28-32mm, and can be 30mm, respectively, from the surface of the structure to be prepared.
[0133] Solar cell modules
[0134] In the solar cell assembly provided in the embodiment of the present application, one solar cell 10 of the first aspect may be included, or multiple solar cells of the first aspect may be included. If there are multiple solar cells, the multiple solar cells may be connected in series, in parallel, or in hybrid connection, wherein the hybrid connection means that the multiple solar cells are connected in series and in parallel.
[0135] In some embodiments, the solar cell assembly includes a protective layer and / or an encapsulation layer.
[0136] [Protective layer]
[0137] The protective layer is disposed between the encapsulation layer and the solar cell, and the protective layer contains metal halides and / or organic halides. The metal halides and organic halides in the protective layer can absorb the infiltrated water and oxygen, reduce the corrosion of water and oxygen on the organic and inorganic perovskite compounds in the light absorption layer, and thus improve the stability of the solar cell, thereby helping to extend the service life of the solar cell.
[0138] In some optional embodiments of the present application, the metal halide has the general formula BX k , wherein the value of k is in the range of 1 to 3. The organic halide has the general formula AX.
[0139] In the above embodiments, the metal halide and the organic halide respectively have the above general formula, which can enable the protective layer to absorb water and oxygen while generating substances similar to or identical to the precursor substances of the organic-inorganic perovskite compounds. These substances can react to generate perovskite compounds with functions close to those of the organic-inorganic perovskite compounds, thereby allowing the solar cell to have a longer service life when water and oxygen penetrate into it.
[0140] In some optional embodiments of the present application, the organic cation in the organic-inorganic perovskite compound and the organic cation in the organic halide are the same or are homologous to each other.
[0141] In the present application, homologues refer to organic compounds with similar structures and molecular compositions that differ by several "CH2" atomic groups.
[0142] In the above embodiments, the organic cation in the general formula ABX3 and the organic cation in the general formula AX are the same or homologous to each other, which can help the organic halide in the protective layer 15 and the precursor material to form an organic-inorganic perovskite compound.
[0143] In some optional embodiments of the present application, the organic cation includes at least one of an amine group and an amine derivative, such as an alkylamine group.
[0144] In some optional embodiments of the present application, the amine group includes at least one of methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine and carboxamidine. The amine derivative includes imidazole.
[0145] Exemplarily, when the organic cation in the organic-inorganic perovskite compound is the same as the organic cation in the organic halide, if the organic cation in the organic-inorganic perovskite compound is methylamine (CH3NH-), then the organic cation in the organic halide is also methylamine (CH3NH-).
[0146] For example, when the organic cation in the general formula ABX3 and the organic cation in the general formula AX are homologues of each other, and the organic cation in the organic-inorganic perovskite compound is methylamine (CH3NH-), the organic cation in the organic halide can be ethylamine (CH3CH2NH-) or propylamine (CH3CH2CH2NH-).
[0147] In the embodiments of the present application, the protective layer may be a single-layer structure or a multi-layer structure, and the specific number of layers may be designed according to requirements.
[0148] In some optional embodiments of the present application, the protective layer comprises at least one of MOF material, activated carbon, montmorillonite, diatomaceous earth, zeolite, molecular sieve, kaolin, ion exchange resin and 2-methylimidazole zinc salt MAF-4 to provide a porous structure.
[0149] [Encapsulation layer]
[0150] The encapsulation layer can encapsulate the solar cell between the cover plate and the substrate to protect the solar cell.
[0151] The material of some optional packaging layers in the present application includes at least one of a thermoplastic packaging adhesive, a heat-curing packaging adhesive and a light-curing packaging adhesive.
[0152] Exemplarily, the thermoplastic encapsulant includes at least one of ethylene-vinyl acetate copolymer, polyvinyl butyral, ethylene octene copolymer, polyisobutylene, polyolefin encapsulant and butyl rubber. The thermosetting encapsulant includes at least one of epoxy encapsulant, silicone encapsulant and polyurethane encapsulant. The curing encapsulant includes at least one of ultraviolet light curing encapsulant and infrared light curing encapsulant.
[0153] Electrical devices
[0154] In a third aspect, an embodiment of the present application provides an electrical device, comprising the solar cell assembly of the second aspect, wherein the solar cell assembly is used to provide electrical energy.
[0155] Electrical devices may be in, but are not limited to, the fields of construction, military, travel, national defense, power supply, etc., such as: mobile phones, tablets, laptops, electric toys, electric tools, battery vehicles, electric cars, ships, spacecraft, photovoltaic greenhouses, photovoltaic water heaters, etc.
[0156] The following examples more specifically describe the disclosure of the present application, which are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations are possible within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0157] Example 1
[0158] The present invention provides a method for manufacturing a solar cell module, which comprises the following steps:
[0159] (1) Forming a solar cell device: A set of FTO conductive glass with a specification of 30 cm×30 cm is etched with P1 using an infrared laser. The width of P1 is about 30 μm. The whole piece of glass is divided into 44 sub-cells along the long side direction. The series resistance of different sub-cells is greater than 10 MΩ. 10 mm above and below are used as the component welding area; the surface of the etched conductive glass is cleaned twice with acetone and isopropanol in turn, immersed in deionized water for ultrasonic treatment for 10 minutes, and then dried in a forced air drying oven, and placed in a drying room (humidity less than 2%) to serve as the first electrode.
[0160] The cleaned conductive glass is placed in a magnetron sputtering process to deposit a hole transport layer of nickel oxide, the thickness of the nickel oxide layer is about 15 nm;
[0161] Apply a layer of FA using slot coating 0.95 Cs 0.05 The PbI3 perovskite main layer is obtained, and then the heated substrate is transferred to the vacuum equipment for 60s, and the vacuum degree is 15Pa. At this time, the closed oven has a trace of N,N-dimethylformamide solvent atmosphere. The closed oven is used for contactless annealing, and the closed oven structure is as follows: a. The closed oven structure is an upper heating source hot plate and a lower heating source hot plate. The four walls have heat exhaust holes that can be controlled to open, close and adjust the exhaust rate. The perovskite substrate to be heated is heated upwards, and the upper heating source hot plate and the lower heating source are 30mm away from the substrate surface respectively; b. The carrier structure of the substrate to be heated is that there is no contact in the middle of the substrate, and only the four corners have a heat-insulating ejector material that contacts the edge of the substrate by 5mm, so that the substrate to be heated is suspended inside the closed oven.
[0162] The annealing process is to uniformly increase the temperature, slowly crystallize, and anneal at 150°C for 10 minutes to form a light absorption layer with a thickness of about 500nm;
[0163] The prepared device was placed in a vacuum thermal evaporation device and evacuated to 4×10- 4 Pa, deposit 30nm C 60 , 8nmBCP as the charge transport layer of the device;
[0164] After the charge transport layer was deposited in the vacuum thermal evaporation device, 10 nm Ag was deposited on the surface and then the vacuum was broken and taken out. P2 was laser etched. The width of P2 was 150 μm and the depth was etched to the surface of the FTO layer. The interval between P2 and P1 was 20 μm. Then the substrate was put into the evaporation device again and vacuumed to 4×10 -4 After Pa, a layer of Ag is continuously deposited with a thickness of about 80 nm;
[0165] After cooling, the vacuum is broken and P seconds of green laser etching P3 is performed. The width of P3 is 15 μm and the depth is etched to the surface of the FTO layer. The interval between P3 and P2 is 20 μm (the positions of the etching lines are P1 / P2 / P3 in sequence).
[0166] (3) Edge cleaning: Use a laser marking machine to clean the coating in the area extending inward from the edge of the solar cell device to 0.1 cm.
[0167] (4) Glue application: Apply the encapsulation glue to the clean edge area.
[0168] (5) Lamination: The substrate, the adhesive-bonded solar cell device, the encapsulation layer with a protective layer, and the cover plate are bonded together and laminated to obtain a solar cell module.
[0169] Embodiment 2-6
[0170] The difference between this embodiment and embodiment 1 is that the perovskite components used in the light absorption layer are different, which correspond to Table 1 for details.
[0171] Comparative Examples 1-3
[0172] The manufacturing methods of Comparative Examples 1-3 are similar to those of Example 1, except that the annealing method is to use a hot plate for direct contact annealing at 150° C. for 10 min. For details, please refer to Table 1.
[0173] Test Section
[0174] The cross section of the light absorption layer prepared in Examples 1-3 was examined by using a field emission electron scanning microscope of Gemini 360 model from Carl Zeiss Jena (ZEISS) at 3KV, with the lens at a distance of 4.9 to 5.1 mm from the sample surface, and the magnification of the surface morphology of the perovskite layer was 5K to 10K, and the magnification of the cross section was 20K. Figure 4-6 As shown in FIG. 1 , it is found that the particle size distribution of the perovskite compound grains is 1 to 6 μm. Figure 7 As shown, perovskite compound grains were found to penetrate the light absorbing layer.
[0175] Photoelectric conversion efficiency detection: At room temperature and pressure, a sunlight simulation light source is used as a standard light source of AM1.5G, and a four-channel digital source meter (Keithley 2440) is used to measure the volt-ampere characteristic curves of the solar cells prepared in the embodiment and the comparative example under the irradiation of the light source to obtain the open circuit voltage Voc, short circuit current density Jsc, fill factor FF (FillFactor), and energy conversion efficiency Eff (Efficiency) of the solar cell; the test results are shown in Table 1.
[0176] According to Table 1, by comparing the test results of Examples 1-10 and Comparative Examples 1-3, it can be seen that in the solar cells provided in the embodiments of the present application, the overall particle size of the perovskite compound grains of the embodiments is larger than the grain size of the comparative examples, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, promotes charge separation at the interface, and increases the open circuit voltage of the solar cell, thereby improving the comprehensive performance of the solar cell including the energy conversion efficiency.
[0177] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
[0178]
[0179]
Claims
1. A solar cell, characterized in that: comprising a light absorbing layer, The light absorbing layer comprises a plurality of perovskite compound grains, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is ≥90%.
2. The solar cell according to claim 1, characterized in that In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm is ≥ 75%; Optionally, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.0 μm to 3.5 μm is ≥50%.
3. The solar cell according to claim 2, characterized in that: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D greater than or equal to 3.5 μm is 5%-30%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.5 μm to 3.0 μm is ≥ 60%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 1.0 μm to 2.5 μm is 20%-40%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D less than or equal to 1.0 μm is ≤8%.
4. The solar cell according to any one of claims 1 to 3, characterized in that: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, perovskite compound crystal grains having a long diameter D of 1 μm to 6 μm are polygonal.
5. The solar cell according to any one of claims 1 to 4, characterized in that: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 4 μm are N-gonal, where N is a positive integer greater than 5; it can be 6-9.
6. The solar cell according to any one of claims 1 to 5, characterized in that: The light absorbing layer includes perovskite compound crystal grains penetrating the light absorbing layer in at least one cross section in a layer thickness direction.
7. The solar cell according to claim 6, characterized in that: The ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is 50% to 90%, and can be optionally 60% to 85%.
8. The solar cell according to claim 7, characterized in that: The perovskite compound grains include primary grains and secondary grains, and the number of the secondary grains accounts for 80%-100% of the total number of the perovskite compound grains, and can be 65%-95%.
9. The solar cell according to claim 7 or 8, characterized in that: The solar cell comprises a first carrier transport layer and a second carrier transport layer, and the solar cell comprises: A passivation layer located between the light absorbing layer and the first carrier transporting layer and / or a passivation layer located between the light absorbing layer and the second carrier transporting layer; wherein the passivation layer is used to reduce defects when two interfaces are in contact.
10. A method for preparing a solar cell, characterized in that: Methods include: A light absorbing layer comprising a plurality of perovskite compound grains as described in any one of claims 1 to 9 is prepared by a contactless sealed annealing container, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm is ≥90%.
11. The preparation method according to claim 10, characterized in that: The method comprises at least one of the following conditions: 1) The sealed annealing container contains an annealing atmosphere, and the annealing atmosphere includes a polar aprotic solvent; optionally, the polar aprotic solvent includes at least one of N,N-dimethylformamide, 1-methyl-2-pyrrolidone, dimethyl sulfoxide, and dimethylacetamide; 2) The annealing temperature in the sealed annealing container is 100-180°C, and can be optionally 120-160°C; 3) The annealing time in the sealed annealing container is 8 to 30 minutes, and can be optionally 10 to 20 minutes.
12. A solar cell module, characterized in that: The invention comprises the solar cell according to any one of claims 1 to 9 or the solar cell prepared by the preparation method according to claim 10 or 11.
13. An electrical device, characterized in that: The solar cell assembly according to claim 12 is used for providing electric energy.