Potassium bromoborate piezo-electric crystal and cut shape and application thereof
By developing potassium bromide borate piezoelectric crystal and its cutting type, the frequency and temperature instability of existing piezoelectric materials under high frequency and high temperature conditions has been solved, and high voltage performance and wide temperature application range have been achieved, which has met the High requirements in fields such as aerospace and geological surveys.
Patent Information
- Application Number
- CN202310605056.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
Existing piezoelectric crystal materials exhibit frequency instability, temperature instability and difficulty in growth under high frequency and high temperature conditions, and cannot meet the high requirements in fields such as aerospace and geological surveys.
The potassium bromide borate piezoelectric crystal (K3B6O10Br) was developed to grow large-sized single crystals through the flux method, and its piezoelectric properties were measured by the bridge method and the resonance method to prepare piezoelectric components of different cutting types.
Potassium bromide borate crystals have high voltage constants and a wide range of temperature application, which are better than the piezoelectric properties of SiO2 crystals. They are suitable for high-frequency broadband filters and high-frequency stability oscillators, providing higher application prospects.
Smart Images

Figure CN119031818A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of piezoelectric crystals and relates to a potassium bromoborate piezoelectric crystal and its cutting and application. Background Art
[0002] When certain crystal materials are deformed by external forces in a certain direction, polarization will occur inside them, causing the center of gravity of the charge to shift relatively, thereby generating equal and opposite charges on the opposite surfaces of the crystal; when the external force is removed, the crystal returns to an uncharged state. This phenomenon is called the piezoelectric effect, and the amount of charge generated by the crystal when it is subjected to force is proportional to the magnitude of the external force; conversely, if an electric field is applied to the crystal material, the crystal will produce mechanical deformation in the polarization direction; when the external electric field is removed, the deformation disappears as well. This phenomenon is called the inverse piezoelectric effect, also known as the electrostrictive effect. Crystal materials with piezoelectric effect or inverse piezoelectric effect can be called piezoelectric crystals.
[0003] Piezoelectric crystals are widely used in ultrasonic transducers, surface acoustic wave devices, piezoelectric oscillators, piezoelectric filters, sensors, etc. Currently, the commercialized piezoelectric crystals mainly include single crystal quartz (α-SiO2), lithium niobate (LiNbO3), lithium tantalate (LiTaO3) and relaxor ferroelectric PMT-PT.
[0004] Single crystal quartz has the advantages of zero frequency coefficient cut and very good temperature stability, but its piezoelectric coefficient and electromechanical coupling factor are low; at the same time, single crystal quartz tends to form twin domain structure under pressure conditions at temperatures above 350℃, and a phase transition from α-SiO2 to β-SiO2 occurs at a temperature of 573℃. Lithium niobate and lithium tantalate crystals are two very important piezoelectric crystals. Both of these crystals have large piezoelectric coefficients and electromechanical coupling coefficients, and good high-frequency performance. They are often used to make high-frequency broadband filters and high-frequency ultrasonic transducers. However, the frequency temperature coefficients of various cuts of lithium niobate crystals are negative, and the frequency stability of lithium tantalate crystals at room temperature is also poor. Secondly, lithium niobate and lithium tantalate crystals need to be polarized before use. Although PMN-PT crystals have very large piezoelectric coefficients and electromechanical coupling coefficients, they contain environmentally unfriendly elements, do not have a zero temperature coefficient of elastic coefficient, and it is currently difficult to grow PMN-PT single crystals of uniform quality.
[0005] Due to the development of electronics and communications, the need for high-frequency and fast transmission communications has led to an interest in new piezoelectric materials that can be used to make wide-band filters and high-frequency stability oscillators. The above-mentioned piezoelectric crystals cannot meet the demand, and several new piezoelectric materials such as lithium tetraborate (Li2B4O7) and LGS (lanthanum gallium silicate) series crystals have been developed and widely used. Lithium tetraborate has a low delay temperature coefficient, temperature stability comparable to single crystal quartz, an electromechanical coupling coefficient that is 7 times that of quartz, and a high surface acoustic wave velocity, making it an ideal material for making narrow-band pass surface acoustic filters, oscillators, and high-frequency bulk wave devices; however, lithium tetraborate is easily soluble in acid and has a slight deliquescent property, so certain protective measures need to be taken during device manufacturing; LGS series crystals have almost all the advantages of single crystal quartz, and their stability, piezoelectric coefficient, and electromechanical coupling coefficient are much higher than those of single crystal quartz, but it is still difficult to grow large-scale, high-quality LGS series crystals. At the same time, because the melting point of LGS series crystals is very high and the Ga content in the crystals is high, the growth cost is high.
[0006] From the above analysis, we can see that although there are many types of piezoelectric crystals, few of them can be used in practice, and due to their respective insurmountable shortcomings, with the development of modern science and technology, higher requirements are placed on piezoelectric materials used in aerospace, geological survey and other fields, making the development of new piezoelectric crystal materials a top priority. Summary of the invention
[0007] In order to improve the deficiencies of the prior art, the present invention aims to provide a potassium bromoborate piezoelectric crystal and its cutting and application. 10 Br(KBB) crystal is a kind of ultraviolet nonlinear optical crystal with excellent performance. Its basic optical properties such as crystal structure, transmission spectrum, nonlinear effect, etc. have been reported, and large-sized single crystals have been successfully grown using the flux method.
[0008] The study found that potassium bromoborate has a piezoelectric effect and can be used as a piezoelectric crystal material. The relative dielectric constant ε of the potassium bromoborate crystal at room temperature (25°C) was measured by the bridge method and the resonance method. 11 =ε 22 =8.74,ε 33 =8.62, piezoelectric constant d 33 =6.69pC / N,d 15 =6.00pC / N,d 21 =0.87pC / N,d 31 =2.48pC / N, which is higher than the piezoelectric effect of SiO2 crystal, indicating that the potassium bromoborate piezoelectric crystal has good piezoelectric properties and a higher temperature applicable range (20-500°C), and is a piezoelectric material with application prospects.
[0009] The object of the present invention is achieved through the following technical solutions:
[0010] The invention discloses an application of potassium bromoborate crystal as a piezoelectric crystal.
[0011] According to an embodiment of the present invention, the chemical formula of the potassium bromoborate crystal is K3B6O 10 Br.
[0012] According to an embodiment of the present invention, the potassium bromoborate crystal belongs to the trigonal system, R3m space group.
[0013] According to an embodiment of the present invention, the potassium bromoborate crystal has a 3m point group structure.
[0014] According to an embodiment of the present invention, the molecular weight of the potassium bromoborate crystal is 422.07.
[0015] According to an embodiment of the present invention, the unit cell parameters of the potassium bromoborate crystal are
[0016] According to an embodiment of the present invention, the potassium bromoborate crystals are recorded as KBB crystals.
[0017] According to an embodiment of the present invention, the potassium bromoborate crystal has a piezoelectric effect.
[0018] According to an embodiment of the present invention, the cut structure of the potassium bromoborate crystal is a square flake cut, a columnar cut (crystal rod cut) or a rectangular flake cut.
[0019] According to an embodiment of the present invention, the corresponding surfaces at both ends of the potassium bromoborate crystal need to be horizontal and parallel to each other.
[0020] According to an embodiment of the present invention, the potassium bromoborate crystals can be prepared by methods known in the art.
[0021] The invention also provides an application of potassium bromoborate crystal as a piezoelectric crystal in electronic equipment.
[0022] According to an embodiment of the present invention, the electronic device includes at least one of an ultrasonic transducer, a surface acoustic wave device, a piezoelectric oscillator, a piezoelectric filter and a sensor, preferably a narrowband pass surface acoustic wave filter, an oscillator, and a high-frequency bulk wave device.
[0023] The present invention also provides an application of potassium bromoborate crystal as a piezoelectric crystal in a piezoelectric component.
[0024] According to an embodiment of the present invention, conductive materials are plated on both surfaces of the potassium bromoborate crystal to which an electric field is applied to form electrodes, and the electrodes are externally connected to leads to form a piezoelectric component.
[0025] The present invention also provides a potassium bromoborate piezoelectric crystal cut, wherein the physical coordinate axes X, Y and Z of the potassium bromoborate piezoelectric crystal are respectively parallel to the crystallographic
[100] plane,
[120] plane and
[001] plane of the potassium bromoborate piezoelectric crystal, and the physical coordinate axes X, Y and Z are perpendicular to each other and follow the right-hand screw rule; the thickness of the piezoelectric crystal is t, the length of the piezoelectric crystal is l, and the width of the piezoelectric crystal is w; after the piezoelectric crystal is cut, the rotation of the piezoelectric crystal around the X axis is α, the rotation of the piezoelectric crystal around the Y axis is β, and the rotation of the piezoelectric crystal around the Z axis is γ;
[0026] The potassium bromoborate piezoelectric crystal cut type is selected from any one of the following:
[0027] Z-direction columnar cutting refers to a wafer whose length in the physical coordinate axis is cut along the Z direction, and X=Y;
[0028] X-direction square wafer cutting refers to a wafer whose thickness is cut along the X direction in the physical coordinate axis, and Y=Z;
[0029] Y-direction square slice cutting refers to the wafer whose thickness is cut along the Y direction in the physical coordinate axis and X=Z;
[0030] Z-direction square wafer cutting refers to a wafer whose thickness is cut along the Z direction in the physical coordinate axis, and X=Y;
[0031] YX cut type refers to a wafer cut along the Y direction in the physical coordinate axis and along the X direction in length;
[0032] ZX cut refers to a wafer cut with thickness along the Z direction and length along the X direction in the physical coordinate axis;
[0033] XYt / γ cut type refers to a wafer cut in which the thickness is along the X direction and the length is along the Y direction in the physical coordinate axis, and the wafer is cut in the γ direction with the thickness direction as the rotation axis, and γ is 30° to 60°, such as 45°;
[0034] ZXt / γ-cut type refers to a wafer cut in which the thickness is along the Z direction and the length is along the X direction in the physical coordinate axis, and the wafer is cut in the γ direction with the thickness direction as the rotation axis, and γ is 30° to 60°, such as 45°;
[0035] YZt / γ cut type refers to a wafer cut in which the thickness is along the Y direction and the length is along the Z direction in the physical coordinate axis, and the wafer is cut in the γ direction with the thickness direction as the rotation axis, and γ is 30° to 60°, such as 45°.
[0036] According to an embodiment of the present invention, the positive values of the Y-axis and the Z-axis are represented by d 33 Measuring instrument measures d 22 and d 33 It turns out that the direction with positive value is the positive axis.
[0037] According to an embodiment of the present invention, a gold electrode is plated on the surface of the cut crystal, and the dielectric constant, elastic coefficient and piezoelectric constant are measured after polarization.
[0038] The present invention also provides a method for measuring the piezoelectric performance constant of a potassium bromoborate piezoelectric crystal, wherein the physical coordinate axes X, Y and Z of the potassium bromoborate piezoelectric crystal are respectively parallel to the crystallographic
[100] plane,
[120] plane and
[001] plane of the potassium bromoborate piezoelectric crystal, and the physical coordinate axes X, Y and Z are perpendicular to each other and follow the right-hand screw rule; the thickness of the piezoelectric crystal is recorded as t, the length of the piezoelectric crystal is recorded as l, and the width of the piezoelectric crystal is recorded as w; after the piezoelectric crystal is cut, a certain angle rotated around the X axis is recorded as α, a certain angle rotated around the Y axis is recorded as β, and a certain angle rotated around the Z axis is recorded as γ;
[0039] The method comprises the following steps:
[0040] (1) Cut the potassium bromoborate piezoelectric crystal as follows:
[0041] The length of the physical coordinate axis is cut along the Z direction, and X=Y, to obtain a Z-direction cylindrical cut;
[0042] The thickness is cut along the X direction in the physical coordinate axis, and Y=Z, to obtain a square sheet cut in the X direction;
[0043] The thickness is cut along the Y direction in the physical coordinate axis, and X=Z, to obtain a Y-direction square sheet cut;
[0044] The thickness is cut along the Z direction in the physical coordinate axis, and X=Y, to obtain a square sheet cut in the Z direction;
[0045] In the physical coordinate axis, the thickness is cut along the Y direction and the length is cut along the X direction to obtain a YX cut;
[0046] In the physical coordinate axis, the thickness is cut along the Z direction and the length is cut along the X direction to obtain a ZX cut;
[0047] In the physical coordinate axis, the thickness is along the X direction and the length is along the Y direction. The thickness direction is used as the rotation axis and the cutting is rotated in the γ direction to obtain an XYt / γ cut, where γ is 30° to 60°, such as 45°.
[0048] In the physical coordinate axis, the thickness is along the Z direction and the length is along the X direction. The thickness direction is used as the rotation axis and the cutting is rotated in the γ direction to obtain a ZXt / γ cut, where γ is 30° to 60°, such as 45°.
[0049] In the physical coordinate axis, the thickness is along the Y direction and the length is along the Z direction. The thickness direction is used as the rotation axis and the cutting is rotated in the γ direction to obtain a YZt / γ cut, where γ is 30° to 60°, such as 45°.
[0050] (2) Gold electrodes are plated on the two surfaces of the obtained crystal cut to apply an electric field, and the piezoelectric performance constant of the potassium bromoborate piezoelectric crystal is measured.
[0051] According to an embodiment of the present invention, the piezoelectric performance constants include but are not limited to dielectric constant, elastic coefficient and piezoelectric constant.
[0052] According to an embodiment of the present invention, in step (2), the measuring method includes at least one of the following methods:
[0053] Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the square slice cut in the X direction with gold-plated electrodes, and measure the relative dielectric constant ε by AC bridge method 11 ε0;
[0054] Select the piezoelectric coordinate axis, apply an electric field to the two gold-plated electrodes on the surface of the square sheet cut in the X direction, and after electric field polarization, use the thickness cut edge vibration mode and resonance method to measure d 15 ,s 55 ;
[0055] Select the piezoelectric coordinate axis, apply electric field to the two gold-plated electrodes on the Y-axis square slice cut, and after electric field polarization, use the thickness cut edge vibration mode and resonance method to measure s 66 ,s 12 ;
[0056] Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the square slice cut in the Z direction with gold-plated electrodes, and measure the relative dielectric constant ε by AC bridge method 33 ε0;
[0057] Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the Z-axis columnar cut, and measure the piezoelectric constant d using the longitudinal vibration mode. 33 ,s 33 ;
[0058] Select the piezoelectric coordinate axis, apply electric field on the two surfaces of the ZX cut with gold electrodes, and after electric field polarization, use the length stretching vibration mode and resonance method to measure d 31 ,s 11 ;
[0059] Select the piezoelectric coordinate axis, apply electric field on the two surfaces of the YX cut with gold electrodes, and after electric field polarization, use the length stretching vibration mode and resonance method to measure d 21 ;
[0060] Select the piezoelectric coordinate axis, apply electric field on the two surfaces of XYt / γ-cut type, and after electric field polarization, use the length stretching vibration mode and resonance method to measure s 13 ,s 14 ;
[0061] Select the piezoelectric coordinate axis, apply electric field on the two surfaces of ZXt / γ-cut type, plate gold electrodes, and use the length stretching vibration mode and resonance method to measure s after electric field polarization. 66 ,s 12 ;
[0062] The piezoelectric coordinate axis was selected, and gold electrodes were plated on the two surfaces of the YZt / γ-cut type to apply an electric field. After electric field polarization, the resonance method was used to measure s using the length stretching vibration mode. 13 ,s 14 .
[0063] Terminology Notes and Explanations:
[0064] <Piezoelectric effect>
[0065] When some dielectrics are deformed by external forces in a certain direction, polarization will occur inside them, and opposite positive and negative charges will appear on their two opposite surfaces. When the external force is removed, they can restore their uncharged shape. This phenomenon is called the positive piezoelectric effect. On the contrary, when an electric field is applied in the polarization direction of the dielectric, these dielectrics will also be deformed. When the electric field is removed, the shape of the dielectric disappears. This phenomenon is called the inverse piezoelectric effect.
[0066] <Piezoelectric constant>
[0067] The parameters that characterize the coupling relationship between the mechanical parameters (stress, strain) and electrical parameters (charge, electric displacement) of piezoelectric materials can be divided into piezoelectric stress constant and piezoelectric strain constant. The piezoelectric constant in this paper is the abbreviation of piezoelectric strain constant, which involves 4 independent piezoelectric constants of KBB crystal: d 33 d 15 d 21 and d 31 .
[0068] <Wafer Cutting Symbols>
[0069] The wafer cutting symbol consists of two letters and an angle. The two letters are two of the coordinate axes XYZ. The first letter indicates the thickness direction of the wafer before rotation, and the second letter indicates the length direction of the wafer before rotation. For example, YX cutting means that the thickness of the wafer is in the Y direction and the length is in the X direction. The remaining letters in the wafer cutting symbol indicate the rotation axis of the wafer. Rotation around thickness is recorded as t, rotation around length is recorded as l, and rotation around width is recorded as w; rotation around the X axis at a certain angle is recorded as α, rotation around the Y axis at a certain angle is recorded as β, and rotation around the Z axis at a certain angle is recorded as γ. The rotation method follows the right-hand screw rule. For example, (ZXtw)γ / β cutting means that the wafer with thickness direction Z and length direction X is rotated by γ angle with thickness t as the rotation axis, and then rotated by β angle with width as the rotation axis to form a cutting method. The rotation method follows the right-hand screw rule.
[0070] <AC Bridge Method>
[0071] By measuring the capacitance and size of the chip, according to (C is capacitance, t and A are the thickness and area of the chip respectively, and ε0 is the dielectric constant of vacuum) The method for calculating the dielectric constant.
[0072] <Resonance method>
[0073] The method is to determine the elasticity and piezoelectric constant of the piezoelectric array material by measuring the series frequency (parallel resonant frequency) and some other parameters (capacitance, size, density) of the piezoelectric array and performing appropriate calculations.
[0074] The formula used in the above resonance method is as follows:
[0075]
[0076] c=4ρ(f r t) 2
[0077] c=4ρ(f a t) 2
[0078]
[0079]
[0080] d=k(sε) 1 / 2
[0081] c=s -1
[0082] Among them, s is the elastic compliance constant, c is the elastic hardness constant, k is the electromechanical coupling coefficient, d is the piezoelectric strain constant, e is the piezoelectric stress constant, ε is the dielectric constant, ρ is the crystal density, l is the chip length, and fr and f a are the resonant frequency and anti-resonant frequency respectively.
[0083] Beneficial effects of the present invention:
[0084] The present invention provides a potassium bromoborate piezoelectric crystal and its cutting and application. 10 Br(KBB) crystal is a kind of ultraviolet nonlinear optical crystal with excellent performance. Its basic optical properties such as crystal structure, transmission spectrum, nonlinear effect, etc. have been reported, and large-sized single crystals have been successfully grown using the flux method.
[0085] The inventors of this application have found that the potassium bromoborate crystal has a piezoelectric effect and can be used as a piezoelectric crystal material. The relative dielectric constant ε of the potassium bromoborate crystal was measured by the bridge method and the resonance method. 11 =ε 22 =8.74,ε 33 =8.62, piezoelectric constant d 33 =6.69pC / N,d 15 =6.00pC / N,d 21 =0.87pC / N,d 31 =2.48pC / N, which is higher than the piezoelectric effect of SiO2 crystal, indicating that potassium bromoborate crystal is a piezoelectric material with application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1 Schematic diagram of nine wafer cuts for measuring the dielectric, elastic and piezoelectric constants of KBB crystal in Example 1. DETAILED DESCRIPTION
[0087] The present invention will be described in further detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0088] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0089] The KBB crystals selected in the following examples are products purchased through commercial channels.
[0090] Example 1
[0091] according to Figure 1 The KBB crystal is cut in the following direction:
[0092] The 1-X square piece is obtained, and its thickness is along the X direction, and its size is: length × width × height = 4.0 × 4.0 × 1.5m 3 ;
[0093] The 2-Y square sheet is obtained, and its thickness is along the Y direction, and its dimensions are: length × width × height = 6.0 × 5.0 × 1.5 mm 3 ;
[0094] The 3-Z square sheet is obtained, and its thickness is along the Z direction, and its dimensions are: length × width × height = 4.0 × 4.0 × 1.5 mm 3 ;
[0095] The 4-Z crystal rod is obtained, and its length is along the Z direction, and its dimensions are: length × width × height = 8.0 × 4.0 × 4.0 m 3 ;
[0096] The 5-ZX wafer is obtained, with a thickness in the Z direction and a length in the X direction, and a size of: length × width × height = 8.0 × 4.0 × 1.5 m 3 ;
[0097] The 6-YX wafer is obtained, with thickness along the Y direction and length along the X direction, and the dimensions are: length × width × height = 8.0 × 4.0 × 1.5 m 3 ;
[0098] The 7-XYt / 45° wafer is obtained, with its thickness along the X direction and length along the Y direction. It is cut in a direction rotated 45° with the thickness direction as the rotation axis. The size is: length × width × height = 8.0 × 4.0 × 1.5m 3 ;
[0099] The 8-ZXt / 45° wafer is obtained, with its thickness along the Z direction and length along the X direction. It is cut in a direction rotated 45° with the thickness direction as the rotation axis. The size is: length × width × height = 8.0 × 4.0 × 1.5m 3 ;
[0100] The 9-YZt / 45° wafer is obtained, with its thickness along the Y direction and length along the Z direction. It is cut in a direction rotated 45° with the thickness direction as the rotation axis. The size is: length × width × height = 8.0 × 4.0 × 1.5m 3 ;
[0101] Test Example 1
[0102] The following test example uses the AC bridge method and the resonance method to measure the relative dielectric constant, piezoelectric constant and elastic constant of the KBB crystal obtained in Example 1.
[0103] Select the piezoelectric coordinate axis, plate gold electrodes on both surfaces of the 1-X square plate to apply an electric field, and measure the relative dielectric constant ε using the AC bridge method. 11 / ε0. Gold electrodes were plated on both surfaces of the 1-X square plate to apply an electric field. After electric field polarization, the thickness shear vibration mode and resonance method were used to measure d 15 ,s 55 .
[0104] Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the 2-Y wafer, plate gold electrodes, and after electric field polarization, use the thickness shear vibration mode and resonance method to measure s 66 ,s 12 .
[0105] Select the piezoelectric coordinate axis, plate gold electrodes on both surfaces of the 3-Z square to apply the electric field, and measure the relative dielectric constant ε using the AC bridge method. 33 ε0.
[0106] Select the piezoelectric coordinate axis, plate gold electrodes on both surfaces of the 4-Z crystal rod to apply the electric field, and measure the piezoelectric constant d using the longitudinal vibration mode. 33 ,s 33 .
[0107] Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the 5-ZX wafer, plate gold electrodes, and use the length stretching vibration mode and resonance method to measure d after electric field polarization. 31 ,s 11 .
[0108] Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the 6-YX wafer, plate gold electrodes, and use the length stretching vibration mode and resonance method to measure d after electric field polarization. 21 .
[0109] Select the piezoelectric coordinate axis, apply the electric field to the gold-plated electrodes on both surfaces of the 7-Xyt / 45° wafer, and after electric field polarization, use the length stretching vibration mode and the resonance method to measure s 13 ,s 14 .
[0110] Select the piezoelectric coordinate axis, apply the electric field to the gold-plated electrodes on both surfaces of the 8-ZXt / 45° wafer, and after electric field polarization, use the length stretching vibration mode and the resonance method to measure s 66 ,s 12 .
[0111] The piezoelectric coordinate axis was selected, and the gold-plated electrodes on both surfaces of the 9-YZt / 45° wafer were applied with an electric field. After electric field polarization, the resonance method was used to measure s using the face-to-face length stretching vibration mode. 13 ,s 14 .
[0112] The results obtained by the calculations in the examples are shown in Table 1.
[0113] Table 1. Dielectric constant, piezoelectric constant and elastic constant of KBB crystal at room temperature
[0114]
[0115]
[0116] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. Application of potassium bromoborate crystal as piezoelectric crystal.
2. The use according to claim 1, wherein: The chemical formula of the potassium bromoborate crystal is K3B6O 10 Br. And / or, the potassium bromoborate crystal belongs to the trigonal system, R3m space group. And / or, the potassium bromoborate crystal has a 3m point group structure. And / or, the molecular weight of the potassium bromoborate crystals is 422.
07. And / or, the unit cell parameters of the potassium bromoborate crystal are 3. The use according to claim 1 or 2, wherein: The cut structure of the potassium bromoborate crystal is a square flake cut, a columnar cut (crystal rod cut) or a rectangular flake cut.
4. Application of potassium bromoborate crystal as piezoelectric crystal in electronic equipment. Preferably, the electronic device includes at least one of an ultrasonic transducer, a surface acoustic wave device, a piezoelectric oscillator, a piezoelectric filter and a sensor, preferably a narrow-band pass surface acoustic wave filter, an oscillator, a high-frequency bulk wave device.
5. Application of potassium bromoborate crystal as piezoelectric crystal in piezoelectric components. Preferably, conductive material is plated on both surfaces of the potassium bromoborate crystal to which an electric field is applied to form electrodes, and the electrodes are externally connected to leads to form a piezoelectric component.
6. A potassium bromoborate piezoelectric crystal cut, wherein the physical coordinate axes X, Y and Z of the potassium bromoborate piezoelectric crystal are parallel to the crystallographic [100] plane, [120] plane and [001] plane of the potassium bromoborate piezoelectric crystal, respectively, and the physical coordinate axes X, Y and Z are perpendicular to each other and follow the right-hand screw rule; the thickness of the piezoelectric crystal is t, the length of the piezoelectric crystal is l, and the width of the piezoelectric crystal is w; after the piezoelectric crystal is cut, the rotation around the X axis is α, the rotation around the Y axis is β, and the rotation around the Z axis is γ; The potassium bromoborate piezoelectric crystal cut type is selected from any one of the following: Z-direction columnar cutting refers to a wafer whose length in the physical coordinate axis is cut along the Z direction, and X=Y; X-direction square wafer cutting refers to a wafer whose thickness is cut along the X direction in the physical coordinate axis, and Y=Z; Y-direction square slice cutting refers to the wafer whose thickness is cut along the Y direction in the physical coordinate axis and X=Z; Z-direction square wafer cutting refers to a wafer whose thickness is cut along the Z direction in the physical coordinate axis, and X=Y; YX cut type refers to a wafer cut along the Y direction in the physical coordinate axis and along the X direction in length; ZX cut refers to a wafer cut with thickness along the Z direction and length along the X direction in the physical coordinate axis; XYt / γ cut type refers to a wafer cut in which the thickness is along the X direction and the length is along the Y direction in the physical coordinate axis, and the wafer is cut in the γ direction with the thickness direction as the rotation axis, and γ is 30° to 60°, such as 45°; ZXt / γ-cut type refers to a wafer cut in which the thickness is along the Z direction and the length is along the X direction in the physical coordinate axis, and the wafer is cut in the γ direction with the thickness direction as the rotation axis, and γ is 30° to 60°, such as 45°; YZt / γ cut type refers to a wafer cut in which the thickness is along the Y direction and the length is along the Z direction in the physical coordinate axis, and the wafer is cut in the γ direction with the thickness direction as the rotation axis, and γ is 30° to 60°, such as 45°.
7. The potassium bromoborate piezoelectric crystal cut according to claim 6, wherein: Gold electrodes were plated on the surface of the cut crystal, and the dielectric constant, elastic modulus and piezoelectric constant were measured after polarization.
8. A method for measuring the piezoelectric performance constant of a potassium bromoborate piezoelectric crystal, wherein the physical coordinate axes X, Y and Z of the potassium bromoborate piezoelectric crystal are parallel to the crystallographic [100] plane, [120] plane and [001] plane of the potassium bromoborate piezoelectric crystal, respectively, and the physical coordinate axes X, Y and Z are perpendicular to each other and follow the right-hand screw rule; the thickness of the piezoelectric crystal is t, the length of the piezoelectric crystal is l, and the width of the piezoelectric crystal is w; after the piezoelectric crystal is cut, the rotation around the X axis is α, the rotation around the Y axis is β, and the rotation around the Z axis is γ; The method comprises the following steps: (1) Cut the potassium bromoborate piezoelectric crystal as follows: The length of the physical coordinate axis is cut along the Z direction, and X=Y, to obtain a Z-direction cylindrical cut; The thickness is cut along the X direction in the physical coordinate axis, and Y=Z, to obtain a square sheet cut in the X direction; The thickness is cut along the Y direction in the physical coordinate axis, and X=Z, to obtain a Y-direction square sheet cut; The thickness is cut along the Z direction in the physical coordinate axis, and X=Y, to obtain a square sheet cut in the Z direction; In the physical coordinate axis, the thickness is cut along the Y direction and the length is cut along the X direction to obtain a YX cut; In the physical coordinate axis, the thickness is cut along the Z direction and the length is cut along the X direction to obtain a ZX cut; In the physical coordinate axis, the thickness is along the X direction and the length is along the Y direction. The thickness direction is used as the rotation axis and the cutting is rotated in the γ direction to obtain an XYt / γ cut, where γ is 30° to 60°, such as 45°. In the physical coordinate axis, the thickness is along the Z direction and the length is along the X direction. The thickness direction is used as the rotation axis and the cutting is rotated in the γ direction to obtain a ZXt / γ cut, where γ is 30° to 60°, such as 45°. In the physical coordinate axis, the thickness is along the Y direction and the length is along the Z direction. The thickness direction is used as the rotation axis and the cutting is rotated in the γ direction to obtain a YZt / γ cut, where γ is 30° to 60°, such as 45°. (2) Gold electrodes are plated on the two surfaces of the obtained crystal cut to apply an electric field, and the piezoelectric performance constant of the potassium bromoborate piezoelectric crystal is measured.
9. The measuring method according to claim 8, wherein: The piezoelectric performance constants include, but are not limited to, dielectric constant, elastic coefficient and piezoelectric constant.
10. The measuring method according to claim 8 or 9, wherein: In step (2), the measuring method includes at least one of the following methods: Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the square slice cut in the X direction with gold-plated electrodes, and measure the relative dielectric constant ε by AC bridge method 11 ε0; Select the piezoelectric coordinate axis, apply an electric field to the two gold-plated electrodes on the surface of the square sheet cut in the X direction, and after electric field polarization, use the thickness cut edge vibration mode and resonance method to measure d 15 ,s 55 ; Select the piezoelectric coordinate axis, apply electric field to the two gold-plated electrodes on the Y-axis square slice cut, and after electric field polarization, use the thickness cut edge vibration mode and resonance method to measure s 66 ,s 12 ; Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the square slice cut in the Z direction with gold-plated electrodes, and measure the relative dielectric constant ε by AC bridge method 33 ε0; Select the piezoelectric coordinate axis, apply electric field to the two surfaces of the Z-axis columnar cut, and measure the piezoelectric constant d using the longitudinal vibration mode. 33 ,s 33 ; Select the piezoelectric coordinate axis, apply electric field on the two surfaces of the ZX cut with gold electrodes, and after electric field polarization, use the length stretching vibration mode and resonance method to measure d 31 ,s 11 ; Select the piezoelectric coordinate axis, apply electric field on the two surfaces of the YX cut with gold electrodes, and after electric field polarization, use the length stretching vibration mode and resonance method to measure d 21 ; Select the piezoelectric coordinate axis, apply electric field on the two surfaces of XYt / γ-cut type, and after electric field polarization, use the length stretching vibration mode and resonance method to measure s 13 ,s 14 ; Select the piezoelectric coordinate axis, apply electric field on the two surfaces of ZXt / γ-cut type, plate gold electrodes, and use the length stretching vibration mode and resonance method to measure s after electric field polarization. 66 ,s 12 ; The piezoelectric coordinate axis was selected, and gold electrodes were plated on the two surfaces of the YZt / γ-cut type to apply an electric field. After electric field polarization, the resonance method was used to measure s using the length stretching vibration mode. 13 ,s 14 .