Quartz glass crucible for pulling monocrystalline silicon ingot
By controlling the concentration of Na, K and Li in a quartz glass crucible for single crystal silicon ingot lifting, the crystallization of the brown ring is promoted in the depth direction, the pinhole problem during single crystal silicon ingot lifting is solved, and a higher degree of Yield and crucible stability.
Patent Information
- Application Number
- CN202380034926.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-14
- Publication Date
- 2024-11-26
AI Technical Summary
During the lifting process of single crystal silicon ingot, bubbles generated in the brown ring on the inner surface of the quartz glass crucible lead to pinholes, which is difficult to effectively explain and suppress in the prior art.
Design a single crystal silicon ingot lifting quartz glass crucible, which has a crucible shape composed of a straight cylindrical portion, an R portion and a bottom. The outer layer is composed of opaque quartz glass, and the inner layer is composed of transparent quartz glass and the wall thickness is 1.5mm. As above, the concentrations of Na, K, and Li in the inner and outer layers are controlled within a specific range to promote the crystallization of the depth direction of the brown ring and inhibit the release of bubbles.
By controlling the Na, K, and Li concentrations of the inner and outer layers of the quartz glass crucible, the pinholes of the single crystal silicon ingot can be effectively suppressed, the yield can be improved, and the crucible can be prevented from pouring and sinking during high-temperature heating.
Smart Images

Figure CN119032203A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a quartz glass crucible for pulling a single crystal silicon ingot. Background Art
[0002] In the manufacture of single crystal silicon (single crystal silicon ingot), the so-called Czochralski method (CZ method) is widely used. The CZ method is to place a silicon melt in a quartz glass crucible, bring a seed crystal into contact with the surface of the silicon melt, rotate the quartz glass crucible, and simultaneously pull the seed crystal upward while rotating it in the opposite direction, thereby growing a single crystal silicon at the lower end of the seed crystal.
[0003] Single crystal silicon ingots produced using quartz glass crucibles sometimes contain bubbles ranging from a few micrometers to a few millimeters in size, called pinholes. Although silicon wafers containing such bubbles can be detected by visual inspection or infrared inspection, the presence of even a single pinhole can cause a decrease in yield.
[0004] The sources of bubbles that cause pinholes in the pulled single crystal silicon ingot include the gas in the pulling device, bubbles contained in the inner surface of the quartz glass crucible, or gas generated by the reaction between the silicon melt and the quartz glass crucible. Countermeasures against these bubbles are currently being sought (for example, Patent Document 1).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2013 / 140706 Summary of the invention
[0008] 1. Technical issues to be resolved
[0009] As described above, conventionally, countermeasures have been sought for bubbles that are the cause of pinholes in pulled single crystal silicon ingots. However, pinholes that cannot be explained by these bubbles may occur, and a quartz glass crucible with fewer pinholes in pulled single crystal silicon ingots has been sought.
[0010] The present invention is made to solve the above-mentioned technical problems, and its object is to provide a quartz glass crucible for pulling a single crystal silicon ingot, which can suppress pinholes in the pulled single crystal silicon ingot.
[0011] (II) Technical solution
[0012] The present invention is completed in order to solve the above-mentioned technical problems, and provides a quartz glass crucible for pulling a single crystal silicon ingot, the quartz glass crucible for pulling a single crystal silicon ingot having a crucible shape consisting of a straight tube portion, an R portion and a bottom portion, and having: an outer layer consisting of an opaque quartz glass containing bubbles, and an inner layer consisting of a transparent quartz glass with a wall thickness of 1.5 mm or more, the quartz glass crucible for pulling a single crystal silicon ingot being characterized in that, with respect to the concentrations of Na, K and Li at a position 1 mm away from the inner surface of the quartz glass crucible of the inner layer, Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 100 mass ppb, and with respect to the average concentrations of Na, K and Li in the wall thickness direction of the R portion and the bottom portion of the outer layer, Na is less than 10 mass ppb, K is less than 50 mass ppb, and Li is less than 180 mass ppb.
[0013] Such a quartz glass crucible can promote crystallization in the depth direction in the brown ring generated on the inner surface of the quartz glass crucible during the pulling of the single crystal silicon ingot. As a result, the release of bubbles generated inside the brown ring can be suppressed, thereby suppressing pinholes in the pulled single crystal silicon ingot.
[0014] At this time, the concentrations of Na, K and Li in the inner layer at a position 1 mm away from the inner surface of the quartz glass crucible are preferably: Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 50 mass ppb, and the average concentrations of Na, K and Li in the wall thickness direction of the R portion and the bottom of the outer layer are preferably: Na is less than 5 mass ppb, K is less than 50 mass ppb, and Li is less than 100 mass ppb.
[0015] By satisfying such concentrations of impurity elements (in the following description, Na, K, and Li may be collectively referred to as impurity elements) in the inner and outer layers of the quartz glass crucible, pinholes in the pulled single crystal silicon ingot can be more effectively suppressed.
[0016] In addition, it is preferred that the average concentrations of Na, K and Li in the wall thickness direction of the straight tube portion of the outer layer satisfy at least any one of the following concentrations: Na is 10 mass ppb or more; K is 50 mass ppb or more; Li is 180 mass ppb or more.
[0017] By satisfying such an impurity concentration in the straight tube portion of the outer layer, it is possible to suppress the quartz glass crucible from tipping over or sinking during high-temperature heating, compared with making the entire crucible high in purity.
[0018] In addition, the outer diameter of the quartz glass crucible may be greater than 800 mm.
[0019] Therefore, the present invention can be suitably applied even to a quartz glass crucible having a large diameter of 800 mm or more.
[0020] In addition, it is preferred that the quartz glass crucible holds the silicon melt therein, and after the single crystal silicon ingot is pulled from the silicon melt, a brown ring is formed on the inner surface of the quartz glass crucible, and the density of bubbles with a diameter of 3.0 μm or more in the inner layer in the inner area of the brown ring is 4.0 bubbles / mm 2 above.
[0021] A quartz glass crucible having such a brown ring formed on the inner surface of the quartz glass crucible after pulling a single crystal silicon ingot can more effectively suppress pinholes in the pulled single crystal silicon ingot.
[0022] In addition, it is preferred that the quartz glass crucible retains a silicon melt therein, and after a single crystal silicon ingot is pulled from the silicon melt, a brown ring is formed on the inner surface of the quartz glass crucible. As the brown ring, when a bisector of the brown ring along the circumferential direction of the quartz glass crucible is defined as an outer diameter reference line of the brown ring, the length of the outer diameter reference line is in a range of 10 mm to 13 mm. When the length of the outer diameter reference line of the brown ring is set to x (mm), the uppermost portion of the end of the outer diameter reference line of the brown ring is taken as a reference height 0 (μm), and the height of the convex portion of the uppermost portion on the outer diameter reference line as the inner area of the brown ring is set to y (μm), in the brown ring in which the length of the outer diameter reference line is in a range of 10 mm to 13 mm, the following formula (1) is satisfied:
[0023] y≥10x-70 ・・・(1).
[0024] The quartz glass crucible having such a brown ring formed thereon can more effectively suppress pinholes in the pulled single crystal silicon ingot.
[0025] (III) Beneficial effects
[0026] The quartz glass crucible of the present invention can promote the crystallization in the depth direction of the brown ring during the pulling of the single crystal silicon ingot, thereby suppressing the release of bubbles generated inside the brown ring and suppressing the pinholes of the pulled single crystal silicon ingot. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic cross-sectional view showing parts of a typical quartz glass crucible.
[0028] Figure 2 This is a photo of a brown ring generated on the inner surface of a quartz glass crucible.
[0029] Figure 3 is a graph showing the diameter of the bubble inside the brown ring.
[0030] Figure 4 : is a graph showing the relationship between the Li concentration in the inner layer of the quartz glass crucible and the bubble density inside the brown ring.
[0031] Figure 5 : is a graph showing the correlation between the Na concentration in the outer layer and the Na concentration in the inner layer of the quartz glass crucible.
[0032] Figure 6 : is a graph showing the correlation between the K concentration in the outer layer and the K concentration in the inner layer of the quartz glass crucible.
[0033] Figure 7 : is a graph showing the correlation between the Li concentration in the outer layer and the Li concentration in the inner layer of the quartz glass crucible.
[0034] Figure 8 Graphs showing the concavo-convex shapes of the brown rings in Experimental Examples 1 to 4.
[0035] Fig. 9 A schematic diagram illustrating the brown ring. DETAILED DESCRIPTION
[0036] As described above, a countermeasure against bubbles that are the cause of pinholes has been sought. However, unexplained pinholes may occur in some cases, and the inventors of the present application attempted to investigate the cause.
[0037] As a result, a brownish brown ring called a brown ring is generated on the inner surface of the quartz glass crucible after the single crystal silicon ingot is pulled. A detailed examination of the brown ring revealed that there are bubbles with a diameter of several microns to tens of microns inside the brown ring. It is expected that the bubbles will be exposed to the silicon melt and become pinholes.
[0038] In addition, as described above, there are bubbles of several microns to tens of microns in size inside the brown ring, but according to the research of the inventors, by reducing the concentration of Na, K, and Li in the inner layer of the quartz glass crucible, the diameter of the bubbles inside the brown ring can be reduced, and the crystallization in the depth direction inside the brown ring can be promoted, thereby reducing the melting loss into the silicon melt. In other words, it is possible to inhibit the release of bubbles inside the brown ring into the silicon melt, thereby reducing the bubbles incorporated into the single crystal silicon ingot and reducing the pinhole defects of the silicon wafer.
[0039] The present invention is described in more detail below. The present invention is a quartz glass crucible for pulling a single crystal silicon ingot, which has a crucible shape consisting of a straight tube, an R portion, and a bottom, and has: an outer layer consisting of an opaque quartz glass containing bubbles, and an inner layer consisting of a transparent quartz glass with a wall thickness of 1.5 mm or more, and the quartz glass crucible for pulling a single crystal silicon ingot is characterized in that, with respect to the concentration of Na, K, and Li at a position 1 mm away from the inner surface of the quartz glass crucible of the inner layer, Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 100 mass ppb, and with respect to the average concentration of Na, K, and Li in the wall thickness direction of the R portion and the bottom of the outer layer, Na is less than 10 mass ppb, K is less than 50 mass ppb, and Li is less than 180 mass ppb. These regulations need to be met before pulling a single crystal silicon ingot.
[0040] First, refer to Figure 1 The parts of the quartz glass crucible of the present invention will be described. Figure 1 The quartz glass crucible 10 has an outer layer 21 and an inner layer 22, wherein the outer layer 21 is made of opaque quartz glass containing bubbles, and the inner layer 22 is made of transparent quartz glass. Figure 1 As shown, the crucible shape of the quartz glass crucible 10 is typically composed of a bottom 12, an R portion 13, and a straight portion 14. A bottom center 11 is provided at the center of the bottom 12, the bottom 12 is sometimes referred to as a large R portion, and the R portion 13 is sometimes referred to as a small R portion.
[0041] As described above, the concentrations of Na, K, and Li at a position 1 mm away from the inner surface of the quartz glass crucible in the inner layer 22 having a wall thickness of 1.5 mm or more in the quartz glass crucible 10 of the present invention are as follows: Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 100 mass ppb. By making such a high-purity quartz glass crucible 10 having a predetermined concentration of Na, K, and Li in the inner layer 22, the crystallization in the depth direction of the brown ring can be promoted during the pulling of the single crystal silicon ingot. Thus, the release of bubbles generated inside the brown ring can be suppressed. In addition, the average concentrations of Na, K, and Li in the wall thickness direction at the R portion 13 and the bottom 12 in the outer layer 21 of the quartz glass crucible 10 of the present invention are as follows: Na is less than 10 mass ppb, K is less than 50 mass ppb, and Li is less than 180 mass ppb. By satisfying such element concentrations in the R portion 13 and the bottom 12 of the outer layer 21 , diffusion of the impurity elements to the inner surface of the crucible can be suppressed, and the crucible inner layer 22 can be maintained at a high purity.
[0042] It is preferable to further set the above impurity concentration to a high purity in the following manner. That is, in the inner layer 22, with respect to the concentration of Na, K and Li at a position 1 mm away from the inner surface of the quartz glass crucible, it is preferable that Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 50 mass ppb. In addition, in the outer layer 21, with respect to the average concentration of Na, K and Li in the wall thickness direction of the R portion 13 and the bottom 12, it is preferable that Na is less than 5 mass ppb, K is less than 50 mass ppb, and Li is less than 100 mass ppb. By satisfying such concentrations of impurity elements, pinholes in the pulled single crystal silicon ingot can be more effectively suppressed.
[0043] The concentration of impurity elements in each layer of the quartz glass crucible of the present invention can be measured by preparing a sample from the quartz glass crucible 10 and using ICP-MS (inductively coupled plasma mass spectrometry) or the like. In addition, the measurement point is set at least one location in each of the straight tube portion 14, the R portion 13, and the bottom portion 12 in the inner layer 22 and the outer layer 21. The measurement point can be set at two or more locations in each location to obtain an average value.
[0044] Reference Figure 5~Figure 7 Diffusion of each impurity element between the outer layer 21 and the inner layer 22 will be described. Figure 5~Figure 7 , respectively, show the correlation between the concentration of Na, K, and Li in the outer layer 21 of the quartz glass crucible (average concentration in the direction of the crucible wall thickness) and the concentration in the inner layer 22 (concentration at a position 1 mm away from the inner surface of the quartz glass crucible 10). The correlations shown in these figures are measured by making a quartz glass crucible 10 with an outer diameter of 32 inches (800 mm) and making samples from the quartz glass crucible. As can be seen from these figures, when the Na content in the outer layer 21 is less than 10 mass ppb, the Na content in the inner layer 22 can be set to less than 5 mass ppb, when the K content in the outer layer 21 is less than 50 mass ppb, the K content in the inner layer 22 can be set to less than 5 mass ppb, and when the Li content in the outer layer 21 is less than 180 mass ppb, the Li content in the inner layer 22 can be set to less than 100 mass ppb.
[0045] On the other hand, the average concentration of Na, K and Li in the wall thickness direction of the straight tube portion 14 of the outer layer 21 of the quartz glass crucible 10 of the present invention preferably satisfies at least one of the following concentrations: Na is 10 mass ppb or more; K is 50 mass ppb or more; Li is 180 mass ppb or more. In the straight tube portion 14, in order to suppress the quartz glass crucible 10 from tipping over or sinking inward when heated at high temperature, it is preferable to set the lower limit of the concentration of the impurity elements as described above. However, in the inner layer 22 of the quartz glass crucible 10, since the above-mentioned high purity requirement needs to be met, it is best not to make the concentration of the impurity elements too high even in the straight tube portion 14 of the outer layer 21 so as not to be contaminated by diffusion.
[0046] The reason for dividing the bottom 12 to R portion 13 and the straight tube portion 14 in the outer layer 21 in this way is that, in particular, the bottom 12 to R portion 13 of the quartz glass crucible has a long contact time with the silicon melt, so the diameter of the brown ring is easier to expand than the straight tube portion 14. Therefore, by reducing the Na, K, and Li concentrations on the inner surface of the bottom 12 to R portion 13 to promote crystallization in the depth direction of the brown ring, the release of bubbles generated inside the brown ring can be suppressed. In addition, by reducing only the Na, K, and Li concentrations of the outer layer 21 of the bottom 12 to R portion 13, the deformation of the straight tube portion 14 when using the quartz glass crucible 10 can be suppressed, and pinhole defects can be suppressed.
[0047] In addition, the present invention can be suitably applied to a quartz glass crucible 10 with an outer diameter of 800 mm or more. Such a quartz glass crucible 10 can pull a single crystal silicon ingot of a larger diameter, and can pull a quartz glass crucible that can suppress the occurrence of pinholes even in such a large diameter single crystal silicon ingot. The specifications for pinholes in single crystal silicon wafers with a diameter of 12 inches (300 mm) or more are relatively strict, and the quality requirements for the quartz glass crucible with an outer diameter of 800 mm or more used for the single crystal silicon wafer are also relatively high. In such a case, both the single crystal silicon wafer and the quartz glass crucible are large, and the probability of catching bubbles under the pulled single crystal silicon ingot is high, so it is necessary to apply this technology.
[0048] Hereinafter, the relationship between the state of the brown ring on the surface of the inner layer of the quartz glass crucible and the concentration of the impurity element in the inner layer of the quartz glass crucible will be described.
[0049] As described above, a brown ring called a "brown ring" was found to be generated on the inner surface of the quartz glass crucible due to contact with the silicon melt, and bubbles of several micrometers to tens of micrometers were confirmed inside the brown ring. When comparing the Na and K concentrations in the inner layer of the quartz glass crucible of less than 5 mass ppb and the Na and K concentrations in the inner layer of the quartz glass crucible of 50 mass ppb or more, it was found that the bubble diameter of the bubble was smaller when the Na and K concentrations in the inner layer of the quartz glass crucible were less than 5 mass ppb.
[0050] Figure 2 A photograph of a brown ring generated on the inner surface of a quartz glass crucible is shown in FIG. Figure 2 (a) shows the inner surface of a quartz glass crucible. Figure 2 The circular shape in (a) is the brown ring. The brown ring exists in a single independent case, and also exists in the case of Figure 2 (a) shows the case of multiple fusions. Figure 2 (b) Figure 2 (a) is a magnified view of a part of the image. Figure 2 As shown in (b), bubbles ranging from several micrometers to tens of micrometers in size can be confirmed inside the brown ring.
[0051] Figure 3 It is shown in Figure 2 (b) shows the diameter of the bubble inside the brown ring. Figure 3 In the graph, the concentration of impurity elements in the inner layer of the quartz glass crucible is compared between Na and K less than 5 mass ppb and Li less than 50 mass ppb and Na and K greater than 50 mass ppb and Li less than 50 mass ppb. As can be seen from the graph, when the Li concentration is less than 50 mass ppb, the bubble diameter becomes smaller if both the Na concentration and the K concentration are less than 5 mass ppb.
[0052] In addition, if Figure 4 As shown, it can be seen that for the bubbles, when the Li concentration in the inner layer of the quartz glass crucible is 180 mass ppb or more and when the Li concentration in the inner layer of the quartz glass crucible is less than 100 mass ppb, the number density of bubbles near the center of the brown ring is high when the Li concentration in the inner layer of the quartz glass crucible is less than 100 mass ppb. Among them, the high number density of bubbles means that the bubbles are not released and remain, which means that the bubbles exist in a deeper position and are not incorporated into the silicon melt.
[0053] Based on this finding, it can be seen that if the Na and K concentrations in the inner layer of the quartz glass crucible are less than 5 mass ppb and the Li concentration is less than 100 mass ppb, there are fewer pinholes with a size of several microns to tens of microns when pulling a single crystal silicon ingot.
[0054] Based on this, it is speculated that by reducing the concentration of Na and K in the inner layer of the quartz glass crucible, the bubble diameter can be reduced, and by reducing the Li concentration, the release of bubbles into the silicon melt can be suppressed, thereby improving the occurrence of pinholes in the pulled single crystal silicon ingot. To summarize the effects of the provisions of the impurity elements of the present invention, the advantage of setting Na and K to low concentrations is that the bubbles in the brown ring can be suppressed to a smaller size by reducing the concentrations of Na and K. In addition, the advantage of setting Li to a low concentration is that the crystallization in the depth direction of the brown ring is fast, and the bubbles generated by crystallization can be present in a relatively deep position, and the crystallization slows down the melting loss rate and the bubbles will not be released into the silicon melt.
[0055] As described above, the brown ring is generated by the crystallization of the inner surface of the quartz glass crucible, so it is estimated that the crystallization state varies depending on the Na, K, and Li concentrations on the inner surface of the quartz glass crucible. The lower the Na, K, and Li concentrations, the more the crystallization inside the brown ring, that is, the crystallization in the depth direction from the inner surface of the quartz glass crucible, will progress, and the melting loss to the silicon melt can be reduced. Therefore, as shown in the following experimental example, the uneven shape of the brown ring with a diameter of 12 mm generated in the quartz glass crucibles with different Na, K, and Li concentrations on the inner surface was measured using a surface roughness measuring machine.
[0056] [Experimental Examples 1 to 4]
[0057] Four types of quartz glass crucibles having different Na, K, and Li concentrations in the inner layer of the quartz glass crucible were prepared. The concentration of the impurity element at a depth of 1 mm from the inner surface of each quartz glass crucible was as follows.
[0058] Experimental Example 1: Na: 3 mass ppb, K: 1 mass ppb, Li: 200 mass ppb
[0059] Experimental Example 2: Na: 2 mass ppb, K: 3 mass ppb, Li: 200 mass ppb
[0060] Experimental Example 3: Na: 3 mass ppb, K: 2 mass ppb, Li: 70 mass ppb
[0061] Experimental Example 4: Na: 4 mass ppb, K: 1 mass ppb, Li: 70 mass ppb
[0062] The surface roughness measuring machine was used to measure the uneven shapes of the brown rings with a diameter of 12 mm produced in these quartz glass crucibles with different Na, K, and Li concentrations in the inner layer. The results are as follows Figure 8 shown.
[0063] Depend on Figure 8 It can be seen that the bulges in the case where the Na concentration and K concentration of the inner layer of the quartz glass crucible are less than 5 mass ppb and the Li concentration is less than 100 mass ppb (Experimental Examples 3 and 4) are about 10 to 20 μm higher than the case where the Na concentration and K concentration are less than 5 mass ppb and the Li concentration is more than 100 mass ppb (Experimental Examples 1 and 2). That is, when the Na concentration and K concentration are less than 5 mass ppb and the Li concentration is less than 100 mass ppb, the crystallization inside the brown ring can be promoted and the melting loss to the silicon melt can be suppressed. The melting loss difference of 10 to 20 μm is believed to affect the release of bubbles of several microns to tens of microns.
[0064] In addition, generally, if there is a large amount of alkali metal, the crystallization of quartz glass is promoted, but the opposite phenomenon occurs inside the brown ring generated by the reaction of quartz glass with a low metal concentration and silicon melt. Based on this, it is speculated that by setting the concentration of impurity elements in the inner layer of the quartz glass crucible to less than 5 mass ppb of Na, less than 5 mass ppb of K, and less than 100 mass ppb of Li, the crystallization inside the brown ring can be promoted and the exposure of bubbles inside the brown ring can be suppressed.
[0065] As described above, the quartz glass crucible that satisfies the concentration requirements of the impurity elements of the present invention can promote the crystallization of the brown ring in the depth direction during the pulling of the single crystal silicon ingot. As a result, the quartz glass crucible of the present invention can be defined in the following manner based on the brown ring after the single crystal silicon ingot has been pulled. That is, the quartz glass crucible of the present invention holds the silicon melt inside it, and after the single crystal silicon ingot is pulled from the silicon melt, a brown ring is formed on the inner surface of the quartz glass crucible, and preferably, the density of bubbles with a diameter of 3.0 μm or more in the inner layer within the inner region of the brown ring is 4.0 bubbles / mm 2 The above is the result. A quartz glass crucible having such a brown ring formed on the inner surface of the quartz glass crucible after pulling a single crystal silicon ingot can more effectively suppress pinholes in the pulled single crystal silicon ingot.
[0066] In addition, single crystal silicon ingots are often pulled by a multiple pulling method in which multiple ingots are pulled from a single quartz glass crucible. However, the regulation of the bubbles of the brown ring after pulling in the quartz glass crucible of the present invention is the regulation after the first single crystal silicon ingot is pulled. In this case, the use time of the quartz glass crucible is about several tens of hours to 100 hours. This is because when multiple ingots are pulled, the use time will be prolonged, and sometimes the brown ring generated for the first time will disappear.
[0067] In addition, the quartz glass crucible of the present invention holds the silicon melt inside it, and after a single crystal silicon ingot is pulled from the silicon melt, a brown ring is formed on the inner surface of the quartz glass crucible, but it is preferred that the height of the convex portion of the brown ring satisfies the following regulations at this time. That is, it is preferred to form the following brown ring: when the bisector along the circumferential direction of the quartz glass crucible is defined as the outer diameter reference line of the brown ring, the length of the outer diameter reference line is within the range of 10 mm to 13 mm. In addition, it is preferred that when the length of the outer diameter reference line of the brown ring is set to x (mm), the uppermost portion of the end of the outer diameter reference line of the brown ring is taken as the reference height 0 (μm), and the height of the convex portion of the uppermost portion on the outer diameter reference line as the inner area of the brown ring is set to y (μm), in the brown ring in which the length of the outer diameter reference line is within the range of 10 mm to 13 mm, the following formula (1) is satisfied:
[0068] y≥10x-70 ・・・(1).
[0069] The quartz glass crucible having such a brown ring formed thereon can more effectively suppress pinholes in the pulled single crystal silicon ingot.
[0070] A more detailed description is given below. Fig. 9 The density, outer diameter or reference height of the bubbles inside the brown ring in the present invention is Fig. 9 Individual brown rings are shown as objects. Rings formed by combining multiple brown rings are not used in the calculation of these values.
[0071] Fig. 9The figure shows the direction from the bottom side of the quartz glass crucible to the end face side of the crucible (the upper end side of the straight tube), that is, the vertical direction. The so-called bisector along the circumferential direction of the crucible is a line that divides the brown ring into two with a plane that is perpendicular to the vertical direction of the quartz glass crucible. The outer diameter reference line represents the line segment between the two points where the above-mentioned bisector intersects with the outer periphery of the brown ring. In the present invention, it is preferred to form a brown ring in which the length of the outer diameter reference line after pulling the first single crystal silicon ingot is in the range of not less than 10 mm and not more than 13 mm. The length of the outer diameter reference line can also be said to be the outer diameter of the brown ring. Since the brown ring is not limited to forming a complete circle, it is defined in this way.
[0072] The uppermost part of the end of the outer diameter reference line of the brown ring is the higher of the above two points. Figure 8 This is explained. Figure 8 The figure shows the inner surface of the quartz glass crucible measured by a surface roughness measuring machine. Fig. 9 The result is the height of the brown ring. Figure 8 The top of the end of the outer diameter reference line shown on the right side is set as the reference height 0 (μm). The height of the convex portion which is the top of the outer diameter reference line of the inner area of the brown ring is set as y (μm). Figure 8 In Experiment 4, the length of the outer diameter reference line is about 12.2 mm. In addition, the position of the reference height 0 (μm) is located at about 15.5 mm on the horizontal axis of the figure. Since this position is set as the reference height 0 (μm), the height of the uppermost portion of the outer diameter reference line located at about 10 mm on the horizontal axis of the figure is about 54 μm. That is, y=54, x=12.2, satisfying equation (1).
[0073] The convex shape of the brown ring is presumed to be caused by the fact that the melting of the silicon melt is accompanied by the progress of crystallization, and the crystallized part is spared from melting, resulting in a convex shape. Figure 8 The portion on the left side of the maximum value of the curve of each experimental example in is melted due to the flow of the silicon melt, and it is estimated that this causes most of the brown portion (crystallized portion) to disappear.
[0074] [Method for manufacturing quartz glass crucible]
[0075] The quartz glass crucible of the present invention can be manufactured by a known method except for controlling the concentration of impurity elements in the inner layer and the outer layer. For example, it can be manufactured by a method called arc rotary melting method. At this time, first, silicon dioxide powder (silicon dioxide powder, quartz powder) as a raw material powder is supplied to a rotating mold, and then formed into a crucible-shaped molded body by centrifugal force. Then, the molded body is heated and melted from the inside by an arc flame to form a translucent quartz glass crucible base (outer layer) (base forming process). Furthermore, during or after the formation of the crucible base, silicon dioxide powder is re-supplied into the heated atmosphere in the crucible base to form a transparent quartz glass inner layer on the inner side of the crucible base (inner layer forming process). The method of forming an inner layer composed of transparent quartz glass by scattering quartz powder while heating is also called a scattering method. In addition, for example, the concentration of impurity elements in the inner and outer layers can be adjusted by adjusting the concentration of impurity elements in the raw material powder of each layer.
[0076] Example
[0077] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the examples.
[0078] [Examples 1 to 3, Comparative Examples 1 to 4]
[0079] A quartz glass crucible with an outer diameter of 800 mm was manufactured by an arc rotary melting method. At this time, the impurity concentration of the inner layer, the impurity concentration in the outer layer (R portion and bottom), and the impurity concentration in the outer layer (straight tube portion) of the manufactured quartz glass crucible were adjusted as shown in Table 1. That is, the impurity concentrations shown in Table 1 are the concentrations of various parts of the quartz glass crucible before the single crystal silicon ingot is pulled (unit: mass ppb). In addition, as mentioned above, the impurity concentration of the inner layer is the concentration at a position 1 mm away from the inner surface of the quartz glass crucible, and the impurity concentration of each part of the outer layer is the average concentration in the wall thickness direction.
[0080] Next, the manufactured quartz glass crucible is used to pull up a single crystal silicon ingot. The brown ring generated on the inner surface of the quartz glass crucible after the first single crystal silicon ingot is pulled up is observed. As the observed brown ring, a brown ring whose length of the outer diameter reference line is in the range of 10 mm to 13 mm is selected. As the state of the bubbles in the inner layer in the inner area of the brown ring, the bubble diameter of the largest bubble among the bubbles contained and the density of bubbles with a diameter of 3.0 μm or more in the brown ring are shown in Table 2. In addition, the length x of the outer diameter reference line in the above formula (1) obtained by observing the brown ring and the height y of the convex portion which is the height of the uppermost part on the outer diameter reference line are also shown in Table 2. In addition, the state of the pinhole generated after the first single crystal silicon ingot is pulled up is shown in Table 2 as a "pinhole score". The evaluation of the pinhole score is divided into three levels of "particularly good", "good" and "unqualified". Here, for convenience, it is described as follows. Among the pinholes detected when making single crystal silicon wafers from single crystal silicon ingots, based on Comparative Example 1, those above that number are set as "unqualified", those less than half of the "unqualified" numbers are set as "good", and those less than half of the "good" numbers are set as "particularly good".
[0081] [Table 1]
[0082]
[0083] [Table 2]
[0084]
[0085] As shown in Tables 1 and 2, when the impurity concentrations of Na, K and Li in the inner layer are less than 5 mass ppb for Na, less than 5 mass ppb for K and less than 100 mass ppb for Li, and the concentrations of Na, K and Li in the R part and the bottom of the outer layer are less than 10 mass ppb for Na, less than 50 mass ppb for K and less than 180 mass ppb for Li, the pinhole performance is good. In addition, when such impurity concentration requirements are met, the density of bubbles with a diameter of 3.0 μm or more in the brown ring can be made 4.0 / mm 2 As a result, a high number density indicates that the bubbles are not released and remain, which means that the bubbles are present at a deeper position in the brown ring and are not incorporated into the silicon melt. In addition, as can be seen from Table 2, in Examples 1 to 3, the brown rings whose outer diameter reference line length is within the range of 10 mm to 13 mm satisfy the above formula (1), and the pinhole results are "particularly good" or "good". On the other hand, Comparative Examples 1 to 4 do not satisfy the above formula (1).
[0086] In addition, in the outer layer of the manufactured quartz glass crucible, the impurity elements in the straight tube portion have a relatively high concentration (satisfying any one of Na being 10 mass ppb or more, K being 50 mass ppb or more, and Li being 180 mass ppb or more) in any of the embodiments and comparative examples, so that tipping and sinking are suppressed.
[0087] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any embodiments having substantially the same configuration and exhibiting the same functions and effects as the technical concept described in the claims of the present invention are all within the technical scope of the present invention.
Claims
1. A quartz glass crucible for pulling a single crystal silicon ingot, which has a crucible shape consisting of a straight tube portion, an R portion and a bottom portion, and has an outer layer consisting of an opaque quartz glass containing bubbles, and an inner layer consisting of a transparent quartz glass with a wall thickness of 1.5 mm or more, The quartz glass crucible for pulling a single crystal silicon ingot is characterized in that: Regarding the concentrations of Na, K and Li in the inner layer at a position 1 mm away from the inner surface of the quartz glass crucible, Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 100 mass ppb, The average concentrations of Na, K, and Li in the wall thickness direction of the R portion and the bottom of the outer layer are less than 10 mass ppb for Na, less than 50 mass ppb for K, and less than 180 mass ppb for Li.
2. The quartz glass crucible for pulling a single crystal silicon ingot according to claim 1, characterized in that: Regarding the concentrations of Na, K and Li in the inner layer at a position 1 mm away from the inner surface of the quartz glass crucible, Na is less than 5 mass ppb, K is less than 5 mass ppb, and Li is less than 50 mass ppb, The average concentrations of Na, K, and Li in the wall thickness direction of the R portion and the bottom of the outer layer are less than 5 mass ppb for Na, less than 50 mass ppb for K, and less than 100 mass ppb for Li.
3. The quartz glass crucible for pulling a single crystal silicon ingot according to claim 1 or 2, characterized in that: The average concentrations of Na, K and Li in the wall thickness direction of the straight tube portion of the outer layer satisfy at least one of the following concentrations: Na is 10 mass ppb or more; K is 50 mass ppb or more; Li is 180 mass ppb or more.
4. The quartz glass crucible for pulling a single crystal silicon ingot according to any one of claims 1 to 3, characterized in that: The outer diameter of the quartz glass crucible is greater than 800 mm.
5. The quartz glass crucible for pulling a single crystal silicon ingot according to any one of claims 1 to 4, characterized in that: The quartz glass crucible holds the silicon melt therein, and after a single crystal silicon ingot is pulled out from the silicon melt, a brown ring is formed on the inner surface of the quartz glass crucible. The density of bubbles with a diameter of 3.0 μm or more in the inner layer within the inner region of the brown ring is 4.0 bubbles / mm 2 above.
6. The quartz glass crucible for pulling a single crystal silicon ingot according to any one of claims 1 to 5, characterized in that: The quartz glass crucible holds a silicon melt therein, and after a single crystal silicon ingot is pulled from the silicon melt, a brown ring is formed on the inner surface of the quartz glass crucible. When a bisector of the brown ring along the circumferential direction of the quartz glass crucible is defined as an outer diameter reference line of the brown ring, the length of the outer diameter reference line is within a range of 10 mm to 13 mm. When the length of the outer diameter reference line of the brown ring is set to x (mm), The uppermost part of the end of the outer diameter reference line of the brown ring is taken as the reference height 0 (μm). When the height of the convex portion which is the height of the uppermost portion on the outer diameter reference line of the inner region of the brown ring is y (μm), In the brown ring where the length of the outer diameter reference line is within the range of 10 mm to 13 mm, the following formula (1) is satisfied: y≥10x-70 ・・・(1)。
Citation Information
Patent Citations
A silica container for pulling up monocrystalline silicon and method for manufacturing same
WO2013140706A1