Coating on inner surface of particle containing chamber
By depositing high thermal conductivity diamond or round-grain diamond coatings on the interior surface of the plasma accommodating chamber, absorbing and managing X-ray radiation, the problem of excessive heat generation of the wall in the plasma accommodating chamber is solved, and the thermal management and material protection effect of the system is improved .
Patent Information
- Application Number
- CN202380021444.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-16
- Filing Date
- 2023-02-16
- Publication Date
- 2024-11-26
AI Technical Summary
In the plasma storage chamber, excessive heat generation and potential damage caused by high-energy X-ray radiation makes it difficult for the prior art to effectively manage heat accumulation and material protection.
Coatings with high thermal conductivity and long X-ray penetration depths, such as diamond or round diamond coatings, are deposited on the inner surface of the plasma accommodating chamber, absorbing X-rays and conducting heat through them, reducing wall temperature.
Effectively absorb X-rays, reduce wall temperature peaks, extend the service life of the coating, improve the thermal management capabilities of the system, and extend the operating time.
Smart Images

Figure CN119032412A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority under 35 U.S.C. §119(e) to U.S. Provisional Application Serial No. 63 / 310,793, filed on February 16, 2022, entitled “Bort Coatings on Inner Surfaces of Plasma Confinement Chambers,” which is incorporated herein by reference in its entirety. Background Art
[0003] Electrons with keV energies (e.g., 1 keV to 10 keV) can emit bremsstrahlung radiation in the form of high-energy X-rays, for example, when interacting with other charged particles such as atomic nuclei. Such high-energy X-ray emission can also come from activation decay, synchrotron radiation, cyclotron radiation, and beta decay. In addition, electron excitation during ionization or recombination may also generate high-energy photons, such as X-rays.
[0004] Plasma containment chambers can be used to generate energetic particles and can also be used to accelerate particles or objects to high speeds. Energetic particles such as high-energy electrons and ions can generate significant electromagnetic radiation when interacting with other charged particles and can also interact with magnetic fields (e.g., in a bremsstrahlung process). Strong magnetic or electric fields can be used to confine and accelerate energetic particles and / or plasma. In some cases, the electromagnetic radiation and energetic particles generated may heat and / or degrade the wall surfaces of the plasma containment chamber to the extent that the wall surfaces must be replaced in order for the system to operate correctly. Summary of the invention
[0005] The described technology relates to a particle manipulation system and a particle holding chamber, an example of which is a plasma holding chamber. The particle manipulation system can move, accelerate, and decelerate particles, such as electrons, ions, and / or atoms of a plasma. The particle holding chamber can be configured to hold high-energy particles, such as accelerated electrons, ions, and atoms of a plasma, which can produce energy radiation, such as X-rays and / or gamma rays. In some cases, the energy atoms in the plasma can undergo fusion, thereby releasing gamma rays and high-energy particles, which can cause X-rays to be produced. The radiation can be absorbed by a coating on the inner surface of the particle holding chamber, which alleviates excessive and potentially destructive heating of the inner surface of the chamber that would otherwise occur without the coating.
[0006] Some embodiments relate to a method of containing a plasma in a plasma chamber. The method may include the following acts: injecting plasma into the plasma chamber; applying a magnetic field to the plasma to manipulate the plasma; receiving electromagnetic radiation including X-rays from the plasma in a coating deposited on an inner surface of a wall of the plasma chamber facing the plasma, a portion of the X-rays having a certain energy range, wherein the thickness of the coating is at least half of the penetration depth of the portion of the X-rays having the energy range, and wherein, in the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 millimeter of the inner surface of the wall.
[0007] Some embodiments relate to a plasma chamber to contain a plasma. The plasma chamber may include: a wall surrounding a volume that contains the plasma when the plasma chamber is in operation; and a coating in thermal communication with an inner surface of the wall, the coating being configured to receive electromagnetic radiation including X-rays from the volume. A portion of the X-rays may have an energy range. A first thermal conductivity of the coating may be greater than a second thermal conductivity of the wall of the plasma chamber. The coating may have a thickness that is at least half of a penetration depth of X-rays in the energy range, and in the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 millimeter of the inner surface of the wall.
[0008] Some embodiments relate to a system comprising: a plasma chamber having walls extending around an interior volume, the plasma chamber adapted to support a vacuum in the interior volume, the walls of the plasma chamber having a relative humidity of no greater than 5 W m -1 K -1a thermal conductivity of ; a plasma source, the plasma source being used to generate plasma and inject the plasma into the interior volume of the plasma chamber; at least one gas inlet, the at least one gas inlet being coupled to the plasma source to introduce a gas or a gaseous mixture into the plasma source; and a plurality of electromagnetic coils, the plurality of electromagnetic coils being arranged to generate a magnetic field within the plasma chamber, such that interaction of particles of the plasma with the magnetic field produces electromagnetic radiation including X-rays. A first portion of the X-rays may be absorbed by a wall of the plasma chamber to cause heating of the wall. The plasma chamber may also include a coating, the coating including at least one of boron nitride, graphite, or diamond, wherein the coating is disposed on an inner surface of the wall of the plasma chamber to absorb at least a second portion of the X-rays included in the first portion of the X-rays, such that local peak heating of the wall near the inner surface that occurs during operation of the system due to absorption of the first portion of the X-rays is reduced compared to absorption of the first portion of the X-rays that would occur in the absence of the coating.
[0009] Some embodiments relate to a method of depositing a coating on an inner surface of a wall of a plasma chamber, wherein electromagnetic radiation including X-rays is incident on the coating, wherein a portion of the X-rays has a certain energy range. The method may include the following actions: heating the plasma chamber so that the inner surface of the wall is at a temperature of 300° C. to 2500° C.; and introducing a gas mixture into the plasma chamber. The gas mixture may include: a first gas including a hydrocarbon; and a second gas including at least one of protium or deuterium. The method may also include the following actions: generating a plasma in the plasma chamber; and depositing the coating on the inner surface of the wall. The coating may include at least one of diamond, graphite, or bobbin diamond. The coating may be deposited to a thickness of at least half of the penetration depth of the portion of the X-rays having the energy range. In the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 mm of the inner surface of the wall.
[0010] Some embodiments relate to a method of refurbishing a coating on an inner surface of a plasma confinement system. The plasma confinement system may include: a plasma chamber having a bobby diamond coating on at least a portion of the inner surface of the plasma chamber, wherein the bobby diamond coating is arranged to receive X-rays having a certain energy range from a plasma confined by the plasma confinement system. The method may include the following actions: purging the plasma chamber to remove any residual gas; heating the inner surface of the plasma chamber to a temperature in the range of 300° C. to about 2500° C.; and introducing a gas mixture into the plasma chamber. The gas mixture may include: a first gas including a hydrocarbon; and a second gas including at least one of protium or deuterium. The method may also include the following actions: generating a plasma in the plasma chamber by applying radio frequency electromagnetic waves to dissociate and ionize the gas mixture; and depositing additional bobby diamond on the bobby diamond coating to refurbish the bobby diamond coating on the inner surface of the plasma chamber, so that the refurbished bobby diamond coating absorbs at least half of the X-rays having the energy range.
[0011] All combinations of the foregoing concepts and the additional concepts discussed in more detail below (assuming these concepts are not mutually inconsistent) are part of the inventive subject matter disclosed herein. In particular, all combinations of the claimed subject matter appearing at the end of this disclosure are part of the inventive subject matter disclosed herein. Terms used herein that may also appear in any disclosure incorporated by reference should be given the meaning most consistent with the specific concepts disclosed herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Those skilled in the art will appreciate that the drawings are primarily for illustrative purposes and are not intended to limit the scope of the inventive subject matter described herein. The drawings are not necessarily drawn to scale; in some cases, various aspects of the inventive subject matter disclosed herein may be shown exaggerated or enlarged in the drawings to facilitate understanding of different features. In the drawings, similar reference characters generally refer to similar features (e.g., functionally and / or structurally similar elements).
[0013] Figure 1A An example of a particle manipulation system with a plasma containment chamber is shown.
[0014] Figure 1B Depicted is a chamber having a coating applied to the inner surface of the chamber wall. Figure 1A part of a tubular chamber.
[0015] Figure 2A X-ray penetration depths in quartz and diamond are shown.
[0016] Figure 2BAn exemplary energy spectrum of X-rays having a range of energies is depicted.
[0017] Figure 3 A diamond or bobby diamond deposition scheme is shown.
[0018] Figure 4 A particle manipulation system configured for in-situ deposition of a coating on an interior surface of a containment chamber is shown.
[0019] Figure 5 A cross section of a plasma containment chamber having a bobby diamond coating is shown.
[0020] Fig. 6A A cross section of a plasma containment chamber with a passage through the chamber wall is shown.
[0021] Figure 6B A cross section of a plasma containment chamber having a chamber wall formed in multiple segments is shown.
[0022] Fig. 7A A cross section of a plasma containment chamber having a multi-layer coating is shown.
[0023] Figure 7B A cross section of a portion of a wall of a plasma containment chamber having a multi-layer coating is shown. DETAILED DESCRIPTION
[0024] 1. Plasma confinement and thermal management
[0025] Plasma confinement is the spatial extent of limiting plasma in at least one dimension within a vacuum environment, wherein confinement is usually achieved by applying electric and / or magnetic fields to the vacuum environment. Plasma can be constrained and manipulated (e.g., translated, accelerated, decelerated, compressed and expanded) to change its density and energy. Compression can be used to heat the plasma to very high temperatures (e.g., more than 100 million degrees or more) by adding energy to the plasma, reducing the available volume and increasing the probability of collisions between particles in the plasma. This in turn can promote the ionization of the particles of the plasma so that it can increase the ion lifetime in the plasma. Plasma confinement and manipulation can be used for various research and manufacturing applications, including but not limited to plasma reactions (e.g., chemical or atomic reactions), particle and object acceleration systems (e.g., for basic research or generation of industrial or medical isotopes) and material deposition (e.g., chemical vapor deposition).
[0026] The particle manipulation system can use a strong magnetic field (e.g., a peak field value between 0.01 Tesla (T) and 50 T) to constrain and (if necessary) increase the kinetic energy of the particles. The strong magnetic field can be generated by a plurality of magnetic coils arranged around the particle holding chamber to cooperatively generate a magnetic field in the chamber. For example, the chamber can be a tube, a ring, a sphere, or a box. In order to cooperatively generate a magnetic field, the magnetic coils are spaced sufficiently close to each other so that the magnetic field generated by any one coil is added to the magnetic field generated by at least one other coil in the system.
[0027] Alternatively or in addition to using a magnetic field, a particle manipulation system can use an electric field to confine and / or manipulate particles (e.g., to increase the kinetic energy of a plasma or particle). For example, an inertial confinement system uses an electric field to confine a plasma, rather than using a magnetic field for confinement. Many inertial electrostatic confinement systems pull electrons or ions through a potential well, beyond which the electric potential drops, and the particle continues to move due to its inertia. To create a potential well, an inertial electrostatic confinement system can include an arrangement of conductive wire grids (e.g., two concentric spherical grids of metal wire). These confinement systems can also use electron guns instead of or in addition to an electrical grid. Examples of systems that use electric fields to confine or increase the kinetic energy of a plasma or particle include some ion engines (also called thrusters), vacuum tubes, electron guns, and accelerators that use alternating electric fields.
[0028] In other cases, some particle manipulation systems combine magnetic fields and electric fields to confine and / or manipulate particles. Examples of such systems include polyhedral potential wells and Penning traps. Lasers, neutral beam injection, and / or directed radio frequency (referred to as RF heating) may also be used with any of the above systems to accelerate charged particles to high energy states in a plasma confined by a magnetic field or electric field. In any of these systems, the chamber containing the vacuum and plasma may still be a tube, torus, sphere, box, or other arrangement.
[0029] Figure 1AAn example of a particle manipulation system 200 configured to confine and manipulate a plasma 205 is depicted. The system 200 includes a tubular chamber 250 in which the plasma 205 is confined by a magnetic field. The system 200 also includes electromagnetic coils 230-1, 230-2, 230-3 (collectively referred to as 230) surrounding the tubular chamber 250 to generate a magnetic field within the chamber 250. The system may also include electronic circuits (e.g., power supply circuits 220) and controllers 210 to drive current through the coils 230 to generate a magnetic field within the tubular chamber 250. Additional details of the exemplary particle manipulation system 200 are described in International Application PCT / US2022 / 032276, entitled "Apparatus and Methods for Generating a Pulsating, High-Strength Magnetic Field," filed on June 3, 2022, which is incorporated herein by reference in its entirety.
[0030] Plasma confinement using a magnetic field can benefit from chamber walls 252 formed of dielectric and / or non-magnetic materials that do not interfere with the magnetic field that passes through the chamber walls 252 to confine the plasma 205. The dielectric and / or non-magnetic materials may also have certain other desirable characteristics for use in a plasma environment, such as vacuum compatibility, sputtering resistance, and / or mechanical durability. Currently, cost-effective materials that are dielectric and have these characteristics (e.g., some ceramics, silicon dioxide, and graphite) have low thermal conductivity (e.g., less than 5 Watts / meter / Kelvin (W m -1 K -1 )), and therefore cannot easily dissipate the heat that may be generated within the tubular chamber 250. For example, the chamber wall 252 may be made of a material having a thermal conductivity of no greater than 5 W m -1 K -1 , not more than 3W m -1 K -1 or even no more than 1.5W m in some cases -1 K -1 of material formation.
[0031] The tubular chamber 250 that contains at least one plasma 205 during operation of the system 200 can have one or two open ends or openings (e.g., for injection and removal of the plasma). The tubular chamber 250 can have one or more cross-sectional shapes (e.g., circular, oval, square, hexagonal, polygonal, etc.). In some embodiments, the tubular chamber 250 is part of a larger vacuum chamber 260 in which the tubular chamber 250 is connected. In some cases, the chamber 250 can be formed as a ring with its ends joined together (e.g., as a circular ring). In addition, the tubular chamber 250 can be formed from multiple pieces joined together using a sealant to form a vacuum-compatible assembly, such as in conjunction with international patent application PCT / US2022 / 079394, entitled “Ceramic Fibers for Shielding in Vacuum Chamber Systems and Methods for Using Same,” filed on November 7, 2022. Figures 1A to 3 D, which application is incorporated herein by reference.
[0032] During operation of the system 200, the plasma 205 may contain energetic charged particles (e.g., ions, electrons) that may be ejected toward the interior surfaces of the chamber 250. When the charged particles strike the interior surfaces of the chamber 260, contaminants may be sputtered off the interior surfaces of the chamber and enter the plasma 205. Such contaminants may adversely affect the handling or use of the plasma 205.
[0033] The generation of contaminants can be reduced by forming the chamber walls 252 from a material that is more resistant to sputtering when exposed to charged particles ejected from the plasma 205. Furthermore, in applications where plasma manipulation includes chemical or nuclear reactions that are sensitive to the presence of specific contaminants, the material forming the chamber walls 252 can be selected such that, if contaminants are generated, the composition of the contaminants does not or minimally reacts with the plasma 205 in an undesirable manner.
[0034] For example, in some applications, the plasma 205 contains primarily hydrogen and helium ions (some of which may fuse together to release energy). Under these conditions, the chamber wall 252 may preferably be formed of a material that does not contain heavy elements, such as tungsten, that may otherwise remove thermal energy from the plasma. If the magnetic field generated by the coil 230 is used to modify the shape of the plasma 205, the chamber wall 252 may be at least partially formed of a dielectric so that the chamber wall 252 does not act as an electrical conductor that affects the transmission and / or spatial distribution of the magnetic field in the tubular chamber 250 that confines the plasma 205. Examples of materials that may be used to form the chamber wall 252 include, but are not limited to, silicon dioxide (SiO2) and sapphire (Al2O3), which may produce fewer contaminants than, for example, metals and elastomers.
[0035] In some embodiments, the chamber wall 252 can be formed of a combination of materials that can include dielectric materials, ceramics, and / or graphite materials. Advantageously, the chamber wall 252 is vacuum compatible (e.g., having at least a surface material with a sufficiently low outgassing rate to allow a vacuum level to be established within the chamber to at least the millitorr level or lower or even to 10 -6 Torr or lower). For example, chamber wall 252 may include quartz glass, graphite, silicon, silicon dioxide, silicon nitride, boron nitride, or boron carbide; preferably silicon dioxide. If chamber wall 252 includes silicon dioxide, the silicon dioxide may include fully single crystal quartz or fully fused silica glass. In some cases, silicon dioxide and / or another material may be applied to chamber wall 252 as a coating 253, such as Figure 1B For example, coating 253 may include silicon dioxide melted on inner layer 256 and sintered on outer layer 254 contacting chamber wall 252, such as Figure 1B A heat sink 270 (eg, including pipes or lines for coolant flow) may be placed in thermal contact with the chamber wall 252 .
[0036] As described above, the tubular chamber 250 can be part of a larger vacuum chamber 260 having at least one first port 282 to allow gases, particles, and / or plasma to move into and / or out of the tubular chamber 250. For example, the larger vacuum chamber 260 can include at least one plasma source 290 to form and inject at least one plasma into the tubular chamber 250. The chamber 250 can have separate ports for different gases, particles, and / or plasmas. The chamber 250 can have a second port 284 for introducing gases, particles, and / or plasmas into and / or removing them from the tubular chamber 250. The tubular chamber 250 and / or the vacuum chamber 260 can be fluidly coupled to at least one vacuum pump (not shown) via at least one port to create a vacuum environment within the tubular chamber 250 that will support the plasma. In some cases, at least one port on the tubular chamber 250 can serve as both an inlet port and an outlet port for exchanging at least one of the gases, plasmas, and / or particles. In some cases, the inlet and outlet can be connected to or include valves (eg, to close and form a vacuum seal at the ports).
[0037] The chamber wall 252 can have a thickness sufficient to provide structural stability to withstand mechanical forces applied via a vacuum (e.g., 15 psi or more if the external pressure is greater than the atmosphere) while allowing the magnetic field to effectively pass through its wall 252. In some applications, the wall material is silicon dioxide and the wall thickness is about 5 mm to about 10 mm. The wall thickness can depend at least in part on the size and shape of the chamber. For example, a tubular chamber 250 in the shape of a cylinder with a larger radius R can have thicker walls than a comparable cylindrical chamber with a smaller radius R for structural reasons. If the tubular chamber 250 has a flat surface (as occurs with a hexagonal cross section), the wall thickness can be greater than a tubular chamber 250 of the same diameter with a circular cross section. For example, for a system measuring a length from about or exactly 0.1 meters to about or exactly 6 meters and a width from about or exactly 0.01 meters to about or exactly 3 meters (e.g., a diameter with a circular cross section), the wall thickness is at least about 1 mm to about 10 mm. Although the chamber wall 252 can be made thicker than necessary to withstand the atmospheric pressure acting on the tubular chamber or other considerations (e.g., earthquakes), due to cost and weight considerations, among other reasons, it may be beneficial to reduce the wall thickness to a value sufficient to withstand the application of atmospheric pressure acting on the chamber wall 252. Another consideration is heat transfer through the chamber wall 252, as discussed further below. Reducing the wall thickness can improve heat transfer through the chamber wall 252 to the heat sink 270 located on the exterior of the chamber wall.
[0038] Each of the electromagnetic coils 230 may be fed with current from one or more power supply circuits 220-1, 220-2, 220-3 (only one power supply circuit is shown for each electromagnetic coil to simplify the illustration). Figure 1A 230). Current may be provided on one or more power supply lines 225 connected to each coil. For some applications, the peak amount of current delivered to each electromagnetic coil may be between 1 ampere (A) and 200,000,000 A. If other restraining or accelerating devices (e.g., electrodes or lasers) are used in addition to or in place of the electromagnetic coil 230, they may be driven by the power supply circuit 220 and the controller 210.
[0039] Each of the power supply circuits 220 may include a power source (e.g., a voltage source), at least one energy storage component (e.g., a capacitor), and at least one switch that controls the flow of current from the at least one energy storage component to the associated electromagnetic coil. The switches in each power supply circuit may be controlled independently of the switches in the other power supply circuits 220 in the system. In this way, the current waveform and the timing of the waveform delivered to each of the electromagnetic coils 230 may be controlled to a large extent independently of the current delivered to the other electromagnetic coils 230 in the system 200. This may provide pulsing of the electromagnetic coils to accelerate the plasma. In some cases, the structural limitations of the system 200 may limit the amount of variation in amplitude, waveform, and / or timing between two or more of the electromagnetic coils 130. In practice, the electromagnetic coils may also be operated at a steady-state capacity to confine the plasma, and the charged particles therein may be accelerated or heated by alternative means, including by lasers, neutral beam injection, or RF heating.
[0040] The controller 210 can communicate with at least one of the power supply circuits 220 to control the delivery of current from the at least one power supply circuit to one or more of the electromagnetic coils 230 (e.g., by activating a switch of the power supply circuit). In some cases, the controller 210 can include a computer. In other cases, the controller can include a field programmable gate array, a programmable logic circuit, an application specific integrated circuit, a digital signal processor, a logic circuit, an analog circuit, or some combination thereof.
[0041] In some cases, control of the current delivery to the electromagnetic coil 230 can be distributed in the power supply circuit or in the trigger control circuit connected to the power supply circuit. For example, the controller 210 can issue a command to deliver current to the first coil 230-1. The command can be received by the first power supply circuit 220-1 or the trigger control circuit connected to the first power supply circuit. Similarly, the controller 210 can issue a command to deliver current to other coils 230 in the system. Once the first coil 230-1 is triggered, the trigger control circuit can issue a trigger command to one or more other power supply circuits 220 or trigger control circuits connected to other power supply circuits 220. In this way, all electromagnetic coils can be triggered. Utilizing Figure 1AThe particle manipulation system 200 can (at least to some extent) independently control the energization of each of the electromagnetic coils 230. Through such independent control of the amplitude, waveform, and timing of the current delivered to each of the electromagnetic coils 230, a dynamic and pulsating strong magnetic field can be generated in the chamber 250. Because the electromagnetic coils 230 are independently controlled, the strength and shape of the local electric and magnetic fields in the chamber 250 are highly adjustable.
[0042] Without being particularly limited by any theory, during confinement, compression and / or acceleration of the plasma or particles within the particle manipulation system 200, the interior walls of the chamber may be exposed to bombardment by high-energy particles and / or radiation, including, in particular, bremsstrahlung in the form of X-ray radiation and even gamma-ray radiation in some cases. Electrons operating in the keV range (e.g., 1 keV to 10 keV, including 5 keV) emit bremsstrahlung in the form of high-energy X-rays (e.g., having energies in excess of 1 keV). Other types of high-energy X-ray emission may also occur in these systems, including activation decay, synchrotron radiation, cyclotron radiation, and beta decay. In addition, electron excitation during ionization or recombination may also produce high-energy photons, such as X-rays. The X-ray radiation emitted during operation of the system 200 presents structural and operational challenges, as the X-rays may be absorbed by the chamber walls 252 and may generate high levels of heat in the chamber walls. Such high heat, if not dissipated quickly, may accumulate damage to the chamber walls and / or desorb contaminants from the chamber walls, which may interfere with the manipulation of the plasma 205 .
[0043] The average distance that X-ray radiation travels into the chamber wall before significant absorption occurs is described by the penetration depth, sometimes also called the skin depth. Figure 2A 430-1, 430-2 are defined as the distance d from the surface of the material upon which the radiation is incident to the location in the material where the intensity of the X-ray radiation 410 drops to 1 / e of its original value, or to about 37% of the initial value due to attenuation of the radiation in the material. The penetration depth depends largely on the wavelength of the incident radiation and the material properties (e.g., atomic number and density for absorbing the X-rays). Materials with higher atomic number elements and materials with higher densities generally have shorter penetration depths, primarily because there are more electrons per unit volume available to absorb the X-rays. For example, the penetration depth of 5 keV X-rays in silicon dioxide is about 40 μm.
[0044] When absorbed, X-ray energy is converted to heat, which for some applications may result in significant heating of the chamber. During operation of the system 200, pulsed or continuous X-rays may be emitted. If not carefully managed, excess heat from absorbed X-rays may result in dangerous temperature increases, which may cause material cracking or sublimation and system failure. Conventional thermal management within the system includes cooling the outer surface of the chamber using a high-speed cooling device (e.g., a liquid cooling pipe) that is thermally connected to the outer surface of the chamber. However, cooling the outer surface of the chamber is generally not sufficient to prevent a steady increase in the average temperature of the inner wall surface of the chamber wall 252 during operation of the system 200. The temperature increase may limit the system operating time - when the temperature limit is reached, operation is stopped to allow the system to cool.
[0045] Without being bound by any particular theory, a localized increase in temperature of the chamber wall 252 (e.g., near its inner surface) may indicate that the rate of heat transfer away from the chamber wall 252 is not fast enough to keep up with the rate at which the absorbed X-ray radiation is generating heat. The rate of heat transfer depends on the thermal conductivity of the chamber wall 252 and the distance that heat must be transferred to the outer chamber wall where the cooling line can provide the heat sink 270. As the thermal conductivity increases, the heat transfer rate increases. The heat transfer distance is determined by the thickness of the chamber wall 252 and the penetration depth 430-1, 430-2 of the X-ray radiation 410. As the penetration depth increases relative to the total chamber wall thickness, heat is deposited further into the chamber wall 252 and the heat transfer distance is effectively reduced.
[0046] As described above, for low energy X-rays, the penetration depth of 5 keV X-rays in silica is about 40 μm and less, which means that most of the X-ray energy in this energy range is absorbed within much less than 0.05 mm of a conventional chamber wall thickness of about 5 mm. This is less than 1% of the thickness of the chamber wall, and effectively means that if the incident X-ray spectrum consists essentially of X-rays with energies up to about 5 keV, all of the heat is deposited at the inner surface of the chamber wall 252. Since silica has a low thermal conductivity, it takes a long time for the heat generated by the absorption of X-rays to transfer through the silica to the outer wall surface. If the X-ray radiation intensity is high enough to generate heat in the silica at a rate faster than the rate of heat transfer through the silica, the heat accumulates in the silica, concentrated at the penetration depth, which can lead to structural failure of the chamber wall, and thereby potential operational failure of the entire particle manipulation system.
[0047] There are several potential ways to manage heat transfer through the walls of a plasma containment chamber. One way is to change the thermal conductivity of the chamber. The thermal conductivity of the chamber walls can be changed by changing the material and / or density of the chamber. The chamber material selection is somewhat limited, and changes in material density can have negative structural and / or vacuum consequences. The density of some materials (e.g., ceramics or glasses) can be changed by changing the process used to make the material (e.g., changing baking conditions and / or doping concentrations). Typically, materials with higher thermal conductivity (e.g., metals) also conduct electricity and adversely affect magnetic fields, making most thermally conductive materials unsuitable for the above-described particle manipulation system 200. Preferably, the chamber material is dielectric and / or ceramic, is vacuum compatible, and is structurally supportive. Alternatively or in addition, at least a portion of the chamber material can be graphite. Because the chamber material is dielectric or ceramic, it typically has low thermal conductivity, resulting in a slow heat transfer rate. Without being bound by any particular theory, this is because the lattice structure properties of dielectrics or ceramics that inhibit electrical conductivity typically also inhibit thermal conductivity. Constructing the entire chamber using dielectric or ceramic materials may present challenges, including those related to cost and / or structural stability.
[0048] A second way to tune the heat transfer rate is to change the distance that heat must travel to reach the heat sink 270. In the context of a plasma containment chamber, a heat sink 270, such as a water or oil coolant system, can be placed on the exterior of the chamber wall 252. Reducing the distance that heat must travel from the x-ray penetration depth to the exterior chamber wall surface can be achieved by reducing the thickness of the chamber wall 252. While thinner chamber walls reduce the distance to the heat sink, they can also compromise the structural integrity of the tubular chamber 250 to withstand the atmospheric pressure acting on the chamber. If the chamber is too thin, it cannot withstand the pressure difference between the interior of the chamber and the exterior of the chamber (e.g., 15 psi in the case of an exterior pressure at atmospheric pressure).
[0049] A third way to increase the rate of heat transfer away from the interior of the tubular chamber 250 is to select a material (or materials) for the chamber wall 252 of the tubular chamber 250 that has a longer X-ray penetration depth. With a longer penetration depth, the X-rays travel farther into the chamber wall and deposit heat farther into the chamber wall 252, closer to the heat sink 270 at the exterior of the tubular chamber 250. Given that X-ray absorption is statistical in nature, extending the penetration depth increases the total volume in which the X-rays are absorbed. To illustrate, if the penetration depth is doubled, the same amount of heat is deposited in significantly more material (e.g., approximately twice the volume of material), so that the peak temperature rise at the location where the X-rays are absorbed in the chamber wall 252 (e.g., near the interior surface) is significantly reduced (e.g., remains below the melting point of the materials in the chamber wall 252 and coating 251). In addition, the longer the penetration depth, the shorter the distance the deposited heat must travel to reach the exterior chamber wall surface (where the heat sink may be located).
[0050] Unfortunately, as described above, the choice of material for making the chamber wall 252 is limited by the material properties of candidate materials suitable for the application (e.g., materials that are dielectric, have sufficient strength, and are vacuum compatible), so that the chamber material cannot be selected based solely on the X-ray penetration depth. However, as disclosed herein, a coating 251 (e.g., a material that has a longer penetration depth than the material used to form the bulk portion of the chamber wall 252) can be used to form the chamber wall 252. Figure 3 251) can be applied to the inner surface of chamber wall 252. Coating 251 can include one or more layers (multiple) of materials.
[0051] According to aspects disclosed herein, instead of or in addition to selecting a bulk material for the chamber wall 252 itself based at least in part on the X-ray penetration depth, the interior surface of the chamber is coated with a film / coating of at least one material that provides a longer X-ray penetration depth than the bulk material in the chamber wall 252. The coating can have a thickness of about or at 1 μm to about or at 2000 μm, although in some cases (e.g., for applications where there are high energy X-rays in the chamber 250 that penetrate farther into the material, or for cases where the thickness of the chamber wall 252 can be reduced and replaced by the coating to improve thermal conductivity, or where the chamber wall 252 can be completely replaced by the coating material, thereby forming the chamber from the coating material), the coating can be thicker. In some cases, the coating 251 can have a thickness of from about or at 50 μm to about or at 1000 μm. In some cases, the coating 251 can have a thickness of from about or at 100 μm to about or at 700 μm. For some exemplary coating applications, such as to address X-ray bremsstrahlung of 1 keV to 5 keV electrons striking a 5 mm quartz or silica wall, it is preferred that the coating have a thickness between 100 μm and 300 μm, such as about 200 μm (e.g., for diamond or bobbin diamond coatings). Depending on the material used for the coating, the thickness of the coating may be no less than 50 microns, no less than 100 microns, no less than 200 microns, no less than 500 microns, or no less than 1 millimeter, although thicker coatings may be used in some cases.
[0052] By depositing a coating 251 that allows X-rays to penetrate deeper, the X-rays are absorbed across a larger volume of material at the chamber wall. In some embodiments, the coating is thicker than the penetration depth, and the X-ray energy is primarily absorbed in the coating. For example, in some applications, the thickness of the coating 251 can be from half the penetration depth to five penetration depths or more, where the penetration depth is determined by the coating material and the most abundant energy level (or dominant wavelength) of the X-rays incident on the coating 251. The most abundant energy level (or dominant wavelength) can be determined by examining the spectrum of the X-ray emission incident or intended to be incident on the chamber wall 252. In some cases, the penetration depth of one or more X-ray energies of interest is determined based on all X-ray wavelengths incident on the chamber wall 252 (e.g., energy absorbed near the inner surface of the chamber wall causes the most heating near the inner surface, and is therefore most likely to damage the inner surface).
[0053] Adding material that absorbs X-rays can reduce the peak temperature reached in the chamber wall 252. For example, the coating 251 can be the primary recipient of X-ray energy because most of the X-rays can be absorbed by the coating material (when the thickness of the coating is at least one penetration depth) rather than by the other materials that make up the bulk of the chamber wall 252. Absorbing most of the X-rays in the coating 251 and generating most of the heat in the coating can provide the following benefits: the coating material has a higher thermal resistance (higher thermal damage threshold) and / or higher thermal conductivity than the other materials that make up the bulk of the chamber wall 252. In some cases, the thickness of the coating can be less than one penetration depth (e.g., at least half of the penetration depth or from 0.2 penetration depths to one penetration depth).
[0054] In some embodiments, the thickness of the coating is such that X-rays having an energy range that would otherwise be absorbed near the inner surface of the chamber wall 252 are primarily absorbed in the coating. For example, the thickness of the coating may be at least half the penetration depth of an X-ray having that energy range and having at least a 50% probability of being absorbed within a distance D of the inner surface of the chamber wall 252 in the absence of the coating 251 (or where at least 50% of substantially all energy in that energy range is absorbed). The distance D may be a value in the range of about or exactly 50 microns to about or exactly 2 millimeters, including values such as 100 microns, 200 microns, 500 microns, and 1 millimeter. Alternatively, the distance D may be a fraction of the thickness of the chamber wall, such as from about or exactly 1% of the thickness of the wall to about or exactly 50% of the thickness of the chamber wall, including values such as 10%, 20%, 30%, and 40%. X-rays having this energy range may have energies in the range of 1 keV to 5 keV for some applications, in the range of 1 keV to 10 keV for some applications, in the range of 1 keV to 20 keV for some embodiments, and in the range of 1 keV to 50 keV for some cases, but any sub-range within the range of 0.2 keV to 100 keV is possible.
[0055] The thickness of the coating can be determined as follows. In this example, X-rays are incident on the chamber wall, and a portion of the X-ray spectrum extends from 1 keV to 5 keV (as an exemplary energy range). X-rays in this portion of the spectrum can generate a large amount of heat near the inner surface of the chamber wall 252 because their penetration depth in silicon dioxide (as an exemplary material for the chamber wall) is less than 50 microns. At least 50% of the X-rays in this energy range will be absorbed within 50 microns of the inner surface of the chamber wall 252. The coating thickness can then be selected for this energy range. For the boron nitride coating, the penetration depth is about 200 microns for 5 keV X-rays, and the penetration depth is less for low energy X-rays. Therefore, the coating thickness for half of the penetration depth of the coating for X-rays in this exemplary energy range will be about 100 microns. Such a coating can absorb a considerable amount of X-rays in this exemplary energy range, which would otherwise be absorbed in and near the surface of the chamber wall. This absorption of X-rays by the coating can reduce heat generation and peak temperature in the chamber wall and near the surface of the chamber wall 252.
[0056] Figure 2A The difference in the penetration depth of X-rays for two different materials is shown. In a conventional chamber having a chamber wall 252 made of silicon dioxide (silicon dioxide) 420, X-ray radiation 410 having an energy of about 5 keV penetrates about 40 μm into the chamber wall 252 before the intensity drops by 1 / e, referred to as the penetration depth 430-1. Chamber walls 252 made of a different material 422 (e.g., boron nitride) have a longer penetration depth 430-2 (over 200 microns at 5 keV), causing the X-rays 410 to travel farther into the chamber wall 252 and generate heat over a larger volume. Therefore, assuming the two materials have the same thermal conductivity, the peak temperature reached by silicon dioxide 420 in a smaller volume will be higher than the peak temperature reached by the different material 422 in a larger volume. In this example, boron nitride can have a thermal conductivity that is 30 times or more higher than that of silicon dioxide, such that boron nitride can also transfer heat away from the volume where the heat is generated faster than silicon dioxide, thereby further reducing peak temperatures that would otherwise occur in chamber wall 252 without the coating and improving thermal management.
[0057] Because coating 251 has a longer penetration depth, energy can be absorbed over a greater amount of material. In some cases, heat can be generated primarily (e.g., more than 50% of the heat generated) or even entirely in interior coating 251, where most or all of the incident X-rays are absorbed. In some cases, at least some heat is generated in chamber walls 252, where some of the X-rays may be absorbed. Also, because the coating has a higher thermal conductivity, it transfers heat through it more quickly, as in cases involving Figure 2AThe aspects of the larger absorption volume and higher thermal conductivity reduce the local temperature increase in the chamber wall due to X-ray absorption during system operation. In addition, because low energy X-rays are absorbed in a thinner layer, thermal conduction effects can play a greater role in transporting heat away from hot spots in coating 251. For low energy X-rays, the increased thermal conduction of coating 251 may be more beneficial for managing heat than X-ray absorption over a larger volume.
[0058] The operation of the particle manipulation system 200 that can generate X-ray emission can include pulsed or continuous X-ray emission. The pulse repetition rate and / or power level at which the system operates can depend on the thermal management in the chamber wall 252 of the tubular chamber 250. The system 200 should be operated at a level where the heat generated by the absorption of X-rays in the coating 251 and / or the chamber wall 252 is sufficiently dissipated (e.g., by exhausting pollutants) before reaching a level that may damage the coating 251 and / or the chamber wall 252 or adversely affect the manipulation of the plasma 205. Therefore, the coating 251 can reduce the local peak temperature increase in the chamber wall 252 caused by a single X-ray pulse, by many X-ray pulses, and by continuous X-ray emission, thereby allowing the system 200 to operate at a higher pulse repetition rate and / or power level than it would otherwise operate without the coating 251.
[0059] For some applications, a spectrum of X-rays (having a range of energies and wavelengths) may be emitted during operation of system 200. The emitted X-rays may be characterized by spectrum 440 (intensity or power versus energy or wavelength), which may be Gaussian in shape or have a wavelength such as Figure 2B Another shape is shown in the energy spectrum of 440. The energy spectrum 440 shown has a full width at half maximum (FWHM) value of 4 keV extending from 1 keV to 5 keV. In some cases, most of the heat generated in the coating or wall may be due to absorption of X-rays from the low energy portion of the X-ray spectrum 440. Because low energy X-rays can have a shorter penetration depth into any given material than high energy X-rays, low energy X-rays can be deposited into a smaller volume of the coating 251 than high energy X-rays. In some cases (e.g., during pulsed operation), absorption of low energy X-rays may result in a higher local temperature increase than absorption of high energy X-rays. Selecting a coating or wall with a high thermal conductivity (e.g., greater than 5 Wm -1 K -1 ) can very quickly transport heat generated by low energy X-rays through the coating to reduce local peak temperatures not only overall over time, but also during individual pulses when the system 200 is operated in a pulsed mode.
[0060] In addition to having a long penetration depth (e.g., greater than 50 microns) and high thermal conductivity, the coating material is preferably also dielectric and vacuum compatible. Not many materials have all of these properties. Most dielectric materials, such as silicon dioxide, have low thermal conductivity. That is, there are very few materials that conduct heat but not electrons. One of the few exceptions is diamond, which is a dielectric material that conducts heat through lattice vibrations. Diamond also has a longer X-ray penetration depth than silicon dioxide, given that carbon has a lower atomic number than silicon or oxygen. Therefore, coating 251 can be diamond and / or include diamond-like carbon, known as bobby diamond.
[0061] Diamond has advantageous thermal properties for particle manipulation systems. In contrast to metals, where conduction electrons are responsible for high thermal conductivity, dielectric crystalline materials such as diamond conduct heat via lattice vibrations. At a sound speed of 17,500 m / s, diamond is the material with the highest Debye temperature (2,220 K), an order of magnitude higher than most other insulating materials. The Debye temperature is a good approximation of the low-temperature heat capacity of an insulating crystalline solid, where other contributions (such as highly mobile conduction electrons) are negligible. Diamond has the highest thermal conductivity of any material at room temperature (2,000-2,500 W m -1 K -1 ), which is five times more than the thermal conductivity of copper. For X-ray energies of about 5 keV, diamond and bobbin diamond have an X-ray penetration depth of about 200 microns.
[0062] Diamond has other properties that are advantageous for use as coating 251 in particle manipulation system 200. Diamond is an extremely hard material and therefore may not substantially sputter or degrade when interacting with a plasma. In some embodiments, diamond coating 251 may also contribute to the structural stability of the chamber, allowing for a reduction in the thickness of chamber walls 252. Diamond also has a low dielectric constant of 5.7, a loss tangent of less than 0.00005 at 145 GHz, and a high dielectric strength of 1,000,000 V / cm.
[0063] Diamond-like carbon or diamond-like carbon is a non-gem quality diamond with a semi-crystalline disordered or amorphous crystal structure. It has a large amount of sp 3 For example, at least 30% of the carbon atoms in the round diamond coating 251 may be sp 3 It can also include more impurities than diamond. Impurities include other forms of carbon (e.g., graphite sp 2Hybridized carbon) and hydrogen (e.g., deuterium or deuterium). While pure diamond has a cubic crystal structure, bobby diamond may have a mixture of cubic and hexagonal crystal structures. Bobby diamond may not have long-range crystal order. Although structurally different from diamond, bobby diamond has somewhat similar electrical, thermal, X-ray and mechanical properties.
[0064] 2. Round diamond coating
[0065] The fundamental problem in diamond synthesis is the allotropic nature of carbon. Graphite is a crystalline phase of carbon that is thermodynamically more stable than diamond. Due to the higher stability of graphite, the use of graphite sp 2 High concentrations of non-diamond carbon etchants (e.g., atomic hydrogen and / or atomic deuterium) are used to suppress graphite sp 2 The formation of bonds. Atomic protium and / or atomic deuterium are prepared by dissociating protium (H2) or deuterium gas activated by heat or plasma. Atomic protium and / or atomic deuterium selectively etches graphite and decomposes double bonds, thereby converting graphite sp 2 bond into diamond sp 3 key.
[0066] Diamond and round diamond films can be deposited using plasma enhanced chemical vapor deposition (PECVD). PECVD is a chemical vapor deposition process for depositing thin films from a gaseous state to a solid state on a substrate. The process involves a chemical reaction that occurs after a plasma of a reactive gas is generated. PECVD involves a surface reaction with a gaseous precursor under non-equilibrium. The precursors are protium and / or deuterium and one or more hydrocarbons. These precursors are activated by the plasma to form atomic protium and / or deuterium and hydrocarbon radicals.
[0067] Typically, PECVD of diamond is limited to surface areas of about 450 mm or less. This is because PECVD is generally intended to produce diamond films with high purity, crystallinity, and precise thickness, which are useful for specific applications, including optics and integrated circuit manufacturing. For these higher purity films, the stability competition between graphite and diamond is a factor. In addition, as the size of the substrate increases, the difficulty of maintaining a uniform ion flux across the substrate increases, thereby limiting the PECVD surface area and increasing the difficulty of scaling high purity diamond deposition.
[0068] For applications where the coating does not require high purity or precise thickness, diamond can be deposited over a larger surface area and with greater thickness. Despite the lower purity, diamond and / or bobbin diamond coatings deposited over a large surface area can have improved structural strength, electrical resistance, and / or thermal conductivity compared to silicon dioxide. For example, some particle manipulation systems 200 described herein can tolerate coatings 251 having high impurity levels of protium, deuterium, and graphite impurities (e.g., up to about 50% graphite impurities) in the diamond and / or bobbin diamond. The system 200 can also tolerate high variability in coating thickness across the interior surface of the chamber wall 252 (e.g., up to about 50% variation).
[0069] Figure 3 An exemplary round grain diamond deposition process is shown for coating at least a portion of the interior surface 510 of the chamber 250. In a first step 511, the interior surface 510 of the chamber 250 is pre-treated with microscopic diamond seeds 520 prior to deposition. Diamond seeding helps form diamonds during deposition. One method of seeding is to polish the surface with diamond powder so that microscopic diamond crystals remain on the surface. During a subsequent PECVD process 513, the size of the diamond crystals increases until they form a continuous, dense polycrystalline diamond coating 251 on the interior surface 510.
[0070] After the inner surface 510 of the chamber 250 is seeded with diamond seeds 520, a coating 251 may be formed on the inner surface of the chamber using a PECVD process 513. Prior to deposition, the chamber 250 is purged to remove residual gases from the interior of the chamber. The temperature of the chamber 250 during deposition may be, for example, in the range of about or at 25°C to about or at 2500°C. In one embodiment, for example, during deposition, the chamber 250 is heated to one or more temperatures in the range of about or at 700°C to about or at 2500°C, and the pressure inside the chamber 250 may be in the range of about or at 1 Torr to about or at 500 Torr. In some cases, the chamber 250 may be heated to one or more temperatures in the range of about or at 300°C to about or at 1000°C during deposition of the coating 251. The chamber 250 may be heated by an RF plasma for PECVD and / or by inductively heating a resistive layer (e.g., graphite) in or in contact with the chamber wall 252. In some cases, the resistive layer can be adjacent to or at the inner surface 510 of the chamber 250. In some embodiments, the resistive layer can be discontinuous around the circumference of the chamber 250 to suppress eddy currents that would otherwise be generated by the magnetic field generated by the coil 230. Alternatively, the chamber 250 can be heated via a rotosil type process, in which an intense arc is struck in a plasma to generate infrared light that is absorbed in the near-surface inner layer of the chamber wall 252. In some cases, the chamber 250 can be placed in a furnace for deposition, or heated by a heating element thermally coupled to the exterior of the chamber 250.
[0071] During the deposition of the round grain diamond and / or diamond coating 251, a process gas, which may include a gas mixture, is introduced into the chamber 250. During the deposition, the process gas may remain statically or continuously flowing through the chamber. The process gas mixture includes at least one of protium or deuterium and at least one hydrocarbon or deuterated hydrocarbon. For example, the hydrocarbon may be methane, acetylene, silane, or a deuterated form thereof. For example, the hydrocarbon or deuterated hydrocarbon is present in the gas mixture in a stoichiometric ratio of about or exactly 0.001:1 to about or exactly 0.1:1 relative to, for example, protium and / or deuterium. Deuterated precursor gases may be used here because protium is an impurity in some plasma confinement processes. The process gas mixture may also include other gases that promote specific carbon phases (e.g., water, oxygen, carbon dioxide) and / or one or more inert gases (e.g., argon, nitrogen, sulfur hexafluoride).
[0072] Plasma is initiated in the process gas. A microwave or radio frequency (RF) plasma discharge dissociates and ionizes the gas, which is then deposited as pure carbon, thereby forming a polycrystalline diamond and round grain diamond (diamond-like carbon) combination of CC and CC:H on the inner surface of the chamber. The RF plasma source may include electrodes without the introduction of metal impurities, including carbon electrodes (e.g., graphite or graphene). The RF plasma source may be operated continuously or in a pulsed manner. The plasma discharge may be a pulsed high-intensity RF wave, the frequency of which is, for example, about or just 0.1 MHz to about or just 10 MHZ, and the RF power level of which is, for example, about or just 0.1 GW to about or just 10 GW (e.g., 1 GW). In some cases, the plasma discharge may be a steady continuous RF wave, the frequency of which is, for example, about or just 100 MHz to about or just 3000 MHZ, and the power level of which is, for example, about or just 10 kW to about or just 100 kW. Pulsed plasma discharges may be preferred because they provide a higher intensity RF field using a similar amount of energy compared to continuous discharges. The plasma may be directed toward the inner surface 510 of the chamber wall 252, with the external electromagnetic coil positioned near the exterior of the chamber. In examples where the chamber 250 has a tubular shape, an external electromagnetic coil may not be needed to direct the plasma toward the inner surface of the chamber wall. In an embodiment, for example when depositing round diamond or diamond, the deposition rate (coating thickness increase) of the coating 251 may be in the range of about or exactly 10 μm per hour to about or exactly 100 μm per hour. In another embodiment, the growth rate is slower. The coating may have a thickness of about or exactly 1 μm to about or exactly 2000 μm (including all values and subranges therebetween). In some cases, the coating 251 may be thicker than 2000 μm.
[0073] In some embodiments, the coating is processed after deposition. For example, the coating can be heated to crystallize or melt the deposited material. Alternatively or in addition, the coating can be polished (e.g., mechanically polished or using a chemical mechanical polishing process) after it is formed.
[0074] In some cases, to provide a more uniform coating, the coating may be deposited on the interior surface 510 of the chamber 250 in sections. For example, sections of the interior surface 510 of the chamber 250 may be covered prior to deposition (e.g., with a quartz fiber tape or a quartz fiber film) so that the coating is not deposited on these sections. At least one section of the interior surface 510 is not covered to allow the coating to be deposited on the section(s). The section(s) may then be covered after the coating is deposited. The tape or film covering another section (or other sections) may be removed for subsequent coating deposition. The tape or film has sufficient mechanical strength to withstand the force used to destroy the coating to remove the tape or film. In some cases, only a portion of the interior surface 510 of the chamber wall 252 may be coated, such as Figure 4 The coated portion may be a portion of the chamber 250 centered around the region where the plasma 205 within the chamber is compressed to its minimum spatial extent during system operation. For example, other portions of the chamber may be shielded to prevent deposition of the coating 251.
[0075] 3. Deposition system
[0076] Figure 4 An exemplary particle manipulation system 200 is shown having a containment chamber 250 for containing particles (e.g., atoms of a plasma). The particle manipulation system 200 may have Figure 1A All features and functions of the particle manipulation system 200 need not be described again. Figure 4 In the illustration of , the particle manipulation system 200 is fluidly coupled to a gas supply apparatus 400 that can adapt the particle manipulation system 200 to in-situ deposit (eg, PECVD) bobbin diamond, diamond, and / or graphite in the tubular chamber 250 .
[0077] The inlet 282 of the tubular chamber 250 can be fluidly connected to different gas supply sources 460, 462, 464 that provide gases and gas mixtures to deposit the coating 251 via a conduit 470. The gas supply source can include a carrier gas 460, a carbon precursor 462 (also referred to herein as a hydrocarbon or deuterated hydrocarbon), and a protium gas 464. Deuterium gas can be used instead of the protium gas 464. A valve 472 is placed between each gas supply source 460, 462, 464 and the chamber 250. Each valve 472-1, 472-2, 472-3 can be an open / close valve (e.g., a ball valve, a butterfly valve, a gate valve, or a diaphragm valve) and / or a metering valve. In some embodiments, the valves 472 are communicatively connected to and controlled by the controller 210, but they can be connected to and controlled by a separate controller for the gas supply device 400. The system 200 also includes a pressure controller 480 upstream of the chamber to control the pressure in the chamber 250. Pressure controller 480 includes sensors that can measure pressure upstream of the chamber, downstream of the chamber, and / or within the chamber. Outlet 284 is coupled to a vacuum pump to provide a vacuum within the chamber.
[0078] In some embodiments, there may be at least some electromagnetic coils 230 that are capable of generating radio frequency (RF) electromagnetic waves inside the tubular chamber 250 for coating deposition. RF excitation of the gaseous mixture from the gas supply sources 460, 462, 464 can generate plasma for PECVD. In some cases, the electromagnetic coils 230-4, 230-5, 230-6, 230-7 (power supply circuits are not shown to simplify the drawing) used to generate RF waves for PECVD in the tubular chamber 250 for deposition are different (e.g., have lower inductance) from the electromagnetic coils 230-1, 230-2, 230-3 used to generate a magnetic field for confining and / or manipulating the plasma inside the chamber 250 that can generate X-rays. Because the electromagnetic coils 230 are independently controlled, the strength and shape of the local RF electromagnetic field in the chamber 250 can be tuned (e.g., to adjust the strength of the RF field at different locations within the chamber 250). This tunability can homogenize the ion density distribution in the chamber during deposition, which can improve the uniformity of the thickness and / or quality of the deposited coating 251. A simulation tool (e.g., Ansys Maxwell) can be used to model the electromagnetic field throughout the chamber and determine the power settings of the different electromagnetic coils 230 that will homogenize the field strength to improve the uniformity of the ion density. Conversely, the RF field can be adjusted to different intensities at different locations within the chamber 250 to spatially vary the thickness of the deposited coating. This can be beneficial if some areas of the chamber receive more radiation and / or degrade more quickly than other areas within the chamber.
[0079] Figure 5 A cross section of a coated tubular chamber 250 is shown according to some embodiments. The coated chamber includes a bulk silica chamber wall 252 and a round grain diamond coating 251 disposed on an inner surface 510 of the silica chamber wall 252. The coating 251 has a thickness of about 1 μm to about 2000 μm or more. Preferably, the coating has a thickness of about 200 μm.
[0080] Fig. 6AA cross section of another embodiment of a coated tubular chamber 600 is shown. The coated chamber 600 includes a bulk silica chamber wall 252 and a round diamond coating 251 disposed on the inner surface of the silica chamber wall 252. A channel 630 partially or completely passes through the silica chamber wall 252 and is filled with a thermally conductive filler (e.g., round diamond, graphene, boron nitride and / or diamond). In some embodiments where dielectric requirements are less stringent, the hole can be filled with a non-magnetic metal (e.g., stainless steel, aluminum, copper). The channel 630 can be formed by mechanical boring, acid etching, or laser boring. The channel 630 can be a cylindrical or prismatic hole, but other shapes are possible. When filled with a material having high thermal conductivity, the channel 630 can provide a high thermal conductivity path between the coating 251 on the inner surface 510 of the chamber and the heat sink 270 on the outer surface. The filler can be formed in the channel 630 by thermal spray coating, PECVD, and / or pouring a suspension of filler particles. This configuration can reduce heat buildup at the interface between the coating 251 and the bulk silica wall 252, and can improve overall heat conduction from the coating 251 and the inner surface 510 to the external heat sink 270. Additional transition or filler materials (e.g., quartz rope, quartz ribbon, ceramic) can be formed between the silica and the channel material to address any issues caused by the different thermal expansion rates of the different materials involved. In some cases, an interlayer material (e.g., graphite or ceramic) can be deposited on the channel wall before the filler is added to relieve stress caused by the different thermal expansion coefficients between the filler material and the bulk silica wall 252.
[0081] Figure 6B A coated chamber 601 is depicted in which the chamber wall 252 is formed of a plurality of segments 650 (e.g., blocks). In some applications, the blocks may be mounted against a heat sink 270, or against an outer chamber wall that may or may not support a vacuum. The gaps 635 between the segments 650 may be filled with a vacuum compatible material that may provide a vacuum seal between the segments and / or have a higher thermal conductivity than the bulk material in the chamber wall 252 from which each segment 650 is made. In some cases, the filler 637 between the segments 650 comprises a vacuum compatible elastomer (e.g., nitrile rubber, fluororubber, etc.) or a vacuum compatible plastic (e.g., fluoropolymer, kapton, polyetheretherketone, etc.). In some embodiments, the filler 637 comprises a dielectric such as boron nitride, diamond, boron nitride, or graphite. In some cases, the filler 637 comprises a conductive non-magnetic metal (e.g., stainless steel, aluminum, copper, etc.). The filler 637 and the gap 635 may be filled or covered with quartz fiber rope or tape 660 .
[0082] Fig. 7AA cross section of another embodiment of a coated tubular chamber 700 is shown. The coated chamber 700 includes a bulk silica chamber wall 252 and a bobby diamond coating 251 disposed on an interface layer 730, the interface layer being disposed between the bobby diamond coating 251 and the silica chamber wall 252. The bobby diamond coating 251 and the interface layer 730 form a multi-layer coating 751 on the inner surface 510 of the chamber wall. The interface layer 730 may be composed of a material having a thermal conductivity between the thermal conductivity of the bobby diamond material in the bobby diamond coating 251 and the thermal conductivity of the bulk silica wall 252. The material of the interface layer 730 may have a different density and carbon purity than the bobby diamond coating 251 and the silica wall 252, and in some cases, may itself be composed of bobby diamond. In this way, the interface layer 730 may reduce or substantially prevent heat accumulation at the interface between the multi-layer coating 751 and the bulk silica wall 252.
[0083] Figure 7B Another form of a multilayer coating 751 is depicted (only a portion of the chamber wall 252 is shown) in which a plurality of interface layers 730-1, 730-2, 730-3 are disposed between the round grain diamond coating 251 and the silicon dioxide chamber wall 252. The interface layers 730 may have two or more different thermal conductivities T c To produce a thermal conductivity gradient. Figure 7B In the illustrated example, each interface layer has a different thermal conductivity, and the layers are arranged so that the interface layer 730-3 with the highest thermal conductivity is in contact with the inner coating 251 (e.g., a round grain diamond coating), and the thermal conductivity value decreases monotonically toward the chamber wall 252. Other arrangements of thermal conductivity values are also possible and may depend at least in part on the penetration depth of the X-rays in the interface layers 730-1, 730-2, 730-3. In some cases, the interface layer may have a coefficient of thermal expansion (CTE) between the CTE of the coating 251 and the CTE of the chamber wall 252 to relieve stress that would otherwise occur if the coating 251 directly contacted the chamber wall 252. One or more interface layers 730-1, 730-2, 730-3 may be deposited using the same method used to deposit the round grain diamond coating 251. Alternatively, the interface layer(s) may be deposited by thermal spray coating or suspension casting.
[0084] The operation of the particle manipulation system 200 described above may degrade the coating 251 over time. For example, coating degradation may be caused by plasma impact, electromagnetic radiation, and mechanical strain caused by thermal expansion and contraction. Certain plasma processes may subject the coating to neutron radiation and gamma rays, which may also degrade the coating and / or transform the coating into other materials that are less suitable for use as coatings in such systems (e.g., smaller X-ray penetration depth, lower thermal conductivity, and / or lower hardness). In some cases, the coating 251 may be slowly ablated from the chamber wall. To offset degradation, the coating 251, 751 may be periodically refurbished by depositing additional coating material on the inner surface of the chamber wall and / or on the pre-existing coating 251, 751. In the presence of multiple coatings (e.g., to form a thermal gradient), frequent refurbishment of the innermost layer facing the plasma may help avoid degradation of the second layer. In some embodiments, a new complete coating 251, 751 may be deposited on the remnants of the pre-existing coating 251, 751. The coating may be refurbished at specific time intervals or when certain operating conditions indicate that the coating has degraded. Operating conditions that may indicate that the coating has degraded include a significant increase in the average temperature in the chamber during operation or a significant increase in contamination of the plasma measured by a spectrometer or when a decrease in performance of the particle manipulation system 200 is observed. This refurbishment process follows the same process described above for depositing the initial coating 251, 751. In an embodiment, (multiple) additional coatings are deposited onto the existing coating 251, 751 so that the process can forgo diamond seeding pretreatment. In another embodiment, the existing coating 251, 751 is partially or completely removed (e.g., by etching with a plasma formed in the plasma chamber) before depositing the additional coating material. If the coating material is transformed due to neutron radiation exposure, it may be beneficial to remove at least some of the existing coating 251, 751. Prior to deposition, plasma confinement operations are stopped, any residual gases in the chamber are purged, and the chamber walls may be heated to a temperature in the range of about or exactly 100°C to about or exactly 1000°C to drive away contaminants from the surface on which the new material will be deposited.
[0085] Various coating embodiments and related methods are possible, some of which are listed below. Different coating configurations can be used in or result from any of the listed methods.
[0086] (1) A method of containing a plasma in a plasma chamber, the method comprising: injecting plasma into the plasma chamber; applying a magnetic field to the plasma to manipulate the plasma; receiving electromagnetic radiation including X-rays from the plasma in a coating deposited on an inner surface of a wall of the plasma chamber facing the plasma, a portion of the X-rays having a certain energy range, wherein the thickness of the coating is at least half of the penetration depth of the portion of the X-rays having the energy range, and wherein, in the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 mm of the inner surface of the wall.
[0087] (2) The method according to (1), wherein the portion of the X-rays having the energy range has an energy in the range of 1 keV to 5 keV.
[0088] (3) The method according to (1) or (2), wherein the coating has a first thermal conductivity higher than a second thermal conductivity of the wall.
[0089] (4) A method according to (3), wherein the coating comprises at least two layers of material, wherein: a first layer of the at least two layers comprises at least one of diamond, graphite or round grain diamond and has the first thermal conductivity; and a second layer of the at least two layers has a third thermal conductivity, the third thermal conductivity having a value between the first thermal conductivity and the second thermal conductivity.
[0090] (5) The method according to any one of (1) to (4), wherein the thickness of the coating layer is not less than 50 μm.
[0091] (6) The method according to any one of (1) to (5), wherein the thickness of the coating is at most three penetration depths of the portions of the X-rays having the energy range.
[0092] (7) The method according to any one of (1) to (6), wherein the coating comprises at least one of diamond, graphite, boron nitride, or boron grit diamond.
[0093] (8) A plasma chamber for containing plasma, the plasma chamber comprising: a wall surrounding a volume that contains the plasma when the plasma chamber is in operation; and a coating in thermal communication with an inner surface of the wall, the coating being configured to receive electromagnetic radiation including X-rays from the volume, a portion of the X-rays having an energy range, wherein: a first thermal conductivity of the coating is greater than a second thermal conductivity of the wall; a thickness of the coating is at least half of a penetration depth of the X-rays within the energy range; and in the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 mm of the inner surface of the wall.
[0094] (9) The plasma chamber according to configuration (8), wherein the portion of the X-rays having the energy range has energy in a range of 1 keV to 5 keV.
[0095] (10) The plasma chamber according to configuration (8) or (9), wherein the thickness of the coating is at most three penetration depths of the portion of the X-rays having the energy range.
[0096] (11) The plasma chamber according to any one of configurations (8) to (10), wherein a thickness of the coating is not less than 50 μm.
[0097] (12) A plasma chamber according to any one of configurations (8) to (11), wherein the coating comprises at least one of diamond, graphite, boron nitride, or boron grain diamond.
[0098] (13) The plasma chamber of any one of configurations (8) to (12), wherein the coating has a first thermal damage threshold higher than a second thermal damage threshold of the wall.
[0099] (14) A plasma chamber according to any one of configurations (8) to (13), wherein the coating comprises at least two layers of material, wherein: a first layer of the at least two layers comprises at least one of diamond, graphite, or round grain diamond and has the first thermal conductivity; and a second layer of the at least two layers has a third thermal conductivity, the third thermal conductivity having a value between the first thermal conductivity and the second thermal conductivity.
[0100] (15) The plasma chamber of any one of configurations (8) to (14), wherein the wall comprises silicon dioxide.
[0101] (16) A system comprising: a plasma chamber according to any one of configurations (8) to (15); a plurality of electromagnetic coils, the plurality of electromagnetic coils being outside the plasma chamber and arranged to generate a magnetic field to confine and manipulate plasma within the plasma chamber; and a heat sink, the heat sink being thermally connected to an outer surface of a wall of the plasma chamber.
[0102] (17) The system according to configuration (16) also includes a circuit for applying current to the plurality of electromagnetic coils so that the plasma is compressed and at least some atoms within the plasma fuse.
[0103] (18) A system according to configuration (16) or (17), wherein the radiator includes a pipe through which the coolant can flow.
[0104] (19) A system comprising: a plasma chamber having walls extending around an interior volume, the plasma chamber being adapted to support a vacuum in the interior volume, the walls of the plasma chamber having a relative humidity of no greater than 5 W -1 K -1 a plasma source to generate plasma and inject the plasma into the interior volume of the plasma chamber; at least one gas inlet coupled to the plasma source to introduce a gas or gaseous mixture into the plasma source; and a plurality of electromagnetic coils arranged to generate a magnetic field within the plasma chamber such that interaction of particles of the plasma with the magnetic field produces electromagnetic radiation including X-rays, a first portion of which may be absorbed by a wall of the plasma chamber to cause heating of the wall; wherein the plasma chamber further comprises a coating comprising at least one of boron nitride, graphite, or diamond, the coating being disposed on an inner surface of the wall of the plasma chamber to absorb at least a second portion of the X-rays included in the first portion of the X-rays such that local peak heating of the wall near the inner surface occurring during operation of the system due to absorption of the first portion of the X-rays is reduced compared to absorption of the first portion of the X-rays that would occur in the absence of the coating.
[0105] (20) The system according to configuration (19) also includes: at least one power supply circuit connected to the multiple electromagnetic coils; and at least one controller, wherein the at least one controller is connected to the at least one power supply circuit to control one or more parameters of the magnetic field.
[0106] (21) A system according to configuration (19) or (20), wherein the at least one gas inlet includes a first gas inlet and a second gas inlet, and wherein the system further includes: a hydrocarbon precursor supply source, which is connected to the first air inlet to deliver the hydrocarbon precursor to the plasma source; and at least one of a protium supply source or a deuterium supply source, which is connected to the second gas inlet to deliver at least one of the protium gas or the deuterium gas to the plasma source.
[0107] (22) A system according to any one of configurations (19) to (21), wherein the plasma chamber includes at least one of a dielectric material, a ceramic material, or graphite.
[0108] (23) The system of any one of configurations (19) to (22), wherein the plasma chamber comprises quartz.
[0109] (24) A system according to any one of configurations (19) to (23), wherein the coating is provided on all exposed surfaces of the inner surface of the wall.
[0110] (25) A system according to any one of configurations (19) to (24), wherein the coating comprises at least two layers of material, wherein: a first layer of the at least two layers comprises at least one of diamond, graphite, or round grain diamond and has the first thermal conductivity; and a second layer of the at least two layers has a second thermal conductivity, the second thermal conductivity having a value between the first thermal conductivity and a third thermal conductivity of the wall.
[0111] (26) The system according to any one of configurations (19) to (25), further comprising a quartz fiber ribbon or quartz fiber rope disposed on at least a portion of the inner surface of the wall.
[0112] (27) A system according to any one of configurations (19) to (26), wherein the plasma chamber has a diameter in the range of 0.01 meters to 3 meters and a length in the range of 0.2 meters to 6 meters.
[0113] (28) The system of any one of configurations (19) to (27), further comprising a resistive layer disposed on at least a portion of a plasma chamber wall, wherein the resistive layer provides induction heating to the plasma chamber.
[0114] (29) A system according to any one of configurations (19) to (28), wherein a thickness of the coating is not less than 200 microns.
[0115] (30) A system according to any one of configurations (19) to (29), wherein: the thickness of the coating is selected to be at least half of the penetration depth of the coating and the first portion of the X-rays, and at least 50% of the first portion of the X-rays are absorbed within a distance of 20% of the thickness of the wall into the wall.
[0116] (31) A system according to any one of configurations (19) to (30), wherein the coating comprises round grain diamond.
[0117] (32) A system according to any one of configurations (19) to (30), wherein the coating comprises diamond.
[0118] (33) A system according to any one of configurations (19) to (30), wherein the coating comprises graphite.
[0119] (34) A system according to any one of configurations (19) to (30), wherein the coating comprises boron nitride.
[0120] (35) The system of any one of configurations (19) to (34) further includes at least one channel, wherein the at least one channel is configured to pass through a wall of the plasma chamber, wherein the channel is filled with a material having a thermal conductivity higher than a thermal conductivity of the wall.
[0121] (36) According to any one of configurations (19) to (35), the system also includes an interface layer arranged between the inner surface of the plasma chamber and the coating, the interface layer having a second thermal conductivity different from the thermal conductivity of the wall of the plasma chamber and different from the third thermal conductivity of the coating.
[0122] (37) A system according to any one of configurations (19) to (36), wherein the electromagnetic radiation includes radiation generated by one or more of the following: confinement of the plasma by the magnetic field; compression of the plasma by the magnetic field; or acceleration of the plasma by the magnetic field.
[0123] (38) A system according to any one of configurations (19) to (37), wherein the electromagnetic radiation includes bremsstrahlung from interactions between particles of the plasma, interactions between particles of the plasma and the magnetic field, or both.
[0124] (39) A method of depositing a coating on the inner surface of a wall of a plasma chamber, wherein electromagnetic radiation including X-rays is incident on the coating, a portion of the X-rays having a certain energy range, the method comprising: heating the plasma chamber so that the inner surface of the wall is at a temperature of 300°C to 2500°C; and introducing a gas mixture into the plasma chamber, the gas mixture comprising: a first gas, the first gas including a hydrocarbon; and a second gas, the second gas including at least one of protium or deuterium; generating a plasma in the plasma chamber; and depositing the coating on the inner surface of the wall; wherein: the coating comprises at least one of diamond, graphite or bobbin diamond; and the coating is deposited to a thickness of at least half the penetration depth of the portion of the X-rays having the energy range; and in the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 mm of the inner surface of the wall.
[0125] (40) The method according to (39), wherein the portion of the X-rays having the energy range has energy in the range of 1 keV to 5 keV.
[0126] (41) The method of (39) or (40), wherein the thickness of the coating is at most three penetration depths of the portion of the X-rays having the energy range.
[0127] (42) The method according to any one of (39) to (41), wherein the thickness of the coating is not less than 50 μm.
[0128] (43) The method according to any one of (39) to (42), wherein the wall of the plasma chamber comprises silicon dioxide.
[0129] (44) A method according to any one of (39) to (43), wherein the coating comprises at least two layers of material, wherein: a first layer of the at least two layers comprises at least one of diamond, graphite, boron nitride or round grain diamond and has a first thermal conductivity; and a second layer of the at least two layers has a second thermal conductivity, the second thermal conductivity having a value between the first thermal conductivity and a third thermal conductivity of the wall.
[0130] (45) The method according to any one of (39) to (44) further includes pre-treating the inner surface of the plasma chamber.
[0131] (46) The method according to any one of (39) to (45), wherein generating the plasma includes applying radio frequency (RF) electromagnetic waves to the gas mixture in the plasma chamber to dissociate and ionize the gas mixture.
[0132] (47) The method of (46), wherein the intensity of the applied RF electromagnetic wave varies spatially across the plasma chamber to spatially vary the thickness of the coating.
[0133] (48) The method of any one of (39) to (47), wherein depositing the coating comprises coating all exposed surfaces of the interior surface of the plasma chamber.
[0134] (49) The method according to any one of (39) to (48) also includes: before depositing the coating, shielding at least a portion of the inner surface of the plasma chamber so that at least a portion of the inner surface is not coated during the deposition of the coating.
[0135] (50) A method according to (49), wherein the coating is deposited to form a coating in a portion of the plasma chamber centered around a region of the plasma chamber where the plasma within the plasma chamber is compressed to its minimum spatial extent during operation of the plasma chamber.
[0136] (51) The method according to any one of (39) to (50), wherein the hydrocarbon is at least one of methane, deuterated methane, or silane.
[0137] (52) The method according to any one of (39) to (51), wherein the second gas is deuterium.
[0138] (53) The method according to any one of (39) to (52), wherein generating the plasma includes generating at least one of a pulsed RF electromagnetic wave or a continuous RF electromagnetic wave.
[0139] (54) The method according to (53), wherein the pulsed RF electromagnetic wave has a frequency in the range of 0.1 MHz to 10 MHz and a power in the range of 0.1 GW to 10 GW.
[0140] (55) The method according to (53), wherein the continuous RF electromagnetic wave has a frequency in the range of 100 MHz to 3000 MHz and a power in the range of 10 kW to 100 kW.
[0141] (56) The method according to any one of (39) to (55), wherein heating the inner surface includes heating the inner surface via the plasma.
[0142] (57) The method of any one of (39) to (56), wherein heating the inner surface comprises inductively heating a wall of the plasma chamber.
[0143] (58) The method of any one of (39) to (57), wherein heating the inner surface includes generating infrared light in the plasma chamber.
[0144] (59) A method for refurbishing a coating on an interior surface of a plasma confinement system, the plasma confinement system comprising: a plasma chamber having a diamond grain coating on at least a portion of the interior surface of the plasma chamber, wherein the diamond grain coating is arranged to receive X-rays having a certain energy range from a plasma confined by the plasma confinement system; the method comprising: purging the plasma chamber to remove any residual gas; heating the interior surface of the plasma chamber to a temperature in the range of 300°C to about 2500°C; introducing a gas mixture into the plasma chamber, the gas mixture comprising: a first gas, the first gas comprising a hydrocarbon; and a second gas, the second gas comprising at least one of protium or deuterium; generating a plasma in the plasma chamber by applying radio frequency electromagnetic waves to dissociate and ionize the gas mixture; and depositing additional diamond grains on the diamond grain coating to refurbish the diamond grain coating on the interior surface of the plasma chamber, such that the refurbished diamond grain coating absorbs at least half of the X-rays having the energy range.
[0145] 4. Conclusion
[0146] Although various inventive embodiments have been described and illustrated herein, a person of ordinary skill in the art will readily conceive of various other devices and / or structures for performing the functions described herein and / or obtaining the results and / or one or more advantages described herein, and each of such changes and / or modifications is considered to be within the scope of the inventive embodiments described herein. More generally, it will be readily appreciated by those skilled in the art that all parameters, dimensions, materials, and configurations described herein are intended to be exemplary, and that actual parameters, dimensions, materials, and / or configurations will depend on one or more specific applications for which the teachings of the present invention are used. A person skilled in the art can identify or be able to determine many equivalents of the specific inventive embodiments described herein using routine experiments at best. Therefore, it should be understood that the foregoing embodiments are presented only by way of example, and within the scope of the appended claims and their equivalents, embodiments of the present invention may be practiced in a manner different from that specifically described and claimed. The inventive embodiments of the present disclosure relate to each individual feature, system, article, material, kit, and / or method described herein. In addition, if such features, systems, articles, materials, kits, and / or methods are not mutually contradictory, any combination of two or more such features, systems, articles, articles, kits, and / or methods is included within the scope of the invention disclosed herein.
[0147] In addition, various inventive concepts may be embodied as one or more methods, examples of which have been provided. The actions performed as part of a method may be ordered in any suitable manner. Thus, embodiments may be constructed in which the actions are performed in an order different from the order shown, which may include performing some actions simultaneously, even though shown as sequential actions in an illustrative embodiment.
[0148] All definitions, as defined and used herein, should be understood to control over dictionary definitions, definitions in documents incorporated by reference, and / or ordinary meanings of the defined terms.
[0149] Unless explicitly stated to the contrary, the indefinite articles "a" and "an" as used herein in the specification and claims should be understood to mean "at least one".
[0150] The phrase "and / or" as used herein in the specification and claims should be understood to mean "either or both" of the elements so combined, i.e., elements that are conjunctively present in some cases and disjunctively present in other cases. Multiple elements listed with "and / or" should be interpreted in the same manner, i.e., "one or more" of the elements so combined. In addition to the elements specifically identified by the "and / or" clause, other elements may optionally be present, whether related or unrelated to the specifically identified elements. Thus, as a non-limiting example, when used in conjunction with open language such as "comprising", a reference to "A and / or B" may refer to only A (optionally including elements other than B) in one embodiment; to only B (optionally including elements other than A) in another embodiment; to both A and B (optionally including other elements) in yet another embodiment; etc.
[0151] As used herein in the specification and claims, "or" should be understood to have the same meaning as "and / or" as defined above. For example, when separating items in a list, "or" or "and / or" should be interpreted as inclusive, that is, including at least one (but also including more than one) of several elements or lists of elements and optionally additional unlisted items. Only terms that clearly indicate the opposite, such as "only one" or "just one", or when used in the claims, "consisting of ..." will refer to including exactly one element in a plurality of elements or lists of elements. In general, the term "or" used herein should be interpreted as indicating exclusive alternatives (that is, "one or the other, but not both") only when there are exclusive terms such as "any", "one", "only one" or "just one" in front. When used in the claims, "essentially consisting of ..." should have its ordinary meaning used in the field of patent law.
[0152] As used herein in the specification and claims, with respect to a list of one or more elements, the phrase "at least one" should be understood to mean at least one element selected from any one or more elements in the list of elements, but does not necessarily include at least one of each element specifically listed in the list of elements, and does not exclude any combination of elements in the list of elements. This definition also allows that elements other than the elements specifically identified in the list of elements referred to by the phrase "at least one" may optionally exist, whether related or unrelated to those elements specifically identified. Thus, as a non-limiting example, "at least one of A and B" (or, equivalently, "at least one of A or B", or equivalently, "at least one of A and / or B") may refer to at least one (optionally including more than one) A without B (optionally including elements other than B) in one embodiment; may refer to at least one (optionally including more than one) B without A (optionally including elements other than A) in another embodiment; may refer to at least one (optionally including more than one) A and at least one (optionally including more than one) B (and optionally including other elements) in yet another embodiment; and so on.
[0153] Unless otherwise indicated, in some embodiments, the terms "approximately" and "about" are used to mean within ±20% of a target size, in some embodiments within ±10% of a target size, in some embodiments within ±5% of a target size, and in some embodiments within ±2% of a target size. The terms "approximately" and "about" may include a target size. The term "substantially" is used to mean within ±3% of a target size.
[0154] In the claims and in the above description, all transitional phrases, such as "comprising," "including," "carrying," "having," "containing," "involving," "having," "consisting of," and the like, shall be understood to be open-ended, i.e., meaning including, but not limited to. Only the transitional phrases "consisting of" and "consisting essentially of" shall be closed or semi-closed transitional phrases, respectively, as set forth in the United States Patent Office Manual of Patent Examining Procedure Section 2111.03.
Claims
1. A method of containing a plasma in a plasma chamber, the method comprising: injecting plasma into the plasma chamber; applying a magnetic field to the plasma to manipulate the plasma; as well as receiving electromagnetic radiation including X-rays from the plasma in a coating deposited on an inner surface of a wall of the plasma chamber facing the plasma, a portion of the X-rays having an energy range; wherein the thickness of the coating is at least half the penetration depth of the portion of the x-rays having the energy range, and wherein, in the absence of the coating, at least 50% of the x-rays having the energy range are absorbed within 1 mm of the inner surface of the wall.
2. The method according to claim 1, wherein: The portion of the X-rays having the energy range has an energy in the range of 1 keV to 5 keV.
3. The method according to claim 1, wherein: The coating includes at least one of diamond, graphite, boron nitride, or boron grit diamond.
4. The method according to any one of claims 1 to 3, wherein: The coating has a first thermal conductivity that is higher than a second thermal conductivity of the wall.
5. The method according to claim 4, wherein: The coating comprises at least two layers of material, wherein: A first layer of the at least two layers comprises at least one of diamond, graphite, or bobby diamond and has the first thermal conductivity; and A second layer of the at least two layers has a third thermal conductivity having a value between the first thermal conductivity and the second thermal conductivity.
6. The method according to any one of claims 1 to 3, wherein: The thickness of the coating is not less than 50 microns.
7. The method according to any one of claims 1 to 3, wherein: The coating has a thickness of at most three penetration depths of the portions of the X-rays having the energy range.
8. A plasma chamber containing plasma, the plasma chamber comprising: a wall surrounding a volume that contains the plasma when the plasma chamber is in operation; as well as a coating in thermal communication with the inner surface of the wall, the coating being adapted to receive electromagnetic radiation including X-rays from the volume, a portion of the X-rays having an energy range, wherein: The first thermal conductivity of the coating is greater than the second thermal conductivity of the wall; The thickness of the coating is at least half of the penetration depth of the X-rays within the energy range; and In the absence of the coating, at least 50% of the X-rays having the energy range are absorbed within 1 mm of the inner surface of the wall.
9. The plasma chamber of claim 8, wherein: The portion of the X-rays having the energy range has an energy in the range of 1 keV to 5 keV.
10. The plasma chamber of claim 8, wherein: The coating includes at least one of diamond, graphite, boron nitride, or boron grit diamond.
11. The plasma chamber according to any one of claims 8 to 10, wherein: The coating has a thickness of at most three penetration depths of the portions of the X-rays having the energy range.
12. The plasma chamber according to any one of claims 8 to 10, wherein: The thickness of the coating is not less than 50 microns.
13. The plasma chamber according to any one of claims 8 to 10, wherein: The coating has a first thermal damage threshold that is higher than a second thermal damage threshold of the wall.
14. The plasma chamber according to any one of claims 8 to 10, wherein: The coating comprises at least two layers of material, wherein: A first layer of the at least two layers comprises at least one of diamond, graphite, or bobby diamond and has the first thermal conductivity; and A second layer of the at least two layers has a third thermal conductivity having a value between the first thermal conductivity and the second thermal conductivity.
15. The plasma chamber according to any one of claims 8 to 10, wherein: The wall comprises silicon dioxide.
16. A system comprising: A plasma chamber according to any one of claims 8 to 10; a plurality of electromagnetic coils external to the plasma chamber and arranged to generate a magnetic field to confine and manipulate plasma within the plasma chamber; as well as A heat sink is in thermal communication with an exterior surface of a wall of the plasma chamber.
17. The system of claim 16, further comprising circuitry to apply current to the plurality of electromagnetic coils such that the plasma is compressed and at least some atoms within the plasma undergo fusion.
18. The system of claim 16, wherein: The radiator includes a pipe in which a coolant can flow.
19. A system comprising: A plasma chamber having walls extending around an interior volume, the plasma chamber being adapted to support a vacuum in the interior volume, the walls of the plasma chamber having a relative humidity of no greater than 5 W m -1 K -1 Thermal conductivity; a plasma source to generate plasma and inject the plasma into the interior volume of the plasma chamber; at least one gas inlet coupled to the plasma source for introducing a gas or a gaseous mixture into the plasma source; as well as a plurality of electromagnetic coils arranged to generate a magnetic field within the plasma chamber such that interaction of particles of the plasma with the magnetic field generates electromagnetic radiation including X-rays, a first portion of which may be absorbed by a wall of the plasma chamber to cause heating of the wall; Wherein, the plasma chamber further comprises a coating comprising at least one of boron nitride, graphite or diamond, the coating being disposed on an inner surface of a wall of the plasma chamber to absorb at least a second portion of the X-rays included in the first portion of the X-rays, so that local peak heating of the wall near the inner surface occurring during operation of the system due to the absorption of the first portion of the X-rays is reduced compared to the absorption of the first portion of the X-rays that would occur in the absence of the coating.
20. The system of claim 19, further comprising: at least one power supply circuit coupled to the plurality of electromagnetic coils; as well as At least one controller is coupled to the at least one power circuit to control one or more parameters of the magnetic field.
21. The system of claim 19, wherein: The at least one gas inlet comprises a first gas inlet and a second gas inlet, and wherein the system further comprises: a hydrocarbon precursor supply coupled to the first air inlet to deliver a hydrocarbon precursor to the plasma source; and At least one of a protium supply or a deuterium supply is coupled to the second gas inlet to deliver at least one of protium gas or deuterium gas to the plasma source.
22. A system according to any one of claims 19 to 21, wherein: The plasma chamber includes at least one of a dielectric material, a ceramic material, or graphite.
23. A system according to any one of claims 19 to 21, wherein: The plasma chamber comprises quartz.
24. A system according to any one of claims 19 to 21, wherein: The coating is disposed on all exposed surfaces of the interior surface of the wall.
25. A system according to any one of claims 19 to 21, wherein: The coating comprises at least two layers of material, wherein: A first layer of the at least two layers includes at least one of diamond, graphite, or bobby diamond and has a first thermal conductivity; and A second layer of the at least two layers has a second thermal conductivity having a value between the first thermal conductivity and a third thermal conductivity of the wall.
26. The system of any one of claims 19 to 21, further comprising a quartz fiber ribbon or rope disposed on at least a portion of the interior surface of the wall.
27. A system according to any one of claims 19 to 21, wherein: The plasma chamber has a diameter in the range of 0.01 meters to 3.0 meters and a length in the range of 0.2 meters to 6 meters.
28. The system of any one of claims 19 to 21, further comprising a resistive layer disposed on at least a portion of a plasma chamber wall, wherein: The resistive layer provides inductive heating to the plasma chamber.
29. A system according to any one of claims 19 to 21, wherein: The thickness of the coating is not less than 200 microns.
30. A system according to any one of claims 19 to 21, wherein: The thickness of the coating is selected to be at least half the penetration depth of the coating and the first portion of the X-rays, and At least 50% of the first portion of the X-rays are absorbed within a distance into the wall of 20% of the thickness of the wall.
31. A system according to any one of claims 19 to 21, wherein: The coating includes bobby diamond.
32. A system according to any one of claims 19 to 21, wherein: The coating includes diamond.
33. A system according to any one of claims 19 to 21, wherein: The coating includes graphite.
34. A system according to any one of claims 19 to 21, wherein: The coating includes boron nitride.
35. The system of any one of claims 19 to 21, further comprising at least one passage disposed through a wall of the plasma chamber, wherein: The channels are filled with a material having a higher thermal conductivity than the walls.
36. The system of any one of claims 19 to 21, further comprising an interface layer disposed between an inner surface of the plasma chamber and the coating, the interface layer having a second thermal conductivity different from a thermal conductivity of a wall of the plasma chamber and different from a third thermal conductivity of the coating.
37. A system according to any one of claims 19 to 21, wherein: The electromagnetic radiation includes radiation generated by one or more of the following: confinement of the plasma by the magnetic field; compression of the plasma by the magnetic field; or The magnetic field accelerates the plasma.
38. A system according to any one of claims 19 to 21, wherein: The electromagnetic radiation includes bremsstrahlung from interactions between particles of the plasma, interactions between particles of the plasma and the magnetic field, or both.
39. A method of depositing a coating on an inner surface of a wall of a plasma chamber, wherein electromagnetic radiation including X-rays is incident on the coating, a portion of the X-rays having a range of energies, the method comprising: heating the plasma chamber so that the inner surface of the wall is at a temperature of 300° C. to 2500° C.; as well as A gas mixture is introduced into the plasma chamber, the gas mixture comprising: a first gas comprising hydrocarbons; and a second gas comprising at least one of protium or deuterium; generating a plasma in the plasma chamber; and depositing the coating on an interior surface of the wall; in: The coating comprises at least one of diamond, graphite, or bobby diamond; and The coating is deposited to a thickness of at least half of the penetration depth of the portion of X-rays having the energy range; And in the absence of said coating, at least 50% of said X-rays having said energy range are absorbed within 1 millimeter of an inner surface of said wall.
40. The method of claim 39, wherein: The portion of the X-rays having the energy range has an energy in the range of 1 keV to 5 keV.
41. The method of claim 40, wherein: The coating has a thickness of at most three penetration depths of the portions of the X-rays having the energy range.
42. The method of claim 40, wherein: The thickness of the coating is not less than 50 microns.
43. The method of claim 39, wherein: The walls of the plasma chamber include silicon dioxide.
44. A system according to any one of claims 39 to 43, wherein: The coating comprises at least two layers of material, wherein: A first layer of the at least two layers includes at least one of diamond, graphite, boron nitride, or boron grit diamond and has a first thermal conductivity; and A second layer of the at least two layers has a second thermal conductivity having a value between the first thermal conductivity and a third thermal conductivity of the wall.
45. The method of any one of claims 39 to 43, further comprising pre-treating an interior surface of the plasma chamber.
46. A method according to any one of claims 39 to 43, wherein: Generating the plasma includes applying radio frequency (RF) electromagnetic waves to a gas mixture in the plasma chamber to dissociate and ionize the gas mixture.
47. The method of claim 46, wherein: The intensity of the applied RF electromagnetic waves is spatially varied across the plasma chamber to spatially vary the thickness of the coating.
48. A method according to any one of claims 39 to 43, wherein: Depositing the coating includes coating all exposed surfaces of the interior surface of the plasma chamber.
49. The method according to any one of claims 39 to 43, further comprising: Prior to depositing the coating, at least a portion of an interior surface of the plasma chamber is shielded such that at least a portion of the interior surface is not coated during deposition of the coating.
50. The method of claim 49, wherein: Depositing the coating forms a coating in a portion of the plasma chamber centered about a region of the plasma chamber where plasma within the plasma chamber is compressed to its minimum spatial extent during operation of the plasma chamber.
51. A method according to any one of claims 39 to 43, wherein: The hydrocarbon is at least one of methane, deuterated methane, or silane.
52. The method according to any one of claims 39 to 43, wherein: The second gas is deuterium.
53. The method according to any one of claims 39 to 43, wherein: Generating the plasma includes generating at least one of a pulsed RF electromagnetic wave or a continuous RF electromagnetic wave.
54. The method of claim 53, wherein: The pulsed RF electromagnetic wave has a frequency in the range of 0.1 MHz to 10 MHz and a power in the range of 0.1 GW to 10 GW.
55. The method of claim 53, wherein: The continuous RF electromagnetic wave has a frequency in the range of 100 MHz to 3000 MHz and a power in the range of 10 kW to 100 kW.
56. A method according to any one of claims 39 to 43, wherein: Heating the inner surface includes heating the inner surface via the plasma.
57. A method according to any one of claims 39 to 43, wherein: Heating the interior surface includes inductively heating a wall of the plasma chamber.
58. A method according to any one of claims 39 to 43, wherein: Heating the interior surface includes generating infrared light in the plasma chamber.
59. A method of refurbishing a coating on an interior surface of a plasma confinement system, the plasma confinement system comprising: a plasma chamber having a bobby diamond coating on at least a portion of an interior surface of the plasma chamber, wherein the bobby diamond coating is arranged to receive X-rays having a range of energies from a plasma confined by the plasma confinement system; The method comprises: purging the plasma chamber to remove any residual gas; heating the inner surface of the plasma chamber to a temperature in the range of 300°C to about 2500°C; A gas mixture is introduced into the plasma chamber, the gas mixture comprising: a first gas comprising hydrocarbons; and a second gas comprising at least one of protium or deuterium; generating plasma in the plasma chamber by applying radio frequency electromagnetic waves to dissociate and ionize the gas mixture; and Additional diamond grains are deposited on the diamond grain coating to renew the diamond grain coating on the inner surface of the plasma chamber, so that the renew diamond grain coating absorbs at least half of the X-rays having the energy range.