Shape memory frozen gel, frozen gel sponge and preparation methods of shape memory frozen gel and frozen gel sponge
The shape memory frozen gel is formed by combining polymer surfactants, polysaccharides and amino-containing polymer compounds, and two-dimensional vermiculite is added, which solves the problem of the lack of shape memory function of frozen gels in the prior art, and achieves narrowness Quick hemostasis effect of wounds.
Patent Information
- Application Number
- CN202411202571.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing frozen gel system lacks shape memory function and cannot be effectively applied to hemostasis of narrow wounds. Traditional polymer sponges also have difficulties when compressing into narrow wounds.
Using a combination of polymer surfactant, polysaccharide and amino polymer compounds, a shape memory frozen gel with an interpenetrating network structure is formed through frozen cross-linking, and two-dimensional vermiculite is added during the preparation process to activate the coagulation factor and improve blood cessation. Effect.
The preparation of shape memory frozen gel is realized, with high porosity and dense network, which can be used quickly and effectively for hemostasis of non-compressive wounds, and improve coagulation efficiency by loading two-dimensional vermiculite, enhancing commercial value and application potential.
Smart Images

Figure CN119033997A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of medical technology, and in particular relates to a shape memory cryogel and a cryogel sponge and a preparation method thereof. Background Art
[0002] Penetrating, non-compressible wounds frequently occur in warfare, traumatic accidents, and surgery. Death after penetrating injuries is often associated with hemorrhage. Excessive bleeding can cause hypothermia, coagulopathy, infection, acidosis, and multiple organ failure, all of which contribute to the excess mortality rate. Therefore, the massive hemorrhage caused by penetrating injuries brings great stress to patients and medical staff.
[0003] Cryogel is a gel that forms a network structure by cross-linking at low temperature. Compared with traditional hydrogel, it has a large pore structure, and liquid can enter and exit freely. It has strong potential for hemostasis in penetrating wounds. Cryogel has water-triggered shape memory behavior. When the water of cryogel is squeezed out, it can remain in a contracted state in the air. When water is reabsorbed, its shape can be restored sharply. Shape memory cryogels show unique characteristics in hemostatic applications in narrow or penetrating wounds. They can be delivered to the wound site in a fixed state by extrusion method, and restore their shape to fill the wound boundary when in contact with human bleeding blood. In the cryogel system of gelatin and hyaluronic acid, the dissipation energy of the system is increased due to the rigid covalent network, but the inherent shape memory function is lacking, and the fixed shape cannot be maintained, and it cannot be applied to hemostasis of narrow wounds. On the other hand, many polymer sponges have been used as hemostatic agents to treat non-pressable bleeding and show a certain degree of hemostatic ability. However, they lack shape memory function and cannot enter narrow wounds by compression. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a shape memory cryogel and cryogel sponge and a preparation method thereof to solve the problem of lack of shape memory function in the cryogel system of gelatin and hyaluronic acid in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a shape memory cryogel comprises the following steps: uniformly mixing a polymer surfactant solution, a polysaccharide solution and an amino-containing polymer compound solution, adding a crosslinking agent to form a mixed system, and then performing freezing crosslinking to obtain a shape memory cryogel.
[0007] A further improvement of the present invention is:
[0008] Preferably, the polymer surfactant solution is prepared by dissolving a polymer surfactant in water; the polymer surfactant is any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyether F-127, polyethylene imine, polymaleimide, polyacrylate, polyethylene oxide propylene oxide, water-soluble phenolic resin, amino resin and sorbitan ester;
[0009] The polysaccharide solution is prepared by dissolving polysaccharide in water; the polysaccharide is any one or more of hyaluronic acid, sodium alginate, carboxymethyl chitosan, malic acid, agaric acid, erythritol, alginic acid, naringin, hawthorn glycosides, echinoxanthin and cyprinoside;
[0010] The amino-containing polymer compound solution is obtained by dissolving an amino-containing polymer compound in water, and the amino-containing polymer compound is any one or more of gelatin, bovine serum albumin, polyacrylamide, chitosan, aminopolylactic acid, aminohyaluronic acid and collagen.
[0011] Preferably, the cross-linking agent is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide;
[0012] The added amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 0.01% to 5% of the mass of the mixed system, and the added amount of N-hydroxysuccinimide is 0.02% to 5% of the mass of the mixed system.
[0013] Preferably, the mass fraction of the amino-containing polymer compound in the mixed system is 0.1% to 25%; the mass fraction of the polysaccharide in the mixed system is 0.1% to 25%; and the mass fraction of the polymer surfactant in the mixed system is 0.01% to 15%.
[0014] Preferably, the freezing cross-linking temperature is -80 to 80°C, and the cross-linking time is 1 to 120 hours.
[0015] Preferably, after the polymer surfactant solution, the polysaccharide solution and the amino-containing polymer compound solution are mixed, the two-dimensional vermiculite suspension is added.
[0016] A shape memory cryogel prepared by any one of the above preparation methods, wherein the polymer surfactant, the polysaccharide and the amino-containing polymer compound form an interpenetrating network.
[0017] Preferably, two-dimensional vermiculite is distributed in the interpenetrating network.
[0018] A method for preparing a frozen gel sponge comprises placing the above-mentioned frozen gel in an environment of -80°C to -20°C, freezing for 1 to 72 hours, and freeze-drying the frozen product to prepare a frozen gel sponge, wherein the freeze-drying temperature is -80°C to -20°C, and the freeze-drying time is 1 hour to 120 hours.
[0019] A frozen gel sponge prepared by the preparation method.
[0020] A frozen gel sponge prepared by the preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The invention discloses a method for preparing a shape memory cryogel based on a polymer surfactant, a polysaccharide and an amino-containing polymer compound. The method comprises the steps of fully mixing a polymer surfactant solution and a polysaccharide solution with an amino-containing polymer compound solution, adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide as crosslinking agents, and obtaining a shape memory cryogel after crosslinking and thawing. The general amino-containing polymer compound crosslinked gel is an aerogel obtained after freeze-drying of a hydrogel, and does not have a shape memory function. The present invention utilizes a polymer surfactant and a polysaccharide to generate dense and stable bubbles after mixing. The bubbles can be used as a pore-forming agent, and the physical crosslinking of the polymer surfactant surface and the system to form hydrogen bonds can obtain a cryogel with a higher porosity and a denser network. The high porosity and dense network can reduce the energy dissipation of the system, thereby having a shape memory function. Furthermore, the formed cryogel uses inexpensive and easily scalable polymer surfactants, polysaccharides and amino-containing polymer compounds as raw materials, which greatly enhances its commercial value and application potential. The shape memory cryogel prepared by the present invention has the characteristic of rapid hemostasis for non-pressible wounds.
[0023] Further, two-dimensional vermiculite can also be added during the preparation of cryogel, and cryogel loaded with two-dimensional vermiculite can be obtained after thawing. Vermiculite, as a silicon-based mineral material, has the same negative charge as kaolin, and has negatively charged silanol groups on the surface, which can interact with positively charged amino acids on the coagulation factor XII chain, activate coagulation factors, activate the intrinsic coagulation pathway, and accelerate the coagulation cascade reaction, thereby improving the hemostatic effect of cryogel materials, while traditional silicon-based mineral materials are mostly zeolites and kaolin, which are prone to cause thermal damage and thrombosis of tissues. In the case of emergency bleeding, timely hemostatic effect can be achieved by pressing and packing the cryogel. Moreover, vermiculite is inexpensive, which greatly enhances its commercial value and application potential.
[0024] The present invention also discloses a method for preparing a cryogel sponge, which is a product obtained by freeze-drying the cryogel. The moisture in the cryogel is drained by freeze-drying technology, and the cryogel sponge can be stored for a longer period of time, making it convenient for next use. Moreover, after encountering liquid, the shape memory function is still maintained, which can meet the needs of packing and pressing some emergency bleeding sites during surgery to achieve hemostasis. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The water-triggered shape memory image of the cryogel of polyvinyl pyrrolidone, hyaluronic acid and gelatin prepared in Example 1 of the present invention;
[0026] (a) shows the cryogel without surfactant, (b) shows the cryogel with polyvinyl pyrrolidone added
[0027] Figure 2 The water-triggered shape memory image of the cryogel of polyvinyl alcohol, hyaluronic acid and gelatin prepared in Example 4 of the present invention;
[0028] Figure 3 This is a water-triggered shape memory image of the cryogel of polyether P-F127, hyaluronic acid and gelatin prepared in Example 5 of the present invention;
[0029] Figure 4 The water-triggered shape memory image of the cryogel of polyethylene glycol, hyaluronic acid and gelatin prepared in Example 6 of the present invention;
[0030] Figure 5 This is a water-triggered shape memory image of a cryogel of polyvinyl pyrrolidone, sodium alginate and gelatin prepared in Example 7 of the present invention;
[0031] Among them, (a) is a sodium alginate system; (b) is a polyvinyl pyrrolidone-sodium alginate system;
[0032] Figure 6 This is a water-triggered shape memory image of the cryogel of polyvinyl alcohol, sodium alginate and gelatin prepared in Example 6 of the present invention;
[0033] Figure 7 This is a water-triggered shape memory image of the cryogel of polyether P-F127, sodium alginate and gelatin prepared in Example 7 of the present invention;
[0034] Figure 8 This is a water-triggered shape memory image of a cryogel of polyethylene glycol, sodium alginate and gelatin prepared in Example 8 of the present invention;
[0035] Fig. 9 This is a diagram for verifying the effect of Example 9 of the present invention;
[0036] (a) The picture shows the bleeding of rat liver treated with medical gelatin sponge and vermiculite cryogel, (b) The picture shows the blood loss of rat liver treated with medical gelatin sponge and vermiculite cryogel, (c) The picture shows the hemostasis time of rat liver treated with medical gelatin sponge and vermiculite cryogel. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0038] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0039] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0040] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0041] The first aspect of the present invention discloses a method for preparing a shape memory cryogel, specifically a method for preparing a shape memory cryogel based on a polymer surfactant, a polysaccharide and an amino-containing polymer compound, and the specific preparation process is:
[0042] After the polymer surfactant solution, polysaccharide solution and amino-containing polymer compound solution are fully mixed, a cross-linking agent is added to form a mixed system, and frozen cross-linking is performed to obtain a shape memory cryogel. In this process, the polymer surfactant and polysaccharide are mixed to produce dense and stable bubbles, which can be used as pore-forming agents, and the polymer surfactant and the system are physically cross-linked, and after thawing, a cryogel with higher porosity and denser network is obtained.
[0043] The polymer surfactant solution is prepared by dissolving a polymer surfactant in water; the polysaccharide solution is prepared by dissolving a polysaccharide in water; and the amino-containing polymer compound solution is prepared by dissolving an amino-containing polymer compound in water.
[0044] The cross-linking agents are 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide.
[0045] In some embodiments of the present invention, the mass fraction of the amino-containing polymer compound in the mixed system is 0.1% to 25%.
[0046] As a preferred solution, the mass fraction of the amino-containing polymer compound in the mixed system is 1% to 15%.
[0047] In some embodiments of the present invention, the mass fraction of the polysaccharide in the mixed system is 0.1% to 25%.
[0048] As a preferred solution, the mass fraction of the polysaccharide in the mixed system is 1% to 5%.
[0049] In some embodiments of the present invention, the mass fraction of the high molecular surfactant in the mixed system is 0.01% to 15%.
[0050] As a preferred solution, the mass fraction of the high molecular surfactant in the mixed system is 1% to 5%.
[0051] In some embodiments of the present invention, the polysaccharide is any one or more of hyaluronic acid, sodium alginate, carboxymethyl chitosan, malic acid, agaric acid, erythritic acid, alginic acid, naringin, hawthorn glycosides, echinoxanthin and cyprinoside.
[0052] In some embodiments of the present invention, the polymer surfactant is an active agent with a molecular weight greater than 2000, any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyether F-127, polyethylene imine, polymaleimide, polyacrylate, polyethylene oxide propylene oxide, water-soluble phenolic resin, amino resin and sorbitan ester; the polymer surfactant can reduce surface tension and generate bubbles.
[0053] In some embodiments of the present invention, the amino-containing polymer compound is any one or more of gelatin, bovine serum albumin, polyacrylamide, chitosan, amino polylactic acid, amino hyaluronic acid and collagen.
[0054] In some embodiments of the present invention, the cross-linking temperature is between -80 and 80° C., and the cross-linking time is between 1 and 120 hours.
[0055] In some embodiments of the present invention, a method for preparing a shape memory cryogel is disclosed: 5 to 1250 mg of an amino-containing polymer compound is dissolved in 2.5 mL of water to form an amino-containing polymer compound solution; 5 to 1250 mg of a polysaccharide is dissolved in 2 mL of water to form a polysaccharide solution. The amino-containing polymer compound solution and the polysaccharide solution are mixed evenly, and then 0.5 to 750 mg of a polymer surfactant is added to form a mixed system, and then 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are added as cross-linking agents, wherein the amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride added is 0.01% to 0.5% of the mass of the mixed system, and the amount of N-hydroxysuccinimide added is 0.02% to 5% of the mass of the mixed system. After mixing evenly, the mixture is frozen at -80 to -80°C for 1 to 120 hours, and the cryogel is obtained after thawing.
[0056] As a preferred solution, the amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride added is 0.01% to 0.5% of the mass of the mixed system, and the amount of N-hydroxysuccinimide added is 0.02% to 0.5% of the mass of the mixed system.
[0057] In some embodiments of the present invention, two-dimensional vermiculite is loaded in the above-mentioned shape memory cryogel, the above-mentioned amino polymer compound solution, polysaccharide solution and polymer surfactant are fully mixed, and then the two-dimensional vermiculite suspension is added, and then 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are added as cross-linking agents. After mixing evenly, the mixture is frozen at -80 to 80°C for 1 to 120 hours, and after thawing, a cryogel loaded with two-dimensional vermiculite material is obtained.
[0058] Preferably, the preparation process of the two-dimensional vermiculite is as follows: the three-dimensional vermiculite is sequentially placed in a NaCl solution and a LiCl solution for ion intercalation, so that the three-dimensional structure expands. Then, after being mixed with 30% hydrogen peroxide, the mixture is condensed and refluxed at 110° C., and the generated oxygen peels the expanded vermiculite into a two-dimensional sheet structure, and finally a two-dimensional vermiculite solution is prepared.
[0059] One of the implementation cases provided by the present invention is to provide a method for preparing a shape memory cryogel loaded with two-dimensional vermiculite, comprising the following steps:
[0060] (1) Vermiculite peeling. The three-dimensional vermiculite was separated by Na + Solution and Li + The solution was subjected to ion intercalation, and then mixed with 30% hydrogen peroxide, and condensed and refluxed at 110° C. to obtain a two-dimensional vermiculite solution.
[0061] (2) Preparation of cryogel loaded with two-dimensional vermiculite. Dissolve 5-1250 mg of gelatin in 2.5 mL of water to form a gelatin solution; dissolve 5-1250 mg of polysaccharide in 2 mL of water to form a polysaccharide solution. Mix the gelatin solution and the polysaccharide solution evenly, then add 0.5-750 mg of a polymer surfactant, then add 1-10 mg of a two-dimensional vermiculite suspension, and finally add 0.5-250 mg of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 1-250 mg of N-hydroxysuccinimide as a cross-linking agent, mix evenly, and freeze at -20°C for 20 h. After thawing, a cryogel is obtained.
[0062] The second aspect of the present invention discloses a shape memory cryogel based on a polymer surfactant, a polysaccharide and an amino-containing polymer compound prepared by the above method, wherein the shape memory cryogel is a gel having an interpenetrating network structure formed by the polymer surfactant, the polysaccharide and the amino-containing polymer compound. When the cryogel is used, the cryogel can be compressed into a fixed shape in a wet state, filled into a wound, and restored to its original shape by absorbing blood from the wound, thereby playing a role in stopping bleeding.
[0063] Furthermore, when two-dimensional vermiculite is added to the gel, the two-dimensional vermiculite is distributed in the interpenetrating network structure formed above.
[0064] The third aspect of the present invention discloses a method for preparing a cryogel sponge. In order to improve the utilization rate of cryogel and make it easier to store, cryogel is made into a sponge. The specific process is: put the hydrogel into an environment of -80℃ to -20℃, freeze for 1 to 72 hours, freeze the frozen product in a freeze dryer for 1 hour to 120 hours, and the freeze drying temperature is -80 to -20℃ to make a cryogel sponge.
[0065] As a preferred solution, the freezing temperature is -80°C. The frozen product is freeze-dried in a freeze dryer for 24h to 48h at a freeze drying temperature of -80°C to prepare a frozen gel sponge, which is dried and stored at -80 to 4°C for a long term.
[0066] The fourth aspect of the present invention discloses a cryogel sponge prepared by the above method.
[0067] The following is further described in conjunction with specific embodiments:
[0068] Example 1
[0069] Polyvinyl pyrrolidone, hyaluronic acid and gelatin are examples of the raw materials of shape memory cryogels of polymer surfactants, polysaccharides and amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 60 mg of polyvinyl pyrrolidone. The hyaluronic acid solution and polyvinyl pyrrolidone solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C to react for 16 hours. After thawing, the mixture was soaked in deionized water to remove unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel. Figure 1 As shown, the cryogel with polyvinyl pyrrolidone, hyaluronic acid and gelatin as monomers has good water-triggered shape memory properties.
[0070] Example 2
[0071] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino polymer compounds are polyvinyl pyrrolidone, hyaluronic acid and gelatin. At 37°C, 5 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 5 mg of hyaluronic acid and 0.5 mg of polyvinyl pyrrolidone. The hyaluronic acid solution and polyvinyl pyrrolidone solution were fully mixed with the gelatin solution, and then 0.5 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 1 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into the mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel.
[0072] Example 3
[0073] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino polymer compounds are polyvinyl pyrrolidone, hyaluronic acid and gelatin. At 37°C, 1250 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 1250 mg of hyaluronic acid and 750 mg of polyvinyl pyrrolidone. The hyaluronic acid solution and polyvinyl pyrrolidone solution were fully mixed with the gelatin solution, and then 250 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 250 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen and placed in a vacuum freeze dryer for freeze drying for 2 days to obtain a dry cryogel.
[0074] Example 4
[0075] Polymer surfactants, polysaccharides and amino-containing polymer compounds are used as shape memory cryogel raw materials, including polyvinyl alcohol, hyaluronic acid and gelatin. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid in deionized water, and 50 mg of polyvinyl alcohol is dissolved at 80°C. The hyaluronic acid solution and polyvinyl alcohol solution are fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, the mixture is poured into a mold. The mixture is placed at -20°C to react for 16 hours. After thawing, it is soaked in deionized water to remove unreacted monomers, and finally frozen. It is placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel. Figure 2 As shown, the cryogel with polyvinyl alcohol, hyaluronic acid and gelatin as monomers has good water-triggered shape memory properties.
[0076] Example 5
[0077] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino-containing polymer compounds are polyether P-F127, hyaluronic acid and gelatin. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 80 mg of polyether P-F127. The hyaluronic acid solution and the polyether P-F127 solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C to react for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers. Finally, the mixture was frozen and placed in a vacuum freeze dryer for freeze drying for 2 days to obtain a dry cryogel. Figure 3 As shown, the cryogel with polyether P-F127, hyaluronic acid and gelatin as monomers has good water-triggered shape memory properties.
[0078] Example 6
[0079] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino polymer compounds are polyethylene glycol, hyaluronic acid and gelatin as examples. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 40 mg of polyethylene glycol. The hyaluronic acid solution and polyethylene glycol solution are fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, pour into the mold. Place it at -20°C to react for 16 hours. After thawing, soak it in deionized water to remove the unreacted monomers, and finally freeze it. Put it in a vacuum freeze dryer and freeze-dry it for 2 days to obtain a dry cryogel. Figure 4 As shown, the cryogel with polyethylene glycol, hyaluronic acid and gelatin as monomers has good water-triggered shape memory properties.
[0080] Example 7
[0081] Polyvinyl pyrrolidone, sodium alginate and gelatin are examples of the raw materials for shape memory cryogels of polymer surfactants, polysaccharides and amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of sodium alginate and 60 mg of polyvinyl pyrrolidone. The sodium alginate solution and polyvinyl pyrrolidone solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C to react for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel. Figure 5 As shown, the cryogel with polyvinyl pyrrolidone, sodium alginate and gelatin as monomers has good water-triggered shape memory properties.
[0082] Example 8
[0083] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino-containing polymer compounds are polyvinyl alcohol, sodium alginate and gelatin. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, and then 15 mg of sodium alginate is dissolved in deionized water. The dissolution of 100 mg of polyvinyl alcohol is carried out at 80°C. The sodium alginate solution and the polyvinyl alcohol solution are fully mixed with the gelatin solution. Then, 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, pour into the mold. Place it at -20°C to react for 16 hours. After thawing, soak it in deionized water to remove the unreacted monomers, and finally freeze it. Put it in a vacuum freeze dryer and freeze-dry it for 2 days to obtain a dry cryogel. Figure 6 As shown, the cryogel with polyvinyl alcohol, sodium alginate and gelatin as monomers has good water-triggered shape memory properties.
[0084] Example 9
[0085] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino-containing polymer compounds are polyether P-F127, sodium alginate and gelatin. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 15 mg of sodium alginate and 150 mg of polyether P-F127. The sodium alginate solution and the polyether P-F127 solution are fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, pour into the mold. Place it at -20°C to react for 16 hours. After thawing, soak it in deionized water to remove the unreacted monomers, and finally freeze it. Put it in a vacuum freeze dryer and freeze-dry it for 2 days to obtain a dry cryogel. Figure 7 As shown, the cryogel with polyether P-F127, sodium alginate and gelatin as monomers has good water-triggered shape memory properties.
[0086] Example 10
[0087] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino polymer compounds are polyethylene glycol, sodium alginate and gelatin as examples. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 150 mg of polyethylene glycol. The sodium alginate solution and polyethylene glycol solution are fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, pour into the mold. Place it at -20°C to react for 16 hours. After thawing, soak it in deionized water to remove the unreacted monomers, and finally freeze it. Put it in a vacuum freeze dryer and freeze-dry it for 2 days to obtain a dry cryogel. Figure 8 As shown, the cryogel with polyethylene glycol, sodium alginate and gelatin as monomers has good water-triggered shape memory properties.
[0088] Embodiment 11
[0089] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyvinyl pyrrolidone surfactant, hyaluronic acid polysaccharide and gelatin amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 60 mg of polyvinyl pyrrolidone. The hyaluronic acid, polyvinyl pyrrolidone solution and the above-exfoliated vermiculite solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite. The cryogel was filled into the wound of the liver of SD rats (the wound was a circle with a diameter of 12 mm). Fig. 9 As shown, the shape memory cryogel loaded with two-dimensional vermiculite had less blood loss and shorter hemostasis time compared with the medical sponge group.
[0090] Example 12
[0091] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyvinyl alcohol surfactant, hyaluronic acid polysaccharide and gelatin amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 50 mg of polyvinyl alcohol. The hyaluronic acid, polyvinyl alcohol solution and the above-exfoliated vermiculite solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite.
[0092] Example 13
[0093] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyether P-F127 surfactant, hyaluronic acid polysaccharide and gelatin amino-containing polymer compounds as examples. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 80 mg of polyether P-F127. The hyaluronic acid, polyether P-F127 solution and the above-exfoliated vermiculite solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite.
[0094] Embodiment 14
[0095] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyethylene glycol surfactant, hyaluronic acid polysaccharide and gelatin amino-containing polymer compounds as examples. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 15 mg of hyaluronic acid and 40 mg of polyethylene glycol. The hyaluronic acid, polyethylene glycol solution and the above-exfoliated vermiculite solution are fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, pour into the mold. Place it at -20°C for reaction for 16 hours, thaw it, soak it in deionized water to remove the unreacted monomers, and finally freeze it. Put it in a vacuum freeze dryer and freeze-dry it for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite.
[0096] Embodiment 15
[0097] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyvinyl pyrrolidone surfactant, sodium alginate polysaccharide and gelatin amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of sodium alginate and 60 mg of polyvinyl pyrrolidone. The sodium alginate, polyvinyl pyrrolidone solution and the above-exfoliated vermiculite solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite. The cryogel was filled into the wound of the liver of SD rats (the wound was a circle with a diameter of 12 mm). Fig. 9 As shown, the shape memory cryogel loaded with two-dimensional vermiculite had less blood loss and shorter hemostasis time compared with the medical sponge group.
[0098] Example 16
[0099] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyvinyl alcohol surfactant, sodium alginate polysaccharide and gelatin amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of sodium alginate and 100 mg of polyvinyl alcohol. The sodium alginate, polyvinyl alcohol solution and the above-exfoliated vermiculite solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite.
[0100] Embodiment 17
[0101] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyether P-F127 surfactant, sodium alginate polysaccharide and gelatin amino-containing polymer compounds. At 37°C, 200 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 15 mg of sodium alginate and 150 mg of polyether P-F127. The sodium alginate, polyether P-F127 solutions and the above-exfoliated vermiculite solution were fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -20°C for reaction for 16 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen. The mixture was placed in a vacuum freeze dryer and freeze-dried for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite.
[0102] Embodiment 18
[0103] The raw materials of the shape memory cryogel loaded with two-dimensional vermiculite are polyethylene glycol surfactant, sodium alginate polysaccharide and gelatin amino-containing polymer compounds. At 37°C, 200 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 15 mg of sodium alginate and 150 mg of polyethylene glycol. The sodium alginate, polyethylene glycol solution and the above-exfoliated vermiculite solution are fully mixed with the gelatin solution, and then 18 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 12 mg of N-hydroxysuccinimide (NHS) are added to the system, mixed thoroughly, and poured into the mold. The reaction is placed at -20°C for 16 hours. After thawing, it is soaked in deionized water to remove the unreacted monomers, and finally frozen and placed in a vacuum freeze dryer for freeze drying for 2 days to obtain a dry cryogel loaded with two-dimensional vermiculite.
[0104] Embodiment 19
[0105] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino polymer compounds are polyvinyl pyrrolidone, hyaluronic acid and gelatin. At 37°C, 50 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 10 mg of hyaluronic acid and 45 mg of polyvinyl pyrrolidone. The hyaluronic acid solution and polyvinyl pyrrolidone solution were fully mixed with the gelatin solution, and then 15 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 10 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -80°C for reaction for 50 hours. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen and placed in a vacuum freeze dryer for freeze drying for 2 days to obtain a dry cryogel.
[0106] Embodiment 20
[0107] The raw materials of shape memory cryogel of polymer surfactants, polysaccharides and amino polymer compounds are polyvinyl pyrrolidone, hyaluronic acid and gelatin. At 37°C, 750 mg of gelatin was dissolved in 2.5 mL of deionized water, followed by 50 mg of hyaluronic acid and 150 mg of polyvinyl pyrrolidone. The hyaluronic acid solution and polyvinyl pyrrolidone solution were fully mixed with the gelatin solution, and then 25 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 15 mg of N-hydroxysuccinimide (NHS) were added to the system. After fully mixing, the mixture was poured into a mold. The mixture was placed at -80°C for reaction for 1 hour. After thawing, the mixture was soaked in deionized water to remove the unreacted monomers, and finally frozen and placed in a vacuum freeze dryer for freeze drying for 2 days to obtain a dry cryogel.
[0108] Embodiment 21
[0109] Polymer surfactants, polysaccharides and amino-containing polymers are used as shape memory cryogel raw materials, such as polyvinyl pyrrolidone, hyaluronic acid and gelatin. At 37°C, 750 mg of gelatin is dissolved in 2.5 mL of deionized water, followed by 50 mg of hyaluronic acid and 150 mg of polyvinyl pyrrolidone. The hyaluronic acid solution and polyvinyl pyrrolidone solution are fully mixed with the gelatin solution, and then 25 mg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) and 15 mg of N-hydroxysuccinimide (NHS) are added to the system. After fully mixing, the mixture is poured into a mold. The mixture is placed at -20°C for reaction for 120 hours. After thawing, the mixture is soaked in deionized water to remove the unreacted monomers, and finally frozen and placed in a vacuum freeze dryer for freeze drying for 2 days to obtain a dry cryogel.
[0110] Embodiment 22
[0111] The cryogel prepared in Example 1 was placed in a -20°C environment and frozen for 10 hours. The frozen product was freeze-dried at -20°C for 20 hours to obtain a cryogel sponge.
[0112] Embodiment 23
[0113] The cryogel prepared in Example 1 was placed in a -80°C environment and frozen for 1 hour. The frozen product was freeze-dried at -80°C for 1 hour to obtain a cryogel sponge.
[0114] Embodiment 24
[0115] The cryogel prepared in Example 1 was placed in a -60°C environment and frozen for 72 hours. The frozen product was freeze-dried at -60°C for 120 hours to obtain a cryogel sponge.
[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a shape memory cryogel, characterized in that: The method comprises the following steps: uniformly mixing a polymer surfactant solution, a polysaccharide solution and an amino-containing polymer compound solution, adding a crosslinking agent to form a mixed system, and then performing freezing crosslinking to obtain a shape memory cryogel.
2. The method for preparing a shape memory cryogel according to claim 1, characterized in that: The polymer surfactant solution is prepared by dissolving the polymer surfactant in water; the polymer surfactant is any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyether F-127, polyethylene imine, polymaleimide, polyacrylate, polyethylene oxide propylene oxide, water-soluble phenolic resin, amino resin and sorbitan ester; The polysaccharide solution is prepared by dissolving polysaccharide in water; the polysaccharide is any one or more of hyaluronic acid, sodium alginate, carboxymethyl chitosan, malic acid, agaric acid, erythritol, alginic acid, naringin, hawthorn glycosides, echinoxanthin and cyprinoside; The amino-containing polymer compound solution is obtained by dissolving an amino-containing polymer compound in water, and the amino-containing polymer compound is any one or more of gelatin, bovine serum albumin, polyacrylamide, chitosan, aminopolylactic acid, aminohyaluronic acid and collagen.
3. The method for preparing a shape memory cryogel according to claim 1, characterized in that: The cross-linking agent is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide; The added amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 0.01% to 5% of the mass of the mixed system, and the added amount of N-hydroxysuccinimide is 0.02% to 5% of the mass of the mixed system.
4. The method for preparing a shape memory cryogel according to claim 1, characterized in that: The mass fraction of the amino-containing polymer compound in the mixed system is 0.1% to 25%; the mass fraction of the polysaccharide in the mixed system is 0.1% to 25%; and the mass fraction of the polymer surfactant in the mixed system is 0.01% to 15%.
5. The method for preparing a shape memory cryogel according to claim 1, characterized in that: The freezing cross-linking temperature is -80 to 80°C, and the cross-linking time is 1 to 120 hours.
6. The method for preparing a shape memory cryogel according to claim 1, characterized in that: After the polymer surfactant solution, the polysaccharide solution and the amino-containing polymer compound solution are mixed, the two-dimensional vermiculite suspension is added.
7. A shape memory cryogel prepared by the preparation method according to any one of claims 1, characterized in that: The polymer surfactant, polysaccharide and amino-containing polymer compound form an interpenetrating network.
8. The shape memory cryogel according to claim 7, characterized in that: Two-dimensional vermiculite is distributed in the interpenetrating network.
9. A method for preparing a cryogel sponge, characterized in that: The cryogel according to claim 7 or 8 is placed in an environment of -80°C to -20°C, frozen for 1 to 72 hours, and the frozen product is freeze-dried to prepare a cryogel sponge, wherein the freeze-drying temperature is -80°C to -20°C, and the freeze-drying time is 1 hour to 120 hours.
10. A cryogel sponge prepared by the preparation method of claim 9.
Citation Information
Patent Citations
Aerogel material and preparation method thereof
CN103599734A
Preparation method of gelatin filled silk protein gelatin gel fiber membrane
CN108560244A
Rapid hemostatic sponge and preparation method thereof
CN114569783A
Shape memory double-network cryogel as well as preparation method and application thereof
CN117285727A
Hemostatic sponge with high imbibition capacity and preparation method thereof
CN117982715A