Preparation method of ordered hierarchical pore composite adsorbent for removing oxygen-containing compounds from light hydrocarbons
By introducing metals such as copper and nickel into light hydrocarbon adsorbents, the charge distribution and electrostatic field of the channel are enhanced, and the coordination force is used for deep adsorption, the problems of insufficient adsorption force and difficulty in industrial promotion are solved, and high efficiency is achieved The oxygen-containing compound removal and easy regeneration effect.
Patent Information
- Application Number
- CN202411188405.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, oxygen-containing compound adsorbents in light hydrocarbons have weak adsorption forces, mainly relying on van der Waals forces, easy to desorption, and high investment costs in industrial equipment, difficult to promote industrial use, and cannot take into account both oxygen-containing organic matter and Remove water at the same time.
The TiO2 and Al2O3 precursors with Ti:Al molar ratio of (1-5): (1-5) were dissolved in a mixed solvent of deionized water, ethanol, and strong organic alkali, and surfactant, structural guide agent and organic carbon were added. Source: Prepare adsorbents with multi-stage pore structures through ultrasonic and crystallization reactions, and introduce metals such as copper and nickel into the adsorbent to enhance the charge distribution and electrostatic field strength of the pores, and use coordination force to perform deep adsorption.
The prepared adsorbent has a large specific surface area and pore volume, a large adsorption capacity, strong adsorption force, good deep adsorption effect, and simple regeneration operation. The performance has not decreased significantly after multiple regenerations. It is suitable for industrial applications.
Smart Images

Figure CN119034674A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorbent preparation, and in particular relates to a method for preparing an ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons. Background Art
[0002] The ethylene and propylene industry chains are the two most important industrial chain structures in China's large-scale chemical industry. Ethylene is regarded as a key indicator to define the level of the chemical industry, and propylene is known as the most important basic raw material for the extension of China's chemical industry chain. With the continuous improvement of the refinement rate in China's chemical industry and the rapid construction of domestic PDH units in the past decade, propylene produced by propane dehydrogenation has become an important focus in the propylene industry chain, and its market share is also increasing year by year.
[0003] One of the branches of the C3 (propylene) industry chain currently formed uses propane as the initial raw material, propane dehydrogenation to produce propylene, part of the propylene is oxidized to acrylic acid, and the other part of the propylene reacts with water gas to produce butyl octanol, and finally acrylic acid and butyl octanol are esterified to produce butyl acrylate and octyl acrylate. The propylene production butyl octanol unit will produce unqualified propylene, the main components of which are propylene, propane, butyraldehyde, butanol, water, etc. If this stock of material is used as LPG fuel for the heating furnace, it will cause waste of propylene and propane, and it will not be able to reflect the advantages of the C3 industry chain and realize the concept of maximizing the economic value of the industry chain; if this stock of material is sent to the downstream separation system of the propane dehydrogenation (PDH) unit, impurities such as butyraldehyde, butanol, and water cannot be removed in the propane refining unit, and will enter the reactor together with the propane feed, react with propylene in the high temperature environment of the Pt series catalyst to generate oxygen-containing heterocyclic compounds, promote the formation of coke, block the catalyst pores and surface, and cause the catalyst activity to decrease. In addition, water reacts with coke at high temperature to generate carbon monoxide, which poisons the catalyst. Therefore, if you want to recycle the unqualified propylene from the butanol unit, you must remove the impurities in the unqualified propylene before you can use it.
[0004] Chinese patent CN115722189A discloses "an adsorbent for removing oxygen-containing compounds from low molecular weight hydrocarbons". The adsorbent used in the invention can weaken the competitive adsorption between oxides of different polarities when adsorbing oxygen-containing compounds of different polarities, and has a higher adsorption performance for oxides of weak polarity and large molecular size. However, the adsorption force is the van der Waals force, which is weak, and it is easy to fall off the adsorbent, and the adsorption depth is shallow.
[0005] Chinese patent CN114100568A discloses "an adsorbent for deep removal of oxygenated compounds from Fischer-Tropsch synthetic oil and its preparation method". The adsorbent described in the invention has high adsorption selectivity for oxygenated compounds, fast mass transfer rate, and deep deoxygenation depth. However, the adsorbent needs to be used with an adsorption tower and a desorbent, and the investment and operating costs are relatively high, making it difficult to promote and use in large-scale chemical plants.
[0006] Chinese patent CN117582939A discloses "a preparation method and application of an adsorbent for purifying oxygenated compounds in olefin streams". The adsorbent described in the invention has the advantages of high purification accuracy, low adsorption temperature, low regeneration temperature, simple preparation and high strength. However, the adsorbent is only for the adsorption of organic matter such as methanol, dimethyl ether and propionaldehyde, and does not involve the adsorption of water, which is somewhat one-sided. There is more or less water in the recycled olefin materials of chemical plants, and the water molecules are highly polar and are more easily adsorbed by the adsorbent, hindering the adsorption of other oxygenated compounds.
[0007] In summary, it can be seen from the currently disclosed adsorbents for oxygen-containing compounds in hydrocarbon substances that the adsorption force between oxygen-containing compounds and the adsorbent is weak, mainly dominated by van der Waals force; the investment cost of industrial equipment is high, and it is difficult to promote industrialization; the adsorption range of oxygen-containing compounds is narrow, especially the inability to take into account the simultaneous removal of oxygen-containing organic matter and water. Summary of the invention
[0008] The purpose of the present invention is to provide a method for preparing an ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons. The prepared adsorbent has a large specific surface area, pore volume and high adsorption capacity; the adsorption force between the adsorbent and the oxygen-containing compound is strong, mainly in the form of coordination force, which effectively solves the problem of easy desorption during the adsorption process and realizes deep adsorption; the adsorbent regeneration operation is simple, and the adsorption performance is not significantly reduced after repeated regeneration and reuse.
[0009] To achieve the above purpose, the technical solution of the present invention is as follows:
[0010] A method for preparing an ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons comprises the following steps:
[0011] 1) According to the Ti:Al molar ratio of (1-5):(1-5), weigh a TiO2 precursor and an Al2O3 precursor and dissolve them in a mixed solvent consisting of deionized water, ethanol and a strong organic base to obtain a mixed solution A;
[0012] The volume ratio of deionized water, ethanol and strong organic base in the mixed solvent is (1-10):(1-10):(1-5);
[0013] The mass / volume ratio of the TiO2 precursor to the mixed solvent is 1:(1-20);
[0014] Weigh a certain amount of surfactant, structure directing agent, and organic carbon source and dissolve them in a mixed solution of deionized water and ethanol to obtain a mixed solution B;
[0015] The volume ratio of deionized water to ethanol in the mixed solution is (1-10):(1-10);
[0016] The mass ratio of the TiO2 precursor to the surfactant, the structure directing agent, and the organic carbon source is (1-5):(1-3):(1-3):(1-5);
[0017] The mass / volume ratio of the mixed solution of the surfactant, water and ethanol is 1:(1-20);
[0018] Weigh a certain mass of M x Cl y The solid salt is dissolved in deionized water and stirred until completely dissolved to obtain a mixed solution C;
[0019] The M x Cl y The solid salt is a mixture of two of CuCl2·2H2O, MnCl2·4H2O, NiCl2·6H2O, ZnCl2, CoCl2·6H2O, and MoCl5 and one of NaCl, MgCl2·6H2O, CaCl2·2H2O, and KCl;
[0020] The M x Cl y The mass / volume ratio of solid salt to deionized water is 1:(1-30);
[0021] The M x Cl y The molar ratio of the solid salt M atom to the TiO2 precursor Ti atom is (1-3):(1-10);
[0022] 2) Pour the mixed solution B and the mixed solution C into the mixed solution A, then add a certain amount of polyvinyl pyrrolidone and stir evenly, then add alkali solution to adjust the pH to 10-14, then place it in a sealed environment at a constant temperature of 50-80° C. for 30-60 minutes of ultrasonic treatment, age it at room temperature for 12-24 hours, and finally transfer it to a stainless steel reactor with a polytetrafluoroethylene liner, and perform a constant temperature crystallization reaction at 120-220° C. for 24-48 hours;
[0023] 3) After the crystallization reaction is completed, filter to obtain a solid product, repeatedly wash with deionized water and centrifuge until the pH value is 7±0.5, put the obtained solid into a vacuum drying oven, and dry it at a vacuum constant temperature of 50-100° C. for 10-20 hours; crush the dried solid into a crucible, put it into a muffle furnace and heat it to 450-550° C. at a heating rate of 2-4° C. / min, then calcine at a constant temperature for 4-16 hours, and naturally cool it to room temperature to obtain an ordered multi-level porous composite adsorbent.
[0024] Preferably, the TiO2 precursor is one of tetrabutyl titanate, isopropyl titanate, titanium tetrachloride, ethoxytitanium, and methyl orthotitanate, preferably tetrabutyl titanate.
[0025] Preferably, the Al2O3 precursor is one of aluminum nitrate nonahydrate, ammonium aluminum carbonate, aluminum trichloride, aluminum isopropoxide, and aluminum carbonate, preferably aluminum isopropoxide.
[0026] Preferably, the strong organic base is one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide, preferably tetrapropylammonium hydroxide.
[0027] Preferably, the surfactant is tetrapropylammonium bromide, PEG-2000, P123, hexadecyltrimethylammonium bromide, triethylbenzylammonium chloride, preferably PEG-2000.
[0028] Preferably, the structure directing agent is one of decaamine, dodecylamine, tetradecylamine and hexadecylamine, preferably dodecylamine.
[0029] Preferably, the organic carbon source is one of starch, glucose, sucrose and fructose, preferably glucose.
[0030] Preferably, the M x Cl y The solid salt is a mixture of CuCl2·2H2O, NiCl2·6H2O and CaCl2·2H2O, and the molar ratio of Cu, Ni and Ca is: (1-5):(1-10):(1-5); more preferably, the molar ratio of Cu, Ni and Ca is: (1-2):(3-7):(1-3).
[0031] Preferably, the mass ratio of polyvinyl pyrrolidone to TiO2 precursor is 1:(1-10); further preferably, the mass ratio is 1:(1-6).
[0032] Preferably, the alkali solution is one of 10-15% sodium hydroxide solution, 10-15% potassium hydroxide solution, and 10-15% ammonia water, preferably 10-15% ammonia water.
[0033] Preferably, the crystallization reaction conditions are preferably a constant temperature of 150-200° C. for 24-30 hours.
[0034] Preferably, the calcination conditions are preferably a constant temperature of 480-520° C. for 6-10 hours.
[0035] The present invention introduces metals such as copper and nickel into the interior and surface of the adsorbent during the preparation process of the adsorbent, thereby improving the charge distribution inside the adsorbent pores and enhancing the electrostatic field strength of the pores, thereby increasing the adsorption force of the adsorbent on oxygen-containing polar molecules and reducing the adsorption force on olefins.
[0036] Oxygen in oxygen-containing compounds such as methanol, formaldehyde, dimethyl ether, and water can form complexes with metals such as copper and nickel in the adsorbent. The coordination force is stronger than the general electrostatic attraction and van der Waals force, and can achieve deep adsorption of oxygen-containing organic matter. At a certain regeneration temperature, the coordination bond force between metal complexes is interrupted, and they are blown out of the adsorbent surface and pores under the action of the regeneration gas to achieve regeneration and recycling. Alkaline metal oxides are introduced into the adsorbent surface and pores, preferably adsorbing water molecules, a highly polar substance in light hydrocarbon materials, to ensure the adsorption of organic oxides at other active sites.
[0037] The strong organic base and the primary amine structure directing agent work together to prepare an adsorbent with strong crystallinity and more stable microporous and mesoporous structures. When the adsorbent is regenerated, the coordination bond force is weakened and the formation of hydrogen bonds is inhibited, so that the desorption effect can be achieved at a lower regeneration temperature. The introduction of an organic carbon source during the preparation of the adsorbent helps the pores of the adsorbent to be arranged in an orderly manner during the calcination preparation process and is not easy to collapse.
[0038] Beneficial effects of the present invention:
[0039] The invention introduces metals such as copper and nickel into the interior and surface of the adsorbent, improves the charge distribution inside the pores of the adsorbent, enhances the electrostatic field strength of the pores, increases the adsorption force of the adsorbent on oxygen-containing polar molecules, and reduces the adsorption force on olefins, so that the obtained adsorbent has the advantages of large adsorption capacity, high removal rate of oxygen-containing compounds, easy regeneration, etc. Compared with the adsorbent prepared by the invention patent (authorization announcement number: CN115721962B), the adsorbent of the invention has milder regeneration conditions, low regeneration temperature, short constant temperature time, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a performance diagram of the adsorbent regeneration and reuse in Example 1 of the present invention.
[0041] Figure 2 This is a schematic diagram of the performance evaluation equipment of the ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons of the present invention. DETAILED DESCRIPTION
[0042] The present invention is further described below by means of specific examples, but the examples do not limit the protection scope of the present invention.
[0043] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all commonly used methods in the art unless otherwise specified.
[0044] Example 1 A method for preparing an ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons comprises the following steps:
[0045] 1): Accurately measure 30 mL of deionized water, 30 mL of ethanol, and 6 mL of tetrapropylammonium hydroxide and pour them into a 250 mL beaker a, where the volume ratio of deionized water, ethanol, and tetrapropylammonium hydroxide is 5:5:1. Slowly add 6.0 g of tetrabutyl titanate and 7.2 g of aluminum isopropoxide to the beaker a, where the Ti / Al molar ratio is 1:1, and stir while adding until all are dissolved to obtain a mixed solution A;
[0046] Accurately weigh 3.0 g PEG-2000, 3.0 g dodecylamine, and 6.0 g glucose into a 100 mL beaker b. The mass ratio of tetrabutyl titanate, PEG-2000, dodecylamine, and glucose is 2:1:1:2. Add 30 mL of deionized water and 30 mL of ethanol into beaker b and stir until completely dissolved to obtain a mixed solution B.
[0047] Accurately weigh 0.17 g CuCl2·2H2O, 0.36 g NiCl2·6H2O, and 0.15 g CaCl2·2H2O and pour them into a 10 mL beaker c. The molar ratio of Cu, Ni, and Ca to the Ti atom in tetrabutyl titanate is 1:5, and the molar ratio of Cu, Ni, and Ca is 2:3:2. Add 5.0 mL of deionized water and stir until completely dissolved to obtain a mixed solution C.
[0048] 2) Under a magnetic stirrer, pour the mixed solution B and mixed solution C into the mixed solution A, add 2.0 g of polyvinyl pyrrolidone, the mass ratio of polyvinyl pyrrolidone to tetrabutyl titanate is 1:3, adjust the pH value to 12 with 15% ammonia solution, seal beaker a with plastic wrap and place it in an ultrasonic cleaner for 30 minutes at 60°C water bath, then age it at room temperature for 24 hours, transfer the solution in beaker a into a stainless steel reactor with a polytetrafluoroethylene liner, and perform crystallization reaction at 180°C for 36 hours.
[0049] 3) After the crystallization reaction is completed, take the solid product, wash it repeatedly with deionized water, centrifuge it until the upper layer is washed to a pH value of 7±0.5, and then put the solid into a vacuum drying oven and dry it at 60°C for 10 hours. Pour the dried solid into a crucible, put it into a muffle furnace and heat it to 500°C at a rate of 3°C / min for 8 hours. The calcined product naturally cools to room temperature to obtain an ordered hierarchical porous composite adsorbent.
[0050] The specific surface area, average pore size and pore volume of the adsorbent were measured using the NOVA 4000 automatic adsorption instrument produced by Quantachrome.
[0051] Test for the performance of adsorbents in deoxygenation of compounds
[0052] See also Figure 2 The detection device includes a mixer 10 connected by pipelines, a U-shaped tube resistance furnace 16 and a tail gas incinerator 24. Propylene gas bottle 1, formaldehyde gas bottle 2 and dimethyl ether gas bottle 3 are respectively passed through their own mass flow meters 7, 8, and 9, methanol passes through a high-pressure constant current pump 4, and water passes through a high-pressure constant current pump 5. The above five materials enter the mixer 10 together, and after being evenly mixed, they enter the U-shaped tube resistance furnace 16 through a main ball valve 25 and a volume flow meter 12. A thermometer 17 and a pressure gauge 18 are arranged on the outlet pipeline of the U-shaped tube resistance furnace 16. The outlet pipeline of the U-shaped tube resistance furnace 16 is connected to the tail gas incinerator 24 through a volume flow meter 19, a ball valve 26, and a flame arrester 23; two branch pipelines are also arranged at the outlet of the mixer 10, and one branch pipeline is connected to the tail gas incinerator 24. A hydrogen cylinder 6 and a mass flowmeter 11 are connected, and a filter 13 and a needle valve 14 are sequentially arranged on another branch pipeline. The terminal of the branch pipeline is connected to the adsorption inlet oxide concentration detection, and a secondary branch pipeline is provided at the terminal of the branch pipeline. A needle valve 15 is provided on the secondary branch pipeline, and the terminal of the secondary branch pipeline is connected to the inlet pipeline of the flame arrester 23; a branch pipeline is provided on the pipeline connected to the flame arrester 23 by the outlet of the ball valve 26, and a filter 20 and a needle valve 21 are sequentially arranged on the branch pipeline, and the terminal of the branch pipeline is connected to the adsorption outlet oxide concentration detection, and a secondary branch pipeline is provided at the terminal of the branch pipeline. A needle valve 22 is provided on the secondary branch pipeline, and the terminal of the secondary branch pipeline is connected to the inlet pipeline of the flame arrester 23.
[0053] 5.0 g of ordered multi-level porous composite adsorbent was tableted and crushed (about 20 mesh particles) and loaded into a U-shaped quartz tube. The remaining space was filled with quartz sand and quartz wool. Propylene was used as a light hydrocarbon medium model to test the adsorbent performance. The volume contents of formaldehyde, dimethyl ether, water, and methanol in the mixed gas were 100 ppm, 100 ppm, 50 ppm, and 100 ppm, respectively. The mixed gas flow rate was 200 mL / min, the pressure was 6.0 bar (g), the resistance furnace was kept at a constant temperature of 30°C, and an automatic gas inlet chromatograph was connected to the U-shaped tube resistance furnace. Sampling and analysis were automatically performed every 20 minutes. Timing started from the introduction of the mixed gas. When the oxide concentration at the outlet reached 10 ppm, the timing and adsorption performance test were stopped, and the penetration capacity (in terms of oxygen atoms) of the adsorbent for adsorbing oxygen-containing compounds was calculated.
[0054] The calculation formula of penetration capacity is:
[0055]
[0056] Example 2
[0057] The volume ratio of deionized water, ethanol and tetrapropylammonium hydroxide in Example 1 is replaced by a volume ratio of 5:5:3, and the other steps are the same as in Example 1.
[0058] Example 3
[0059] The Ti / Al molar ratio in Example 1 is replaced by 1:2, and the other steps are the same as in Example 1.
[0060] Example 4
[0061] The mass ratio of tetrabutyl titanate, PEG-2000, dodecylamine and glucose in Example 1 was replaced by a mass ratio of 2:2:3:1, and the other steps were the same as in Example 1.
[0062] Example 5
[0063] The molar ratio of Cu, Ni and Ca in Example 1 is replaced by 2:5:1, and the other steps are the same as in Example 1.
[0064] Example 6
[0065] The crystallization reaction at a constant temperature of 200° C. for 30 h was used instead of the crystallization reaction at a constant temperature of 180° C. for 36 h in Example 1. The other steps were the same as in Example 1.
[0066] Example 7
[0067] The molar ratio of Cu, Ni, Ca to Ti atoms in tetrabutyl titanate is 3:5 instead of 1:5 in Example 1. Other steps are the same as in Example 1.
[0068] Example 8
[0069] The mass ratio of polyvinyl pyrrolidone to tetrabutyl titanate is 1:5 instead of 1:3 in Example 1. The other steps are the same as in Example 1.
[0070] Example 9
[0071] The calcination conditions are as follows: the temperature is increased to 540°C at a heating rate of 3°C / min and then calcined at a constant temperature for 4 hours instead of the temperature is increased to 500°C at a heating rate of 3°C / min and then calcined at a constant temperature for 8 hours in Example 1. The other steps are the same as in Example 1.
[0072] Comparative Example 1
[0073] Instead of adding glucose, the mass ratio of tetrabutyl titanate, PEG-2000, dodecylamine and glucose in Example 1 is 2:1:1:2, and the other steps are the same as Example 1.
[0074] Comparative Example 2
[0075] Polyvinyl pyrrolidone was not added, and the mass ratio of polyvinyl pyrrolidone to tetrabutyl titanate in Example 1 was 1:3. Other steps were the same as in Example 1.
[0076] Comparative Example 3
[0077] NiCl2·6H2O is not added, and the molar ratio of Cu, Ni and Ca in Example 1 is 2:3:2. Other steps are the same as in Example 1.
[0078] Comparative Example 4
[0079] Instead of adding CuCl2·2H2O, NiCl2·6H2O and CaCl2·2H2O, the molar ratio of Cu, Ni and Ca to the Ti atom in tetrabutyl titanate in Example 1 is 1:5, and the other steps are the same as in Example 1.
[0080] Test for the performance of adsorbents in deoxygenation of compounds
[0081] The adsorbent obtained in the embodiments of the present invention and the comparative examples was subjected to a deoxygenation compound performance test. When the oxide concentration at the outlet reached 10 ppm, the adsorption performance test was stopped. Hydrogen was introduced into the U-shaped tube resistance furnace to regenerate the adsorbent. The adsorbent regeneration conditions were as follows: hydrogen flow rate: 100 mL / min, regeneration pressure: 1 bar(g). The U-shaped tube resistance furnace was heated to 150°C at a heating rate of 50°C / h, kept at a constant temperature for 2 hours, cooled to room temperature, hydrogen was stopped, and the U-shaped tube resistance furnace was depressurized. The adsorbent performance test after regeneration was the same as in Example 1, and the regeneration was repeated 10 times. Figure 1 This is a performance diagram of the adsorbent regeneration and reuse in Example 1. It can be seen from the figure that after 10 regenerations, the adsorption capacity of the adsorbent for oxygen-containing compounds is always maintained at a high level, and there is no sign of obvious decline in the adsorbent performance, which has good industrial application prospects.
[0082] The specific surface area and pore volume of the adsorbents prepared in Examples 1 to 9 and Comparative Examples 1 to 3 were measured, and the test results of the adsorption performance for oxygen-containing compounds are listed in Table 1.
[0083] Table 1
[0084]
[0085] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0086] The above is a detailed introduction to the preparation method and application of an ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing an ordered multi-level porous composite adsorbent for removing oxygen-containing compounds from light hydrocarbons. Its characteristics are: The steps include: 1) According to the Ti:Al molar ratio of (1-5):(1-5), weigh TiO 2 Precursor, Al 2 O 3 The precursor is dissolved in a mixed solvent consisting of deionized water, ethanol, and a strong organic base to obtain a mixed solution A; The volume ratio of deionized water, ethanol and strong organic base in the mixed solvent is (1-10):(1-10):(1-5); The TiO 2 The mass / volume ratio of the precursor to the mixed solvent is 1:(1-20); Weigh a certain amount of surfactant, structure directing agent, and organic carbon source and dissolve them in a mixed solution of deionized water and ethanol to obtain a mixed solution B; The volume ratio of deionized water to ethanol in the mixed solution is (1-10):(1-10); TiO 2 The mass ratio of the precursor to the surfactant, the structure directing agent, and the organic carbon source is (1-5):(1-3):(1-3):(1-5); The mass / volume ratio of the mixed solution of the surfactant, water and ethanol is 1:(1-20); Weigh a certain mass of M x Cl y The solid salt is dissolved in deionized water and stirred until completely dissolved to obtain a mixed solution C; The M x Cl y Solid salt is CuCl 2 ·2H 2 O、MnCl 2 ·4H 2 O、NiCl 2 6H 2 O、ZnCl 2 、CoCl 2 6H 2 O、MoCl 5 Two of them and NaCl, MgCl 2 6H 2 O, CaCl 2 ·2H 2 O, KCl, or a mixture of The M x Cl y The mass / volume ratio of solid salt to deionized water is 1:(1-30); The M x Cl y Solid salt M atoms and TiO 2 The precursor Ti atom molar ratio is (1-3):(1-10); 2) Pour the mixed solution B and the mixed solution C into the mixed solution A, then add a certain amount of polyvinyl pyrrolidone and stir evenly, then add alkali solution to adjust the pH to 10-14, then place it in a sealed environment at a constant temperature of 50-80° C. for 30-60 minutes of ultrasonic treatment, age it at room temperature for 12-24 hours, and finally transfer it to a stainless steel reactor with a polytetrafluoroethylene liner, and perform a constant temperature crystallization reaction at 120-220° C. for 24-48 hours; 3) After the crystallization reaction is completed, filter to obtain a solid product, repeatedly wash with deionized water and centrifuge until the pH value is 7±0.5, put the obtained solid into a vacuum drying oven, and dry it at a vacuum constant temperature of 50-100° C. for 10-20 hours; crush the dried solid into a crucible, put it into a muffle furnace and heat it to 450-550° C. at a heating rate of 2-4° C. / min, then calcine at a constant temperature for 4-16 hours, and naturally cool it to room temperature to obtain an ordered multi-level porous composite adsorbent.
2. The preparation method according to claim 1, Its characteristics are: The TiO 2 The precursor is one of tetrabutyl titanate, isopropyl titanate, titanium tetrachloride, ethoxytitanium, and methyl orthotitanate, preferably tetrabutyl titanate.
3. The preparation method according to claim 1, Its characteristics are: The Al 2 O 3 The precursor is one of aluminum nitrate nonahydrate, ammonium aluminum carbonate, aluminum trichloride, aluminum isopropoxide, and aluminum carbonate, preferably aluminum isopropoxide.
4. The preparation method according to claim 1, Its characteristics are: The strong organic base is one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide, preferably tetrapropylammonium hydroxide.
5. The preparation method according to claim 1, Its characteristics are: The surfactant is tetrapropylammonium bromide, PEG-2000, P123, hexadecyltrimethylammonium bromide, triethylbenzylammonium chloride, preferably PEG-2000.
6. The preparation method according to claim 1, Its characteristics are: The structure directing agent is one of decaamine, dodecylamine, tetradecylamine and hexadecylamine, preferably dodecylamine.
7. The preparation method according to claim 1, Its characteristics are: The organic carbon source is one of starch, glucose, sucrose and fructose, preferably glucose.
8. The preparation method according to claim 1, Its characteristics are: The M x Cl y Solid salt is CuCl 2 ·2H 2 O、NiCl 2 6H 2 O, CaCl 2 ·2H 2 O is a mixture of three components, wherein the molar ratio of Cu, Ni and Ca is: (1-5): (1-10): (1-5); more preferably, the molar ratio of Cu, Ni and Ca is: (1~2):(3~7):(1~3)。 9. The preparation method according to claim 1, Its characteristics are: Polyvinyl pyrrolidone and TiO 2 The mass ratio of the precursors is 1:(1-10); more preferably, the mass ratio is 1:(1-6).
10. The preparation method according to claim 1, Its characteristics are: The alkali solution is one of 10-15% sodium hydroxide solution, 10-15% potassium hydroxide solution, and 10-15% ammonia water, preferably 10-15% ammonia water.
11. The preparation method according to claim 1, Its characteristics are: The crystallization reaction conditions are preferably a constant temperature of 150-200° C. for 24-30 hours.
12. The preparation method according to claim 1, Its characteristics are: The calcination conditions are preferably a constant temperature of 480-520° C. for 6-10 hours.
Citation Information
Cited By
Fluorination pretreatment assisted cobalt-lanthanum bimetal gradient loaded 10X molecular sieve adsorbent and preparation method thereof
CN121695819A