Modified charcoal loaded attapulgite material as well as preparation method and application thereof
By modifying biochar to support attapulgite material, iron ions are used to activate PMS to generate sulfate radicals, which solves the problems of excessive catalyst and high cost in the existing technology of biochar material in activating PMS to degrade antibiotics, and achieves efficient and low-cost antibiotic degradation effect.
Patent Information
- Application Number
- CN202411398706.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-29
AI Technical Summary
In existing technologies, biochar materials have problems such as excessive catalyst materials, easy generation of secondary pollution and high treatment costs when activating potassium persulfate PMS to degrade antibiotics, which limit their widespread application in the field of advanced oxidation technology.
Iron-modified biochar was introduced to support attapulgite material. By providing electrons through transition metal ions, sulfate radicals were generated, which improved the specific surface area and active sites of the biochar material. The preparation process was carried out by low-temperature calcination, which simplified the preparation steps and reduced energy demand.
It achieves highly efficient catalytic degradation of antibiotics, improves the adsorption capacity and degradation rate of biochar materials, reduces preparation costs, and requires no additional energy to activate PMS, making the material environmentally friendly and readily available.
Smart Images

Figure CN119034683A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental functional materials and biomass resource utilization, and specifically relates to a modified biochar-loaded attapulgite material and a preparation method and application thereof. Background Art
[0002] Antibiotics are widely used in medicine, agriculture, animal husbandry and aquaculture due to their excellent bactericidal properties. However, due to improper use, antibiotics are discharged into water bodies in large quantities, posing a threat to the ecological environment and human health.
[0003] At present, the main methods for removing antibiotics include adsorption, photocatalysis, Fenton-like reaction and biodegradation. The adsorption method can only enrich antibiotics but cannot achieve degradation; the photocatalytic process has high energy consumption and is not easy to apply on a large scale; the biodegradation treatment is affected by environmental factors and has low efficiency; the traditional Fenton method needs to be carried out under acidic conditions, which limits its industrial application.
[0004] In contrast, persulfate-activated advanced oxidation technology effectively overcomes the above shortcomings and has gradually become an important method for removing antibiotics.
[0005] CN114653332B discloses a method for degrading antibiotics in water bodies by using pyrite-modified biochar, wherein the method uses pyrite-modified biochar as a catalyst, catalyzes hydrogen peroxide to degrade antibiotics in water bodies, wherein pyrite-modified biochar is prepared by calcining biochar and pyrite as raw materials, and can be used for the removal of ciprofloxacin. However, the catalyst material required for activating potassium persulfate PMS to degrade antibiotics is too much, which is prone to secondary pollution to water bodies, and there are problems such as easy ion precipitation and high processing cost, which limits its wide application in the field of advanced oxidation technology. It can be seen that the biochar used in this method is not fully suitable for activating PMS to degrade antibiotics.
[0006] Therefore, it is of great significance to study materials with the advantages of high efficiency, low cost, and environmental friendliness to activate potassium persulfate PMS to degrade antibiotics. Summary of the invention
[0007] Purpose of the invention: The purpose of the present invention is to address the deficiencies in the prior art and provide a modified biochar-loaded attapulgite material and a preparation method and application thereof, especially in the application of activating PMS to degrade antibiotics.
[0008] The present invention introduces iron ions to activate PMS. Transition metal ions provide electrons to generate sulfate free radicals (SO4 -·); The material prepared by the present invention can effectively catalyze the degradation of antibiotics, and no additional energy is required to activate PMS during the activation process. In addition, the introduction of attapulgite increases the specific surface area of the biochar material, thereby exposing more active sites of the biochar material to achieve a higher removal efficiency.
[0009] Technical solution: The purpose of the present invention is achieved through the following technical solution:
[0010] The present invention provides a method for preparing a modified biochar-loaded attapulgite material, comprising the following steps:
[0011] (1) adding rice straw to a KOH solution, heating and stirring, washing with water and ethanol, centrifuging, drying and grinding to obtain alkalized straw;
[0012] (2) adding the attapulgite powder and the alkalized straw obtained in step (1) to a FeCl3 solution, ultrasonically shaking and heating and stirring to obtain a precursor mother liquor; washing with water and ethanol, centrifuging the mixed sample, drying the precipitate, grinding and sieving after drying to obtain a precursor;
[0013] (3) taking the precursor prepared in step (2), heating it in an inert atmosphere, calcining and carbonizing it, cooling it to room temperature, grinding and sieving it, and obtaining the modified biochar-loaded attapulgite material.
[0014] The rice straw used in the present invention is washed with water before use.
[0015] Preferably, in step (1), the concentration of the KOH solution is 8%-12%.
[0016] Further preferably, the concentration of the KOH solution is 10%.
[0017] Preferably, in step (1), 15 g of rice straw is added to every 300 ml of KOH solution.
[0018] Preferably, in step (1), the heating and stirring temperature is 65-75°C, and the heating and stirring time is 5-7h; the drying temperature is 65-75°C, and the time is 22-26h.
[0019] More preferably, the heating and stirring is carried out at a temperature of 70° C. for 6 hours; and the drying is carried out at a temperature of 70° C. for 24 hours.
[0020] Preferably, in step (1), the centrifugal speed is 4000-8000 rpm, and the centrifugal time is 3-8 min.
[0021] Furthermore, the centrifugal speed is 6000 rpm and the centrifugal time is 5 min.
[0022] Preferably, in step (2), the concentration of the FeCl3 solution is 6-15 g FeCl3·6H2O per 300 mL H2O.
[0023] Preferably, in step (2), the amount of FeCl3 added is calculated as FeCl3·6H2O, and the mass ratio of FeCl3, attapulgite powder and alkalized straw is 6-15:3-6:9.
[0024] Further preferably, the mass ratio of the FeCl3, attapulgite powder and alkalized straw is 10.5:4.5:9.
[0025] Preferably, in step (2), the ultrasonic oscillation time is 0.5-1.5 h; the heating and stirring temperature is 65-75° C., and the time is 5-7 h; the drying temperature is 70-80° C., and the time is 22-26 h.
[0026] Further preferably, the ultrasonic oscillation time is 1 hour; the heating stirring temperature is 70° C. and the time is 6 hours; the drying temperature is 75° C. and the time is 24 hours.
[0027] Preferably, in step (2), the centrifugal speed is 4000-8000 rpm, and the centrifugal time is 3-8 min.
[0028] Furthermore, the centrifugal speed is 6000 rpm and the centrifugal time is 5 min.
[0029] Preferably, in step (3), the inert atmosphere is a nitrogen atmosphere.
[0030] Preferably, in step (3), the heating rate is 4-6°C / min, the calcination temperature is 250-350°C, and the calcination time is 1.5-2.5h.
[0031] Furthermore, the heating rate is 5°C / min, the calcination temperature is 300°C, and the calcination time is 2h.
[0032] The present invention also provides a modified biochar-loaded attapulgite material prepared by the preparation method.
[0033] The present invention also provides an application of the modified biochar-loaded attapulgite material in the adsorption and degradation of antibiotics, for example, for the adsorption and degradation of tetracycline hydrochloride.
[0034] Beneficial effects:
[0035] (1) The raw materials of the modified biochar material prepared by the present invention are low-cost, easy to obtain, pollution-free, can be prepared on a large scale, and have controllable structure and performance; the preparation steps are simple and convenient, and the energy required for low-temperature calcination is less, which has broad application prospects.
[0036] (2) The modified biochar material prepared by the present invention has both an adsorption function and a function as a catalyst to catalyze the degradation of antibiotics by PMS.
[0037] (3) Compared with the unmodified biochar material, the modified biochar material of the present invention effectively increases the specific surface area of the biochar material and provides sufficient active sites. According to the test results, when the sample attapulgite biochar material BC@ATP-1 of the present invention is used as an adsorbent, the maximum adsorption capacity is 264.41 mg / L, and when it is used as a PMS catalyst to degrade antibiotics, the degradation rate reaches 90.3% in 140 min; when BC@ATP-2 is used as an adsorbent, the maximum adsorption capacity is 252.44 mg / L, and when it is used as a PMS catalyst to degrade antibiotics, the degradation rate reaches 88.9% in 140 min; when BC@ATP-3 is used as an adsorbent, the maximum adsorption capacity is 244.09 mg / L, and when it is used as a PMS catalyst to degrade antibiotics, the degradation rate reaches 83.6% in 140 min. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 TEM image, EDS mapping image and SEM image of the modified biochar-loaded attapulgite material prepared in Example 1;
[0039] Figure 2 FTIR spectra of samples prepared in Example 1 and Comparative Example 1;
[0040] Figure 3 The XPS spectra of the samples prepared in Example 1 and Comparative Example 1;
[0041] Figure 4 XRD patterns of samples prepared in Example 1 and Comparative Example 1;
[0042] Figure 5 The adsorption isotherms of tetracycline hydrochloride for the samples prepared in Examples 1-3 and Comparative Example 1 are shown;
[0043] Figure 6 The degradation kinetics of tetracycline hydrochloride by the samples prepared in Examples 1-3 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is described in detail below through specific embodiments, but the protection scope of the present invention is not limited to the embodiments.
[0045] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are commercially available products unless otherwise specified.
[0046] Tetracycline hydrochloride (purity 96%) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0047] Rice straw was obtained from Su Rui Agricultural Products.
[0048] Example 1 Preparation of modified biochar-loaded attapulgite material
[0049] (1) Add 15 g of rice straw to 300 ml of 10% potassium hydroxide solution, heat and stir at 70° C. for 6 h, wash with deionized water and ethanol alternately, centrifuge at 6000 rpm for 5 min, three times each, dry in a vacuum oven at 70° C. for 24 h, and grind to obtain alkalized straw;
[0050] (2) 10.5 g of FeCl3·6H2O was added to 300 mL of H2O, and then 4.5 g of attapulgite powder and 9 g of alkalized straw were added, and the mixture was shaken by an ultrasonic oscillator for 1 h, heated and stirred at 70°C for 6 h, washed alternately with deionized water and ethanol, centrifuged at 6000 rpm for 5 min, 3 times each, placed in a vacuum drying oven, dried at 75°C for 24 h, and ground to obtain a precursor after drying;
[0051] (3) Weigh 1 g of the precursor prepared above, put it into a tubular furnace, pass nitrogen for 10 min to drive out oxygen, heat it to 300 °C at a heating rate of 5 °C / min, calcine and carbonize it at 300 °C in a nitrogen atmosphere for 2 h, cool it to room temperature after carbonization, grind it, and pass it through a 100-mesh sieve. The modified biochar-loaded attapulgite material obtained is named BC@ATP-1.
[0052] Figure 1 TEM images, EDS mapping and SEM images of modified biochar loaded attapulgite materials. Scanning electron microscopy shows that BC@ATP-1 has a macroporous structure, retains part of the original structure of biomass waste, has a fibrous structure, the surface of the composite material is rough, and iron oxides are distributed in the pores and surface of biochar.
[0053] Example 2 Preparation of modified biochar-loaded attapulgite material
[0054] (1) Add 15 g of rice straw to 300 ml of 12% potassium hydroxide solution, heat and stir at 75° C. for 5 h, wash with deionized water and ethanol alternately, centrifuge at 4000 rpm for 8 min, 3 times each, dry at 75° C. for 22 h in a vacuum oven, and grind to obtain alkalized straw;
[0055] (2) 6 g of FeCl3·6H2O was added to 300 mL of H2O, and then 3 g of attapulgite powder and 9 g of alkalized straw were added, and the mixture was shaken by an ultrasonic oscillator for 0.5 h, heated and stirred at 65 °C for 7 h, washed alternately with deionized water and ethanol, centrifuged at 8000 rpm for 3 min, 3 times each, placed in a vacuum drying oven, dried at 80 °C for 22 h, and ground to obtain a precursor;
[0056] (3) Weigh 1 g of the precursor prepared above, put it into a tubular furnace, pass nitrogen for 10 min to drive out oxygen, then heat it to 250 °C at a heating rate of 6 °C / min, calcine and carbonize it at 250 °C in a nitrogen atmosphere for 2.5 h, cool it to room temperature after carbonization, grind it, and pass it through a 100-mesh sieve. The modified biochar-loaded attapulgite material obtained is named BC@ATP-2.
[0057] Example 3 Preparation of modified biochar-loaded attapulgite material
[0058] (1) Add 15 g of rice straw to 300 ml of 8% potassium hydroxide solution, heat and stir at 65° C. for 7 h, wash with deionized water and ethanol alternately, centrifuge at 8000 rpm for 3 min, 3 times each, dry at 65° C. for 26 h in a vacuum oven, and grind to obtain alkalized straw;
[0059] (2) 15 g of FeCl3·6H2O was added to 300 mL of H2O, and then 6 g of attapulgite powder and 9 g of alkalized straw were added, and the mixture was shaken by an ultrasonic oscillator for 1.5 h, heated and stirred at 75 °C for 5 h, washed alternately with deionized water and ethanol, centrifuged at 4000 rpm for 8 min, 3 times each, placed in a vacuum drying oven, dried at 70 °C for 26 h, and ground to obtain a precursor;
[0060] (3) Weigh 1 g of the precursor prepared above, put it into a tubular furnace, pass nitrogen for 10 min to drive out oxygen, then heat it to 350 °C at a heating rate of 4 °C / min, calcine and carbonize it at 350 °C in a nitrogen atmosphere for 1.5 h, cool it to room temperature after carbonization, grind it, and pass it through a 100-mesh sieve. The modified biochar-loaded attapulgite material obtained is named BC@ATP-3.
[0061] Comparative Example 1
[0062] Weigh 1 g of rice straw, grind it to get straw powder, put it into a tubular furnace, pass nitrogen for 10 minutes to drive out oxygen, heat it to 300°C at a heating rate of 5°C / min, carbonize it at 300°C in a nitrogen atmosphere for 2 hours, cool it to room temperature after carbonization, grind it, and pass it through a 100-mesh sieve. The obtained biochar material is named BC.
[0063] Figure 2 The FTIR spectra of the samples prepared in Example 1 and Comparative Example 1 are shown in Table 1. The FTIR spectra show that 3347.86 cm-1 The corresponding broad and strong peaks belong to the OH stretching vibration peaks of cellulose and hemicellulose in rice straw, while the 1700.00 cm -1 The peak nearby is the C=O stretching vibration peak. 1655.11cm -1 The peaks near 1415.10 cm are due to C=C stretching caused by the presence of aromatic rings or benzene rings in lignin. -1 The nearby peak is COC, with a peak at 1029.89 cm -1 The characteristic peaks of 796.57 cm correspond to the aromatic CO stretching vibration peaks, which are attributed to the thermal decomposition of cellulose and the exposure of the residual aromatic core in the lignin residue. -1 The vibrations corresponding to the peaks near 692.80cm are strong -OH-induced bending and are important for the formation of goethite. -1 The characteristic peaks at belong to Fe-O, and these oxygen-containing functional groups can serve as the main active adsorption sites. The Fe-O band confirms the successful combination of Fe and biochar.
[0064] Figure 3 The XPS graphs of the samples prepared in Example 1 and Comparative Example 1. As can be seen from the figure, the C, O and Fe elements present in BC@ATP-1 correspond to the peak values of 283eV, 532eV and 706eV. Compared with Comparative Example 1, the ratio of C and O on the surface of the mixture is reduced, and Fe is newly added, indicating that a large amount of iron is successfully loaded on the surface of the biochar. The iron ions are introduced to activate the PMS process, and the transition metal ions provide electrons to generate sulfate radicals (SO4 - ·), used in the process of activating PMS.
[0065] Figure 4 The XRD patterns of the samples prepared in Example 1 and Comparative Example 1 are shown in the figure. As can be seen from the figure, BC@ATP has a diffraction peak at 2θ=20.84°, which is attributed to the SiO2(100) crystal plane; the diffraction peak at 2θ=26.62° corresponds to the limonite (α-FeOOH) (021) crystal plane; the diffraction peaks at 2θ=40.46° and 50.12° are hematite (α-Fe2O3) (113) crystal plane and (024) crystal plane. The diffraction peak at 2θ=30.15° is Fe3O4. BC has a characteristic diffraction peak of amorphous carbon at 18° to 30°, which confirms that the biomass has been carbonized.
[0066] This indicates that complex chemical changes occurred during the preparation of BC@ATP.
[0067] The method for investigating the adsorption performance of simulated pollutants provided by the present invention is as follows:
[0068] Adsorption test:
[0069] Tetracycline hydrochloride solutions with concentrations of 40, 50, 60, 70, 80, and 100 mg / L were prepared with deionized water. In each test, 100 mL of tetracycline hydrochloride solution was measured and placed in a 250 mL conical flask, 20 mg of the sample prepared in the above embodiment or comparative example was mixed, and placed in a constant temperature shock box at 25 ° C, 180 rpm and shaken for 48 h. In order to obtain adsorption isotherm data, 1 mL of solution was taken out after 48 h, and immediately filtered with a 0.45 um filter membrane after taking out, and then the tetracycline hydrochloride concentration was measured with an ultraviolet spectrophotometer. All experiments were carried out in parallel 3 times, and blank controls were performed simultaneously.
[0070] When performing concentration measurements using a UV spectrophotometer, the Beer-Lambert law is applied to calculate the concentration of the sample.
[0071] The Beer-Lambert law formula is as follows:
[0072] A=ε·C·l
[0073] in,
[0074] A: absorbance (dimensionless)
[0075] ε: Molar absorptivity (L·mol-1·cm-1), which indicates the absorptivity of a solute at a specific wavelength
[0076] C: concentration (mol / L or g / L), concentration of solute
[0077] l: Optical path length (cm), usually the thickness of the cuvette.
[0078] The Freundlich adsorption isotherm model describes multi-molecular layer adsorption. The main mechanism is that the non-uniform adsorbent surface forms adsorption active sites with different energies, thereby increasing the adsorption capacity of the adsorbent.
[0079] The Langmuir adsorption isotherm model describes monolayer adsorption, and its main assumption is that the adsorbent surface is smooth and there is no interaction between adsorbate molecules.
[0080] Figure 5 The adsorption isotherms of tetracycline hydrochloride prepared by the samples of Examples 1-3 and Comparative Example 1 are shown, wherein Qe represents the unit adsorption amount. The equilibrium adsorption amount Qe of Examples 1-3 and Comparative Example 1 increases with the increase of Ce, and the correlation coefficients of the two models are very close, involving both monolayer molecular adsorption and multilayer molecular adsorption.
[0081] Examples 1-3 are more consistent with the Freundlich adsorption isotherm model and are adsorbents with uneven surfaces. Figure 1The observed results are consistent; Comparative Example 1 is more consistent with the Langmuir adsorption isotherm model. According to the isotherm model fitting calculation, the maximum adsorption capacity of tetracycline hydrochloride in Example 1 is 264.41 mg / L, the maximum adsorption capacity of Example 2 is 252.44 mg / L, the maximum adsorption capacity of Example 3 is 244.09 mg / L, and the maximum adsorption capacity of Comparative Example 1 is 28.85 mg / L. It can be seen that the adsorption capacity after modification is greatly improved.
[0082] Degradation test:
[0083] Prepare a tetracycline hydrochloride solution with a concentration of 30 mg / L using deionized water. In each test, 100 mL of tetracycline hydrochloride solution was measured and placed in a 250 mL conical flask, PMS was added at a concentration of 0.5 mmol / L, 20 mg of the sample prepared in the above embodiment or comparative example was mixed, and placed in a constant temperature shaking box at 25°C and 180 rpm for 140 min. In order to obtain adsorption isotherm data, 1 mL of solution was taken out at the specified time period of 0-140 min, and immediately filtered with a 0.45 um filter membrane, and then the tetracycline hydrochloride concentration was determined using a UV spectrophotometer. All experiments were conducted in parallel 3 times, and blank controls were performed simultaneously. The experimental results are shown in Figure 6 .
[0084] Figure 6 The degradation kinetics of tetracycline hydrochloride by the samples prepared in Examples 1-3 and Comparative Example 1 are shown.
[0085] When BC@ATP-1 is used as a PMS catalyst to degrade antibiotics, the degradation rate reaches 90.3% in 140 minutes; when BC@ATP-2 is used as a PMS catalyst to degrade antibiotics, the degradation rate reaches 88.9% in 140 minutes; when BC@ATP-3 is used as a PMS catalyst to degrade antibiotics, the degradation rate reaches 83.6% in 140 minutes. The degradation efficiency of comparative example 1 for tetracycline hydrochloride is about 49.6%. It can be seen that compared with ordinary biochar, the activation effect of the modified BC@ATP is significantly improved.
[0086] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.
Claims
1. A method for preparing a modified biochar-loaded attapulgite material, characterized in that: The following steps are involved: (1) adding rice straw to a KOH solution, heating and stirring, washing with water and ethanol, centrifuging, drying and grinding to obtain alkalized straw; (2) adding the attapulgite powder and the alkalized straw obtained in step (1) to a FeCl3 solution, ultrasonically shaking and heating and stirring to obtain a precursor mother liquor; washing with water and ethanol, centrifuging the mixed sample, drying the precipitate, grinding and sieving after drying to obtain a precursor; (3) taking the precursor prepared in step (2), heating it in an inert atmosphere, calcining and carbonizing it, cooling it to room temperature, grinding and sieving it, and obtaining the modified biochar-loaded attapulgite material.
2. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the KOH solution is 8%-12%.
3. The preparation method according to claim 1, characterized in that: In step (1), 15 g of rice straw was added to every 300 ml of KOH solution.
4. The preparation method according to claim 1, characterized in that: In step (1), the heating and stirring temperature is 65-75°C, and the heating and stirring time is 5-7h; the drying temperature is 65-75°C, and the time is 22-26h.
5. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the FeCl3 solution is 6-15 g FeCl3·6H2O per 300 mL H2O.
6. The preparation method according to claim 1, characterized in that: In step (2), the amount of FeCl3 added is calculated as FeCl3·6H2O. 3、 The mass ratio of attapulgite powder to alkalized straw is 6-15:3-6:
9.
7. The preparation method according to claim 1, characterized in that: In step (2), the ultrasonic oscillation time is 0.5-1.5h; the heating and stirring temperature is 65-75°C, and the time is 5-7h; the drying temperature is 70-80°C, and the time is 22-26h.
8. The preparation method according to claim 1, characterized in that: In step (3), the heating rate is 4-6°C / min, the calcination temperature is 250-350°C, and the calcination time is 1.5-2.5h.
9. A modified biochar-loaded attapulgite material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the modified biochar-loaded attapulgite material according to claim 9 in the adsorption and degradation of antibiotics.
Citation Information
Cited By
Solid material with catalytic oxidation and adsorption functions and preparation method thereof
CN116870911A
Method for synergistically improving soil carbon sequestration yield and efficiency by using modified carbon material
CN120153800A