Catalyst for selectively preparing octanal as well as preparation method and application of catalyst
Through rotary strengthening technology, rotary filler beds and wire mesh fillers are used to improve the dispersion and uniform adsorption of active components, solving the problems of selective preparation of octenaldehyde and high energy consumption, and achieving high efficiency Catalyst preparation and octanaldehyde conversion.
Patent Information
- Application Number
- CN202310601243.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, it is difficult to selectively prepare octanaldehyde in the hydrogenation reaction of octenal, and the noble metal catalyst is costly and the energy consumption of gas phase is large, resulting in low overall efficiency of the catalyst.
Using rotary strengthening technology, using rotary filler beds, wire mesh or cylindrical fillers, liquid mist and droplets are formed under centrifugal force through the impregnation liquid, sprayed onto the surface of the carrier, and the dispersion and uniform adsorption of active components are improved, and the dispersion and uniform adsorption of active components are prepared. A catalyst with high dispersion of metal components and small average particle size.
The high selectivity and conversion rate of the catalyst are achieved, the impregnation time of the metal active components and the crushing risk of the carrier are reduced, the catalytic performance is improved, and it is suitable for industrial production.
Smart Images

Figure CN119034742A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysis, and more particularly to a catalyst for selectively preparing octanal, and a preparation method and application thereof. Background Art
[0002] Octanal is an intermediate product in the hydrogenation process of octenal. Since octenal is an α, β unsaturated aldehyde, it can selectively generate octanal or octenol under the action of different catalysts. Since both contain C=C double bonds or C=O double bonds, they can continue to react with hydrogen to finally generate octanol.
[0003] Octanal is an important chemical product. It is an important organic raw material or fragrance. It is widely present in plant essential oils and has potential antibacterial effects. This type of compound has many aroma types, with a pleasant sweet orange fragrance, a long lasting fragrance, and can increase the naturalness of the flavor. At the same time, octanal can be used as a citrus flavor in beverages and ice cream, and has a wide range of applications. However, octanal is easily oxidized to produce octanoic acid, which destroys the aroma and causes complete deterioration.
[0004] The industrial production of octanal is mainly obtained by the hydrogenation reaction of octenal. Octenal is an α,β-unsaturated aldehyde, which contains both C=C and C=O bonds in the molecule. The bond energy of C=C bond is 615kJ / mol, and the bond energy of C=O bond is 715kJ / mol. Therefore, based on the data comparison of computational chemistry, it is generally believed that the C=C double bond is easier to hydrogenate than the C=O double bond. Octenal can be selectively obtained by hydrogenation with hydrogen once. If the reaction conditions are not accurately controlled, resulting in the residence time of octanal in the reaction process being too long, octanal will be hydrogenated again to produce octanol. Therefore, as an intermediate product of this reaction, octanal requires a catalyst with extremely high selectivity.
[0005] At present, most of the research focuses on the preparation of octanol by hydrogenation of octenal, but there are few reports on the selective preparation of octanal. Chinese invention patent CN107930647A discloses a catalyst for preparing octanal, which uses a noble metal active component Pd and at least one of Ag, Co, and Rh, and is loaded on Al2O3. However, the use of noble metal components will lead to excessively high overall catalyst costs. At the same time, the reaction is carried out under gas phase conditions. First, octenal must be heated to 180-220°C to make it completely gasified and then hydrogen is introduced, so the gas phase method consumes too much energy.
[0006] In summary, it is particularly necessary to develop an octenal hydrogenation catalyst with high conversion rate and good selectivity. Summary of the invention
[0007] In order to solve the technical problems existing in the prior art, the present invention provides a catalyst for selectively preparing octanal and a preparation method and application thereof.
[0008] The present invention utilizes the rotary strengthening technology, uses the rotary packed bed as the catalyst preparation equipment, and adopts the wire mesh or columnar packing. The impregnation liquid forms liquid mist and liquid droplets under the action of centrifugal force, and is sprayed on the surface of the carrier at a very high speed. The highly dispersed fine droplets, the extremely high initial velocity and the constantly updated phase interface can effectively improve the diffusion and penetration rate of the impregnation liquid in the pores of the carrier, promote the uniform adsorption of the active components on the surface of the carrier, greatly shorten the impregnation time, and finally, after drying and roasting, a catalyst with high dispersion of metal components and small average metal particle size is prepared.
[0009] One of the objects of the present invention is to provide a catalyst for selectively preparing octanal.
[0010] The catalyst for selectively preparing octanal comprises a carrier and an active metal component supported on the carrier; the active metal component is one of Cu, Co, and Ni, preferably Ni; the carrier is one of Al2O3, MgO, ZrO2, TiO2, and SiO2, preferably Al2O3;
[0011] Taking the total weight of the catalyst as 100%, the active metal component is 2-15wt%, and the carrier is 85-98wt%; preferably, the active metal component is 5-15wt%, and the carrier is 85-95wt%;
[0012] The catalyst is prepared by using a rotary enhanced impregnation device; the rotary enhanced impregnation device comprises a rotary enhanced packing bed, in which a carrier ring loaded with a carrier and a rotary packing are arranged, and the carrier ring is located outside the rotary packing; the carrier ring and the rotary packing can both rotate independently.
[0013] In a preferred embodiment of the present invention,
[0014] The precursor of the metal element in the active metal component is a soluble salt of the metal element, preferably at least one of the soluble salts of Cu, Co, and Ni, more preferably at least one of the nitrates, carbonates, and sulfates of Cu, Co, and Ni;
[0015] The specific surface area of the carrier is 100 to 300 m 2 / g, pore volume is 0.5~1.5cm 3 / g, preferably, the specific surface area of the carrier is 140 to 250 m 2 / g, pore volume is 0.7~1.2cm 3 / g.
[0016] In a preferred embodiment of the present invention,
[0017] The rotary enhanced impregnation device also includes a liquid storage tank and a liquid pump. The rotary enhanced packing bed is a cylindrical structure and also includes a liquid distributor. The liquid distributor is located at the center of the rotary enhanced packing bed. Rotating packing and carrier rings are sequentially arranged on the periphery of the liquid distributor. The liquid pump is connected to the liquid storage tank to allow the impregnation liquid in the liquid storage tank to enter the liquid distributor through the impregnation liquid inlet. An impregnation liquid outlet is arranged at the lower end of the rotary enhanced packing bed.
[0018] In a preferred embodiment of the present invention,
[0019] The rotary intensified impregnation device further comprises a motor, preferably two motors, which are used to drive the carrier ring to rotate and the filler to rotate respectively;
[0020] The rotating packing is at least one of a wire mesh and a columnar packing, preferably at least one of a stainless steel wire mesh packing and a stainless steel columnar packing;
[0021] The carrier ring is a wire mesh carrier ring.
[0022] like Figure 1 As shown, the rotary enhanced impregnation device used in the present invention includes a motor 1, a motor 2, a rotary enhanced packing bed, a liquid storage tank, and a liquid pump. The rotary enhanced packing bed is a cylindrical structure, including a rotary packing and a carrier ring. The liquid distributor is located at the center of the rotary enhanced packing bed. Rotating packing and carrier rings are sequentially arranged on the periphery of the liquid distributor. The liquid pump allows the impregnation liquid in the liquid storage tank to enter the liquid distributor through the impregnation liquid inlet. An impregnation liquid outlet is arranged at the lower end of the rotary enhanced packing bed. The carrier ring is a wire mesh carrier ring. A certain amount of carrier particles are filled in the carrier ring according to actual needs. The rotary enhanced packing bed is provided with a liquid outlet at the lower end for discharging the liquid that has not been impregnated and returning it to the liquid storage tank. Among them, the carrier ring rotates at a low speed driven by motor 1, and the rotating filler rotates at a high speed driven by motor 2. The impregnation liquid is pumped into the impregnation device by a liquid pump, and is evenly sprayed into the inner side of the rotating filler through a liquid distributor. Under the action of centrifugal force, the mixed salt solution is sheared into tiny liquid elements by the rotating filler, and contacts with the alumina carrier in the carrier ring rotating at a low speed. The carrier is not filled in the carrier ring, and there will be a certain space to facilitate the rotation of the carrier. In this way, the solution can be impregnated at all angles of the carrier, so that the impregnation liquid can be evenly distributed on the carrier, and the catalyst precursor is obtained after a period of intensive impregnation.
[0023] The second object of the present invention is to provide a method for preparing a catalyst for selectively preparing octanal, comprising the following steps:
[0024] (1) In the rotating enhanced impregnation device, the carrier is loaded into a rotatable carrier ring, and the soluble salt solution of the metal element is used as an impregnation liquid and sprayed into the inner side of the rotating filler. Under the action of centrifugal force, the impregnation liquid is sprayed on the rotating carrier to enhance the impregnation, and then a catalyst precursor is obtained, and then after drying and calcination, the catalyst is obtained;
[0025] Optionally, (2) repeat step (1).
[0026] During the rotary enhanced impregnation process, a soluble salt solution of metal elements is pumped into the rotary enhanced impregnation device and evenly sprayed into the inner side of the rotating filler through a liquid distributor. Under the action of centrifugal force, the salt solution is sheared into tiny liquid elements by the rotating filler, which come into contact with the carrier in the slow-rotating carrier ring, and the catalyst precursor is obtained by enhanced impregnation. The enhanced impregnation steps can be repeated, and the carrier can be subjected to multiple enhanced impregnations.
[0027] The preferred specific preparation steps are as follows:
[0028] (1) Impregnation step: After the carrier is treated, it is loaded into a wire mesh carrier ring. The impregnation liquid containing metal salts enters the rotary enhanced impregnation device through a pump and is evenly sprayed onto the inner edge of the rotating filler through a liquid distributor. Under the action of high-speed centrifugal force, the impregnation liquid is sheared into tiny liquid micro-elements by the rotating filler and contacts the carrier in the carrier ring at an extremely high tangential initial velocity. The carrier ring rotates at a low speed to ensure that the carrier is fully in contact with the impregnation liquid micro-elements. The impregnated liquid returns to the liquid storage tank for liquid circulation, and after a certain impregnation time, a catalyst precursor is obtained.
[0029] (2) Drying and calcining step: drying and calcining the catalyst precursor for decomposition;
[0030] (3) Steps (1) and (2) are optionally repeated according to the actual metal content requirement in the catalyst until the final catalyst is obtained.
[0031] In a preferred embodiment of the present invention,
[0032] The mass concentration of the soluble salt solution of the metal element is 5-35%, and the solvent is water, preferably deionized water;
[0033] The soluble salt solution of the metal element is sprayed into the inner side of the rotating filler through a liquid distributor, and the liquid inlet flow rate of the liquid distributor is 1 to 50 ml / min, preferably 5 to 10 ml / min.
[0034] In a preferred embodiment of the present invention,
[0035] The rotating speed of the rotating filler is 1000-2000 rpm;
[0036] The rotation speed of the carrier ring is 10 to 20 rpm;
[0037] The rotating packing and the carrier ring can rotate in the same direction or in opposite directions, as long as the rotating packing rotates at a high speed and the carrier ring rotates at a low speed.
[0038] The time of the enhanced impregnation is 10 to 30 minutes;
[0039] The drying conditions are: drying at 100-120°C for 2-10 hours; preferably drying at 110-120°C for 2-8 hours;
[0040] The calcination conditions are 300-600° C. for 2-10 h, preferably 350-550° C. for 3-6 h.
[0041] The third object of the present invention is to provide a catalyst for selectively preparing octanal obtained by the above method.
[0042] The catalyst obtained by the preparation method provided by the present invention is subjected to reduction treatment to partially reduce the oxide to active metal, thereby obtaining a catalyst with high metal component dispersion and small average particle size, for example, the metal dispersion is 0.5-5% and the metal particle size is 10-100nm.
[0043] A fourth object of the present invention is to provide an application of a catalyst in the selective preparation of octanal. Preferably, octenal and hydrogen are used as raw materials, and the octanal is prepared by reacting in a solvent under the action of the catalyst.
[0044] In a preferred embodiment of the present invention,
[0045] Reaction temperature 60~100℃;
[0046] Reaction pressure 1~3MPa;
[0047] Reaction space velocity 1~3h -1 ;
[0048] The solvent is an alcohol solvent, preferably a monohydric alcohol having 2 to 8 carbon atoms, more preferably ethanol or octanol;
[0049] The mass ratio of the octenal to the solvent is 1:(2-6).
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] The rotating packed bed of the present invention is a chemical intensification device that can highly intensify microscopic mixing and mass transfer. In a hypergravity environment, the huge shear force generated by the rotation of the rotating packing can shear the fluid into very small liquid microelements, increase the contact area of the physical phases, greatly improve the mixing and mass transfer effects between the phases, and increase the mass transfer coefficient by 10 to 1000 times compared with conventional reactors. Therefore, the use of the rotating intensified impregnation method of the present invention can improve the dispersion of catalytic active components and improve catalytic performance.
[0052] The present invention utilizes the rotary strengthening technology, uses the rotary packed bed as the catalyst preparation equipment, and adopts the wire mesh or columnar packing. The impregnation liquid forms liquid mist and liquid droplets under the action of centrifugal force, and is sprayed on the surface of the carrier at a very high speed. The highly dispersed fine droplets, the extremely high initial velocity and the constantly updated phase interface can effectively improve the diffusion and penetration rate of the impregnation liquid in the pores of the carrier, promote the uniform adsorption of the active components on the surface of the carrier, greatly shorten the impregnation time, and finally, after drying and roasting, a catalyst with high dispersion of metal components and small average metal particle size is prepared.
[0053] The preparation method provided by the present invention greatly shortens the impregnation time of the metal active component, and the metal active component can be more evenly adsorbed on the surface of the carrier; at the same time, the carrier ring is equipped with a wire mesh, which can wrap the carrier to prevent the carrier from being damaged;
[0054] The catalyst prepared by the preparation method of the present invention has higher dispersion and smaller particle size;
[0055] The catalyst prepared by the present invention has a low content of metal active components and is suitable for use as a catalyst for selectively preparing octanal.
[0056] The preparation method provided by the invention effectively avoids the breakage of the carrier, has a simple process, is easy to realize industrial production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 It is a schematic diagram of the rotary enhanced impregnation equipment;
[0058] In the figure: 1-1 is motor 1, 1-2 is motor 2, 1-3 is a rotating reinforced packing bed, 1-4 is a liquid storage tank, 1-5 is a liquid pump, 1-6 is a liquid distributor, 1-7 is a rotating packing, 1-8 is a wire mesh carrier ring, 1-9 is an alumina carrier, 1-10 is an impregnation liquid inlet, and 1-11 is an impregnation liquid outlet;
[0059] Figure 2 It is a side view schematic diagram of the internal structure of the rotary enhanced impregnation equipment;
[0060] In the figure: 1-12 is the wire mesh carrier ring gear, 1-3 is the rotating reinforced filler bed, 1-8 is the wire mesh carrier ring, 1-9 is the alumina carrier, 1-7 is the rotating filler, 1-6 is the liquid distributor, and 1-11 is the impregnation liquid outlet. DETAILED DESCRIPTION
[0061] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.
[0062] The test instruments and test conditions used in the examples are as follows:
[0063] The specific surface area (BET) and pore volume of the catalyst were measured by N2 adsorption-desorption method.
[0064] The dispersion and average particle size of the active components in the catalyst were measured by hydrogen chemisorption.
[0065] The sources of raw materials used in the examples are as follows:
[0066] All reagents used were commercially available and of analytical grade.
[0067] The rotary impregnation device used in the embodiment is as follows Figure 1 As shown in, it includes: a motor 1 (1-1), a motor 2 (1-2), a rotating reinforced packing bed 1-3, a liquid storage tank 1-4, and a liquid pump 1-5. The rotating reinforced packing bed 1-3 is a cylindrical structure, including a liquid distributor 1-6, a rotating packing 1-7 and a wire mesh carrier ring 1-8. The center of the rotating reinforced packing bed 1-3 is the liquid distributor 1-6, wherein one end of the liquid distributor 1-6 is closed, and the other end is provided with a pipeline opening 1-10 connected to the liquid pump 1-5 through a pipeline. Rotating packing 1-7 and a wire mesh carrier ring 1-8 are sequentially arranged on the periphery of the liquid distributor 1-6. The lower end of the rotating reinforced packing bed 1-3 is provided with a liquid outlet 1-11 for discharging the liquid that has not been impregnated and returning it to the liquid storage tank 1-4. Among them, the wire mesh carrier ring 1-8 is filled with alumina carrier 1-9, and the rotating filler 1-7 adopts stainless steel wire mesh filler. The motor 1 drives the carrier ring 1-8 to rotate at a low speed, and the motor 2 drives the rotating filler 1-7 to rotate at a high speed. The impregnation liquid is pumped into the impregnation device by the liquid pump 1-5, and is evenly sprayed into the inner side of the rotating filler 1-7 through the liquid distributor 1-6. Under the action of centrifugal force, the impregnation liquid is sheared into tiny liquid elements by the rotating filler 1-7, and contacts with the alumina carrier 1-9 in the slow-rotating carrier ring 1-8. After a period of intensive impregnation, a catalyst precursor is obtained.
[0068] Figure 2 It is a side view of the internal structure of the rotary intensified impregnation equipment, where 1-12 is the wire mesh carrier ring gear, and the other parts are the same as Figure 1 The names are the same as those in the annotations.
[0069] Example 1
[0070] Using the rotary enhanced impregnation method, 50g of the shaped Al2O3 carrier (BET specific surface area of 214m 2 / g, pore volume is 0.97cm 3 / g) is loaded into a wire mesh carrier ring, an impregnation solution containing nickel nitrate (mass concentration is 20%) is placed in a liquid tank, the rotating packed bed is started, the speed of the packed bed is 1500rpm, the speed of the carrier ring is 10rpm, the impregnation solution is pumped into the rotating bed through a horizontal flow pump, the liquid inlet flow rate of the liquid distributor is 10ml / min, after 20min of intensive impregnation, the catalyst precursor is taken out, and then dried at 110°C for 7h and calcined at 450°C for 3h, finally, a catalyst with a Ni content of 10wt% and an Al2O3 carrier content of 90wt% is obtained.
[0071] Example 2
[0072] Using the rotary impregnation method, 50 g of the shaped ZrO2 carrier (BET specific surface area of 187 m 2 / g, pore volume is 1.05cm 3 / g) is loaded into a wire mesh carrier ring, an impregnation solution containing copper nitrate (mass concentration is 30%) is placed in a liquid tank, the rotating packed bed is started, the speed of the packed bed is 2000rpm, the speed of the carrier ring is 15rpm, the impregnation solution is pumped into the rotating bed through a horizontal flow pump, the liquid inlet flow rate of the liquid distributor is 8ml / min, after 30min of intensive impregnation, the catalyst precursor is taken out, and then dried at 120°C for 8h and calcined at 550°C for 4h, finally a catalyst with a Cu content of 5wt% and a ZrO2 carrier content of 95wt% is obtained.
[0073] Example 3
[0074] Using the rotary enhanced impregnation method, 50g of the shaped SiO2 carrier (BET specific surface area of 167m 2 / g, pore volume is 0.95cm 3 / g) is loaded into a wire mesh carrier ring, an impregnation solution containing cobalt nitrate (mass concentration is 10%) is placed in a liquid tank, the rotating packed bed is started, the speed of the packed bed is 2000rpm, the speed of the carrier ring is 15rpm, the impregnation solution is pumped into the rotating bed through a horizontal flow pump, the liquid inlet flow rate of the liquid distributor is 5ml / min, after 15min of intensive impregnation, the catalyst precursor is taken out, and then dried at 120°C for 2h and calcined at 350°C for 6h, finally a catalyst with a Co content of 15wt% and a SiO2 carrier content of 85wt% is obtained.
[0075] Example 4
[0076] 10 ml of the catalyst obtained in Example 1 was loaded into a stainless steel fixed bed reactor, and high-purity N2 was introduced at a flow rate of 300 mL / min. The temperature was raised to 120°C, and the high-purity N2 was switched to H2 at a flow rate of 200 mL / min. The temperature was raised to 400-450°C and maintained for 4 h to reduce the catalyst, and then the temperature was slowly lowered to room temperature. The reactor was opened to unload the catalyst, and 1 g of the reduced catalyst was placed in a reactor. In the presence of 20 g of the reaction raw materials (the mass ratio of octenal to octanol was 1:3), the reaction temperature was 80°C, the reaction pressure was 2 MPa, and the reaction space velocity was 2 h -1 The reaction is carried out to prepare octanal.
[0077] Example 5
[0078] The difference from Example 4 is that the catalyst is replaced by the catalyst obtained in Example 2;
[0079] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanal.
[0080] Example 6
[0081] In addition to the above differences, the differences from Example 4 are: the catalyst is replaced by the catalyst obtained in Example 3;
[0082] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanal.
[0083] Example 7
[0084] The difference from Example 4 is that the mass ratio of octenal to octanol is 1:6, the reaction temperature is 60°C, the reaction pressure is 3MPa, and the reaction space velocity is 1h -1 ;
[0085] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanal.
[0086] Example 8
[0087] The difference from Example 7 is that the catalyst is replaced by the catalyst obtained in Example 2;
[0088] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 7 to prepare octanal.
[0089] Example 9
[0090] The difference from Example 7 is that the catalyst is replaced by the catalyst obtained in Example 3;
[0091] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 7 to prepare octanal.
[0092] Example 10
[0093] The difference from Example 4 is that the mass ratio of octenal to octanol is 1:2, the reaction temperature is 100°C, the reaction pressure is 1 MPa, and the reaction space velocity is 3 h -1 ;
[0094] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanal.
[0095] Embodiment 11
[0096] The difference from Example 10 is that the catalyst is replaced by the catalyst obtained in Example 2;
[0097] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 10 to prepare octanal.
[0098] Example 12
[0099] The difference from Example 10 is that the catalyst is replaced by the catalyst obtained in Example 3;
[0100] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 10 to prepare octanal.
[0101] Comparative Example 1
[0102] 50 g of shaped Al2O3 carrier (BET specific surface area of 214 m 2 / g, pore volume is 0.97cm 3 / g), and impregnated with nickel nitrate solution by equal volume impregnation method. After 20 minutes of impregnation, the catalyst precursor was taken out, and then dried at 110°C for 7h and calcined at 450°C for 3h to finally obtain a catalyst with a Ni content of 10wt% and an Al2O3 carrier content of 90wt%.
[0103] Comparative Example 2
[0104] The difference from Example 4 is that the catalyst is replaced by the catalyst obtained in Comparative Example 1;
[0105] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanal.
[0106] Comparative Example 3
[0107] The difference from Example 7 is that the catalyst is replaced by the catalyst obtained in Comparative Example 1;
[0108] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 7 to prepare octanal.
[0109] Comparative Example 4
[0110] The difference from Example 10 is that the catalyst is replaced by the catalyst obtained in Comparative Example 1;
[0111] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 10 to prepare octanal.
[0112] According to the above evaluation method, the catalysts prepared in Examples 1 to 3 and Comparative Example 1 were respectively evaluated for reaction. Table 1 shows the detailed evaluation results.
[0113] Table 1 BET characterization results and reaction evaluation results of catalysts
[0114]
[0115] Compared with Comparative Example 1, the nickel dispersion of the prepared catalyst in Example 1 increases from 1.14% to 3.12%, and the nickel particle size increases from 78.4 nm to 31.5 nm, which proves that the rotary enhanced impregnation method of the present invention can improve the dispersion of the catalytically active components while reducing their particle size, thereby obtaining a catalyst with higher metal dispersion and smaller metal particle size, which is more conducive to the reaction and has better catalytic performance.
[0116] Compared with Comparative Example 2, the conversion rate of octenal in Example 4 is increased from 85% to 90%, and the yield of octanal is increased from 70% to 75%;
[0117] Compared with Comparative Example 3, the conversion rate of octenal in Example 7 increased from 80% to 88%, and the yield of octanal increased from 65% to 74%.
[0118] Compared with Comparative Example 4, the conversion rate of octenal in Example 10 increased from 82% to 89%, and the yield of octanal increased from 72% to 75%;
[0119] Compared with the corresponding comparative examples, the octenal conversion rate of the above embodiments is increased by about 5-8%, and the octanal yield is increased by about 3-9%, achieving a significant improvement.
[0120] Examples 4 to 12 respectively use the catalysts prepared in Examples 1 to 3 to prepare octanal, with octenal conversion rates of 84 to 90% and octanal yields of 70 to 75%, which confirms that the catalyst prepared by the present invention has a high conversion rate for selectively preparing octanal and has good catalytic performance.
Claims
1. A catalyst for selectively preparing octanal, comprising a carrier and an active metal component supported on the carrier; the active metal component is one of Cu, Co, and Ni; the carrier is one of Al2O3, MgO, ZrO2, TiO2, and SiO2; Taking the total weight of the catalyst as 100%, the active metal component is 2-15wt%, and the carrier is 85-98wt%; preferably, the active metal component is 5-15wt%, and the carrier is 85-95wt%; The catalyst is prepared by using a rotary enhanced impregnation device; the rotary enhanced impregnation device comprises a rotary enhanced packing bed, in which a carrier ring loaded with a carrier and a rotary packing are arranged, and the carrier ring is located outside the rotary packing; the carrier ring and the rotary packing can both rotate independently.
2. The catalyst for selectively preparing octanal as claimed in claim 1, characterized in that: The precursor of the metal element in the active metal component is a soluble salt of the metal element, preferably at least one of the soluble salts of Cu, Co, and Ni, more preferably at least one of the nitrates, carbonates, and sulfates of Cu, Co, and Ni; and / or, The specific surface area of the carrier is 100 to 300 m 2 / g, pore volume is 0.5~1.5cm 3 / g, preferably, the specific surface area of the carrier is 140 to 250 m 2 / g, pore volume is 0.7~1.2cm 3 / g.
3. The catalyst for selectively preparing octanal as claimed in claim 1, characterized in that: The rotary enhanced impregnation device also includes a liquid storage tank and a liquid pump. The rotary enhanced packing bed is a cylindrical structure and also includes a liquid distributor. The liquid distributor is located at the center of the rotary enhanced packing bed. Rotating packing and carrier rings are sequentially arranged on the periphery of the liquid distributor. The liquid pump is connected to the liquid storage tank to allow the impregnation liquid in the liquid storage tank to enter the liquid distributor through the impregnation liquid inlet. An impregnation liquid outlet is arranged at the lower end of the rotary enhanced packing bed.
4. The catalyst for selectively preparing octanal as claimed in claim 1, characterized in that: The rotary intensified impregnation device further comprises a motor, preferably two motors, which are used to drive the carrier ring to rotate and the filler to rotate respectively; and / or, The rotating packing is at least one of a wire mesh and a columnar packing, preferably at least one of a stainless steel wire mesh packing and a stainless steel columnar packing; and / or, The carrier ring is a wire mesh carrier ring.
5. A method for preparing a catalyst for selectively preparing octanal as claimed in any one of claims 1 to 4, comprising the following steps: (1) In the rotating enhanced impregnation device, the carrier is loaded into a rotatable carrier ring, and the soluble salt solution of the metal element is used as an impregnation liquid and sprayed into the inner side of the rotating filler. Under the action of centrifugal force, the impregnation liquid is sprayed on the rotating carrier to enhance the impregnation, and then a catalyst precursor is obtained, and then after drying and calcination, the catalyst is obtained; Optionally, (2) repeat step (1).
6. The method for preparing the catalyst according to claim 5, characterized in that: The mass concentration of the soluble salt solution of the metal element is 5-35%, and the solvent is water, preferably deionized water; and / or, The soluble salt solution of the metal element is sprayed into the inner side of the rotating filler through a liquid distributor, and the liquid inlet flow rate of the liquid distributor is 1 to 50 ml / min, preferably 5 to 10 ml / min.
7. The method for preparing the catalyst according to claim 5, characterized in that: The rotating speed of the rotating filler is 1000-2000 rpm; and / or, The rotation speed of the carrier ring is 10-20 rpm; and / or, The time of the enhanced impregnation is 10 to 30 minutes; and / or, The drying conditions are drying at 100-120° C. for 2-10 hours; preferably drying at 110-120° C. for 2-8 hours; and / or, The calcination conditions are 300-600° C. for 2-10 h, preferably 350-550° C. for 3-6 h.
8. A catalyst obtained by the preparation method according to any one of claims 5 to 7.
9. Use of the catalyst according to any one of claims 1 to 4 or 8 in the selective preparation of octanal, preferably, octenal and hydrogen are used as raw materials, and the octanal is prepared by reacting in a solvent under the action of the catalyst.
10. The use according to claim 9, characterized in that: Reaction temperature 60-100°C; and / or, Reaction pressure 1-3 MPa; and / or, Reaction space velocity 1~3h -1 and / or, The solvent is an alcohol solvent, preferably a monohydric alcohol having 2 to 8 carbon atoms, more preferably ethanol or octanol; and / or, The mass ratio of the octenal to the solvent is 1:(2-6).