Alkali metal doped modified Ni / Al2O3 catalyst as well as preparation method and application thereof
By using alkali metal doping modified Ni/Al2O3 catalyst to catalyze 5-hydroxymethylfurfural in hydrogen atmosphere, the problem of complexity and low efficiency of traditional preparation of 2,5-tetrahydrofuran dimethanol is solved, and high efficiency of high purity products is achieved The preparation and reusability of catalysts have the advantages of industrial applications.
Patent Information
- Application Number
- CN202411390303.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The traditional method of preparing 2,5-tetrahydrofuran dimethanol has complex reaction process, low production efficiency and produces a large amount of waste liquid. The existing 5-hydroxymethylfurfural hydrogenation preparation method has room for improvement in catalyst performance and reaction efficiency, which is difficult to achieve. Industrialized production.
Using alkali metal doping modified Ni/Al2O3 catalyst, a highly active catalyst was prepared by fully contacting the alumina support with the nickel salt solution and the alkali metal solution and sintering treatment, and 5-hydroxymethyl is made in a hydrogen atmosphere. Furfural reacts with a catalyst to obtain high purity 2,5-tetrahydrofuran dimethanol.
It significantly improves catalytic hydrogenation activity and target product selectivity, easy recovery of catalysts, simple reaction process, high purity and low cost, and has the prospect of industrial application.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and in particular relates to an alkali metal doped modified Ni / Al2O3 catalyst and a preparation method and application thereof. Background Art
[0002] 2,5-Tetrahydrofuran dimethanol (THFDM), as a bio-based furan monomer containing a saturated furan ring, has both an oxygen-containing rigid ring structure and a symmetrical diol functional group. It can be widely used in solvents, surfactants, polyesters and other fields, and has unique advantages in barrier properties and dyeing properties. In the field of polymer materials, THFDM has received widespread attention because it can replace ethylene glycol to prepare bio-based polyesters. The main traditional method for preparing THFDM is microbial fermentation, but this method has a complex reaction process, low production efficiency, and produces a large amount of waste liquid and waste, which seriously affects the scale. The synthesis of THFDM from biomass resources is a clean and renewable route. The existing method of preparing THFDM by hydrogenating 5-hydroxymethylfurfural (HMF) still has room for improvement in catalyst performance and reaction efficiency. Therefore, it is urgent to study and develop a preparation method of THFDM suitable for industrial production. Summary of the invention
[0003] The main purpose of the present invention is to provide an alkali metal doped modified Ni / Al2O3 catalyst and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.
[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0005] The embodiment of the present invention provides a method for preparing an alkali metal-doped modified Ni / Al2O3 catalyst, which comprises:
[0006] The alumina carrier is mixed and fully contacted with the nickel salt solution, and then subjected to a first sintering treatment to obtain a Ni / Al2O3 catalyst;
[0007] Furthermore, the Ni / Al2O3 catalyst is mixed and fully contacted with an alkali metal solution, and then subjected to a second sintering treatment to obtain an alkali metal-doped modified Ni / Al2O3 catalyst.
[0008] The embodiment of the present invention also provides an alkali metal-doped modified Ni / Al2O3 catalyst prepared by the aforementioned preparation method.
[0009] The embodiment of the present invention also provides the use of the aforementioned alkali metal-doped modified Ni / Al2O3 catalyst in catalyzing the preparation of 2,5-tetrahydrofuran dimethanol from 5-hydroxymethylfurfural.
[0010] The present invention also provides a method for preparing 2,5-tetrahydrofuran dimethanol, which comprises:
[0011] In a hydrogen atmosphere, a reaction system comprising at least 5-hydroxymethylfurfural, a catalyst and a solvent is reacted to produce 2,5-tetrahydrofuran dimethanol;
[0012] Wherein, the catalyst includes the aforementioned alkali metal-doped modified Ni / Al2O3 catalyst.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] (1) The alkali metal-doped modified Ni / Al2O3 catalyst prepared by the present invention significantly improves its catalytic hydrogenation activity and target product selectivity;
[0015] (2) The alkali metal-doped modified Ni / Al2O3 catalyst used in the preparation of 2,5-tetrahydrofuran dimethanol is easy to recover and has good stability and reusability;
[0016] (3) The present invention benefits from the high selectivity of the target product when preparing 2,5-tetrahydrofuran dimethanol, and a high-purity product can be obtained by simple rotary evaporation, with low refining cost;
[0017] (4) The alkali metal-doped modified Ni / Al2O3 catalyst of the present invention is easy to scale up, the reaction process and post-treatment operations are simple, the product has high added value, and has a prospect for industrial application. DETAILED DESCRIPTION
[0018] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution mainly uses amorphous alumina as a carrier, loads active metal Ni and supplements it with alkali metal doping modification to prepare highly active Ni / Al2O3; in a kettle reactor, using hydrogen as a hydrogen source, the 5-hydroxymethylfurfural raw material solution and the catalyst are fully mixed to react to obtain a THFDM reaction liquid. After the reaction liquid is filtered and rotary evaporated to remove the catalyst and the solvent respectively, a high-purity THFDM product can be obtained. This product has great application prospects in the field of degradable materials; the catalyst and its application method in the present invention have the advantages of simple operation, low cost, and scalable application.
[0019] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Specifically, as one aspect of the technical solution of the present invention, a method for preparing an alkali metal-doped modified Ni / Al2O3 catalyst includes:
[0021] The alumina carrier is mixed and fully contacted with the nickel salt solution, and then subjected to a first sintering treatment to obtain a Ni / Al2O3 catalyst;
[0022] Furthermore, the Ni / Al2O3 catalyst is mixed and fully contacted with an alkali metal solution, and then subjected to a second sintering treatment to obtain an alkali metal-doped modified Ni / Al2O3 catalyst.
[0023] In some preferred embodiments, the preparation method specifically comprises:
[0024] The alumina carrier is fully impregnated in a nickel salt solution, and then the solvent is removed by stirring at 60-90°C, and then a first sintering treatment is performed at 100-600°C for 4-8 hours to obtain a Ni / Al2O3 catalyst;
[0025] Furthermore, the Ni / Al2O3 catalyst is fully impregnated in an alkali metal solution, then stirred at 60-90°C to remove the solvent, and then a second sintering treatment is performed at 100-600°C for 4-8h to obtain an alkali metal-doped modified Ni / Al2O3 catalyst.
[0026] Further, the nickel salt includes nickel nitrate, but is not limited thereto.
[0027] Furthermore, the cations in the alkali metal solution include any one or more combinations of lithium ions, sodium ions, potassium ions, rubidium ions, and cesium ions, but are not limited thereto.
[0028] Furthermore, the cations in the alkali metal solution include sodium ions and / or potassium ions, but are not limited thereto.
[0029] Furthermore, the anions in the alkali metal solution include any one or more combinations of chloride ions, nitrate ions, sulfate ions, and carbonate ions, but are not limited thereto.
[0030] Furthermore, the anions in the alkali metal solution include chloride ions and / or nitrate ions, but are not limited thereto.
[0031] Furthermore, in the Ni / Al2O3 catalyst, Ni is loaded on an Al2O3 carrier in the form of nanoparticles.
[0032] Furthermore, the concentration of nickel ions in the nickel salt solution is 0.01-0.2 mol / L.
[0033] Furthermore, the Ni content in the Ni / Al2O3 catalyst is 5 to 50 wt%.
[0034] Furthermore, the concentration of cations in the alkali metal solution is 0.01 to 0.3 mol / L.
[0035] Furthermore, the concentration of cations in the alkali metal solution is 0.01-0.2 mol / L.
[0036] Furthermore, the temperature of the first sintering treatment is 150-550°C.
[0037] Furthermore, the temperature of the second sintering treatment is 150-550°C.
[0038] Another aspect of the embodiments of the present invention further provides an alkali metal-doped modified Ni / Al2O3 catalyst prepared by the aforementioned preparation method.
[0039] Furthermore, in the alkali metal-doped modified Ni / Al2O3 catalyst, the alkali metal is embedded in the surface of the alumina carrier in the form of oxide, and the content of the alkali metal in the alkali metal-doped modified Ni / Al2O3 catalyst is 0.05-0.47wt%.
[0040] Another aspect of the embodiments of the present invention further provides the use of the aforementioned alkali metal-doped modified Ni / Al2O3 catalyst in catalyzing the preparation of 2,5-tetrahydrofuran dimethanol from 5-hydroxymethylfurfural.
[0041] Another aspect of the embodiments of the present invention further provides a method for preparing 2,5-tetrahydrofuran dimethanol, which comprises:
[0042] In a hydrogen atmosphere, a reaction system comprising at least 5-hydroxymethylfurfural, a catalyst and a solvent is reacted to produce 2,5-tetrahydrofuran dimethanol;
[0043] Wherein, the catalyst includes the aforementioned alkali metal doped modified Ni / A12O3 catalyst.
[0044] In some preferred embodiments, the preparation method specifically includes: placing 5-hydroxymethylfurfural, a catalyst, and a solvent in a reaction device, and stirring the reaction for 2 to 12 hours under the conditions of a hydrogen pressure of 1 to 10 MPa and a temperature of 60-200° C. to obtain 2,5-tetrahydrofuran dimethanol.
[0045] Furthermore, the mass ratio of the 5-hydroxymethylfurfural to the catalyst is 4:1 to 500:1.
[0046] Furthermore, the mass ratio of 5-hydroxymethylfurfural to catalyst is 10:1 to 100:1, and the most preferred ratio is 25:1.
[0047] Furthermore, the hydrogen pressure is 2-6 MPa.
[0048] Furthermore, the temperature is 70°C to 150°C.
[0049] Furthermore, the temperature is 80°C to 150°C.
[0050] Furthermore, the stirring reaction time is 2 to 8 hours.
[0051] Furthermore, the solvent includes any one or more combinations of ethanol, methanol, isopropanol, 1,4-dioxane, and water, but is not limited thereto.
[0052] Furthermore, the solvent is methanol.
[0053] In some preferred embodiments, the concentration of 5-hydroxymethylfurfural in the reaction system is 0.01 to 5 mol / L.
[0054] In some more specific embodiments, the method for preparing 2,5-tetrahydrofuran dimethanol comprises:
[0055] (1) immersing the support in a certain amount of nickel nitrate solution, stirring and evaporating to dryness, and calcining at a certain temperature;
[0056] (2) immersing the above product in an alkali metal solution of a certain concentration, stirring and evaporating, and calcining at a certain temperature to obtain an alkali metal-doped modified Ni / Al2O3 catalyst;
[0057] (3) Adding the prepared alkali metal-doped modified Ni / Al2O3 catalyst, 5-hydroxymethylfurfural, and reaction solvent into a reaction device, stirring and reacting at a certain temperature and hydrogen pressure; then cooling the reaction liquid to room temperature, filtering the catalyst to obtain the reaction stock solution, and rotary evaporating to obtain THFDM.
[0058] Preferably, the calcination temperature is 100-600°C.
[0059] Preferably, the calcination temperature is independently selected from 150, 250, 350, 450, 550°C, most preferably 450°C.
[0060] Preferably, the alkali metal cations are lithium ions, sodium ions, potassium ions, rubidium ions and cesium ions.
[0061] Preferably, the alkali metal cations are sodium ions and potassium ions.
[0062] Preferably, the anion of the alkali metal cation is chloride ion, nitrate ion, sulfate ion, or carbonate ion.
[0063] Preferably, the anion of the alkali metal cation is chloride ion or nitrate ion.
[0064] Preferably, the concentration of the alkali metal cation solution is 0.01-0.3M.
[0065] Preferably, the concentration of the alkali metal cation solution is independently selected from 0.01M, 0.03M, 0.05M, 0.1M, 0.15M, and 0.2M.
[0066] Preferably, the mass ratio of the 5-hydroxymethylfurfural to the catalyst is 4:1 to 500:1, preferably 25:1.
[0067] Preferably, the hydrogen in the hydrogen-containing atmosphere is in excess in terms of the molar ratio of hydrogen to 5-hydroxymethylfurfural.
[0068] Preferably, the reaction conditions are: reaction temperature of 60-200° C.; reaction pressure of 1-10 MPa; reaction time of 2-12 h.
[0069] Preferably, the reaction temperature is independently selected from 200°C, 180°C, 160°C, 150°C, 140°C, 120°C, 100°C, 80°C, 70°C, and 60°C.
[0070] Preferably, the reaction pressure is independently selected from 10 MPa, 8 MPa, 6 MPa, 4 MPa, 2 MPa, and 1 MPa.
[0071] Preferably, the reaction time is independently selected from 12 h, 10 h, 8 h, 6 h, 4 h, and 2 h.
[0072] Preferably, the reaction pressure is 2 MPa to 6 MPa, most preferably 4 MPa.
[0073] Preferably, the reaction temperature is 70°C to 150°C.
[0074] More preferably, the reaction temperature is 80°C to 150°C, most preferably 120°C.
[0075] Preferably, the reaction time is 2 to 8 hours, most preferably 4 hours.
[0076] Preferably, the raw material further comprises a solvent: the solvent is selected from at least one of ethanol, methanol, isopropanol, 1,4-dioxane and water, preferably methanol.
[0077] Preferably, the concentration of 5-hydroxymethylfurfural in the raw material is 0.01-5M.
[0078] Preferably, the concentration of 5-hydroxymethylfurfural in the raw material is independently selected from 0.01M, 0.05M, 0.1M, 0.15M, 0.2M, 0.25M, 0.3M, 0.35M, 0.4M, 0.45M, 0.5M, 1M, 1.5M, 2M, 2.5M, 3M, 4M, 5M, and most preferably 0.25M.
[0079] Preferably, the solvent is analytically pure (>99.8%) anhydrous methanol.
[0080] Preferably, the reaction pressure is stabilized by inputting high-purity hydrogen.
[0081] Preferably, the reaction temperature is raised to a stable reaction temperature by intelligent constant heating.
[0082] Preferably, the reaction time is the reaction time after reaching a constant pressure and a constant temperature.
[0083] Preferably, the catalytically active substance in the present application refers to a metal / carrier-supported catalyst in which metal nanoparticles are uniformly supported on the surface of a carrier.
[0084] Preferably, the reaction is carried out in a reactor.
[0085] The alkali metal doped modified Ni / Al2O3 catalyst prepared by the present invention has excellent hydrogenation activity and selectivity, can realize the one-pot high-selective hydrogenation synthesis of 2,5-tetrahydrofuran dimethanol from 5-hydroxymethylfurfural, the selectivity of 2,5-tetrahydrofuran dimethanol in the reaction solution is greater than 99.5%, and a high-purity product (99.9%) can be obtained by simple rotary evaporation. The catalyst can be recycled and reused, which greatly reduces the production cost of the product.
[0086] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments. This embodiment is implemented on the premise of the technical solution of the invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0087] The experimental materials used in the examples used below, unless otherwise specified, the raw materials and catalysts in the examples of the present invention were purchased through commercial channels, all purchased from Adamas Group Chemical Reagent Co., Ltd.
[0088] Unless otherwise specified, conventional methods were used for testing methods, and instrument settings were all those recommended by the manufacturer. The composition (purity) analysis method of the product and mother liquor was performed using Agilent's 8860 high performance gas chromatograph to analyze the products in the 5-hydroxymethylfurfural synthesis reaction.
[0089] Example 1
[0090] Hydrogenation reaction: In a 5L high-pressure reactor, 250g HMF, 3L methanol and 20g Raney nickel (99%, Ni: 47wt%) were added, the air in the reactor was replaced with hydrogen 3 times, hydrogen was filled to 4.0MPa, the temperature was raised to 130°C, and the reaction was stirred for 2h. After the reaction was completed, the reaction mixture was cooled to room temperature, the catalyst was separated by filtration, and the reaction solution was analyzed by GC. The analysis results are shown in Table 1.
[0091] Example 2
[0092] (1) Preparation of 0.47Ni / Al2O3 catalyst: 73g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and then immersed for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.47Ni / Al2O3 (Ni: 47wt%) catalyst.
[0093] (2) Hydrogenation reaction: A 0.47 Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 1.
[0094] Example 3
[0095] (1) Preparation of 0.47Ni / TiO2 catalyst: 73g of nickel nitrate was dissolved in 200mL of deionized water, 20g of titanium oxide carrier was added, stirred evenly and soaked for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.47Ni / TiO2 (Ni: 47wt%) catalyst.
[0096] (2) Hydrogenation reaction: A 0.47 Ni / TiO2 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 1.
[0097] Example 4
[0098] (1) Preparation of 0.47Ni / ZrO2 catalyst: 73g of nickel nitrate was dissolved in 200mL of deionized water, 20g of zirconium oxide carrier was added, stirred evenly and soaked for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.47Ni / ZrO2 (Ni: 47wt%) catalyst.
[0099] (2) Hydrogenation reaction: A 0.47 Ni / ZrO2 catalyst was used, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 1.
[0100] Table 1 Preparation of THFDM by hydrogenation of HMF catalyzed by commercial Raney nickel and Ni supported on different carriers
[0101]
[0102] Through Examples 1-4, the Ni / Al2O3 catalyst with Ni as the active metal and Al2O3 as the carrier has very high catalytic activity and extremely high selectivity.
[0103] Example 5
[0104] (1) Preparation of 0.05Ni / Al2O3 catalyst: 3.6g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and impregnated for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.05Ni / Al2O3 (Ni: 5wt%) catalyst.
[0105] (2) Hydrogenation reaction: A 0.05Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0106] Example 6
[0107] (1) Preparation of 0.10Ni / Al2O3 catalyst: 7.2g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and soaked for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.01Ni / Al2O3 (Ni: 10wt%) catalyst.
[0108] (2) Hydrogenation reaction: A 0.01Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0109] Example 7
[0110] (1) Preparation of 0.15Ni / Al2O3 catalyst: 11.8g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and then impregnated for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.15Ni / Al2O3 (Ni: 15wt%) catalyst.
[0111] (2) Hydrogenation reaction: A 0.15Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0112] Example 8
[0113] (1) Preparation of 0.20Ni / Al2O3 catalyst: 17.0g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and soaked for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.20Ni / Al2O3 (Ni: 20wt%) catalyst.
[0114] (2) Hydrogenation reaction: A 0.20 Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0115] Example 9
[0116] (1) Preparation of 0.25Ni / Al2O3 catalyst: 23.3 g of nickel nitrate was dissolved in 200 mL of deionized water, 20 g of alumina carrier was added, stirred evenly and impregnated for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.25Ni / Al2O3 (Ni: 25 wt%) catalyst.
[0117] (2) Hydrogenation reaction: A 0.25Ni / A12O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0118] Example 10
[0119] (1) Preparation of 0.30Ni / Al2O3 catalyst: 30.2g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and soaked for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.30Ni / Al2O3 (Ni: 30wt%) catalyst.
[0120] (2) Hydrogenation reaction: A 0.30 Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0121] Embodiment 11
[0122] (1) Preparation of 0.35Ni / Al2O3 catalyst: 39.4g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and impregnated for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.35Ni / Al2O3 (Ni: 35wt%) catalyst.
[0123] (2) Hydrogenation reaction: A 0.35 Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0124] Example 12
[0125] (1) Preparation of 0.40Ni / Al2O3 catalyst: 52.6g of nickel nitrate was dissolved in 200mL of deionized water, 20g of alumina carrier was added, stirred evenly and then impregnated for 10 hours, then stirred and evaporated in a 90°C water bath, and finally calcined at 450°C for 5 hours to obtain 0.40Ni / Al2O3 (Ni: 40wt%) catalyst.
[0126] (2) Hydrogenation reaction: A 0.40 Ni / Al2O3 catalyst was used, and the rest was the same as in Example 1. The reaction solution was analyzed by GC. The analysis results are shown in Table 2.
[0127] Examples 5-12 vary the loading amount of nickel element.
[0128] Table 2 Preparation of THFDM by hydrogenation of HMF catalyzed by xNi / A12O3 with different Ni loadings
[0129]
[0130]
[0131] From Examples 2 and 5-12, it is clear that the optimal loading amount of Ni is 0.35.
[0132] Embodiment 13
[0133] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0134] (2) Optimizing the catalyst: The 0.35Ni / Al2O3 catalyst prepared above was immersed in 20mL of 0.01mol / L potassium chloride solution for 8 hours, evaporated to dryness with stirring in a 90°C water bath, and calcined at 450°C for 5 hours to obtain a 0.01K0.35Ni / Al2O3 catalyst optimized by adding potassium ions.
[0135] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 3.
[0136] Embodiment 14
[0137] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0138] (2) Optimizing the catalyst: Changing the concentration of the potassium chloride solution to 0.03 mol / L, and the rest being the same as in Example 13, a 0.03K0.35Ni / Al2O3 catalyst was obtained.
[0139] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 3.
[0140] Embodiment 15
[0141] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0142] (2) Optimizing the catalyst: Changing the concentration of the potassium chloride solution to 0.05 mol / L, and the rest being the same as in Example 13, a 0.05K0.35Ni / Al2O3 catalyst was obtained.
[0143] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 3.
[0144] Example 16
[0145] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0146] (2) Optimizing the catalyst: The concentration of the potassium chloride solution was changed to 0.10 mol / L, and the rest was the same as in Example 13 to obtain a 0.10K0.35Ni / Al2O3 catalyst.
[0147] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 3.
[0148] Embodiment 17
[0149] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0150] (2) Optimizing the catalyst: Changing the concentration of the potassium chloride solution to 0.15 mol / L, and the rest being the same as in Example 13, a 0.15K0.35Ni / Al2O3 catalyst was obtained.
[0151] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 3.
[0152] Embodiment 18
[0153] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0154] (2) Optimizing the catalyst: Changing the concentration of the potassium chloride solution to 0.20 mol / L, and the rest being the same as in Example 13, a 0.20K0.35Ni / Al2O3 catalyst was obtained.
[0155] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 3.
[0156] Table 3 Preparation of THFDM by hydrogenation of HMF catalyzed by xKxNi / Al2O3 with different potassium ion concentrations (KCl)
[0157]
[0158] Through Examples 13-18, it is clear that the optimal concentration of KCl is 0.10 mol / L.
[0159] Embodiment 19
[0160] (1) Preparation of 0.35Ni / Al2O3 catalyst: Same as Example 11.
[0161] (2) Optimizing the catalyst: The potassium chloride solution was replaced with a potassium nitrate solution, and the rest was the same as in Example 16 to obtain a 0.10K0.35Ni / Al2O3-N catalyst.
[0162] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 4.
[0163] Table 4 Preparation of THFDM by catalytic hydrogenation of HMF with different potassium sources 0.10K0.35Ni / Al2O3
[0164]
[0165] Through Examples 16 and 19, KCl has a relative advantage as a potassium salt source.
[0166] Embodiment 20
[0167] (1) Preparation of 0.35Ni / A12O3 catalyst: Same as Example 11.
[0168] (2) Optimizing the catalyst: The potassium chloride solution was replaced with a sodium chloride solution, and the rest was the same as in Example 16 to obtain a 0.10Na0.35Ni / Al2O3 catalyst.
[0169] (3) Hydrogenation reaction: As in Example 1, the reaction solution was analyzed by GC. The analysis results are shown in Table 5.
[0170] Table 5 Preparation of THFDM by catalytic hydrogenation of HMF with different alkali metal modified 0.10X0.35Ni / Al2O3
[0171]
[0172] Through Examples 16 and 20, it can be seen that potassium ions have a relative advantage in the 0.35Ni / Al2O3 catalyst modified with different alkali metals.
[0173] Embodiment 21
[0174] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 120°C, the reaction time was 2 h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0175] Embodiment 22
[0176] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 110°C, the reaction pressure was 5 MPa, the reaction time was 3 h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0177] Embodiment 23
[0178] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 100°C, the reaction pressure was 5 MPa, the reaction time was 4 h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0179] Embodiment 24
[0180] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 130°C, the reaction time was 0.5h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0181] Embodiment 25
[0182] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 140°C, the reaction time was 0.5h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0183] Embodiment 26
[0184] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 150°C, the reaction time was 0.5h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0185] Embodiment 27
[0186] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 160°C, the reaction time was 0.5h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0187] Embodiment 28
[0188] (1) Hydrogenation reaction: Using 0.10K0.35Ni / Al2O3 catalyst, the temperature was changed to 170°C, the reaction time was 0.5h, and the rest was the same as in Example 1. The reaction liquid was analyzed by GC. The analysis results are shown in Table 6.
[0189] Table 6 Reaction performance of 0.10K0.35Ni / Al2O3 catalyst under different reaction conditions
[0190]
[0191] Through Examples 16 and 21-28, it is clear that the optimal reaction temperature is 150°C and the reaction pressure is 4 MPa.
[0192] The catalyst in Example 26 was used as a typical representative for the catalyst stability test.
[0193] (1) Filtering with a 0.45 μm organic filter membrane to recover the catalyst;
[0194] (2) Hydrogenation reaction: Same as in Example 1, the difference in the number of recycling cycles and catalyst performance is shown in Table 7 below;
[0195] Table 7 Catalyst cycle stability test
[0196] Cycle times HMF conversion rate / % THFDM selectivity / % 1 100 99.6 2 100 99.7 3 100 99.8 4 100 99.7 5 100 99.7
[0197] The reaction solution obtained in Example 16 was used as a typical example to purify THFDM.
[0198] The specific steps are as follows:
[0199] (1) After the reaction liquid is cooled, it is filtered using a 0.45 μm organic microporous filter membrane to remove the catalyst.
[0200] (2) The solution from step (1) after the catalyst is filtered out is transferred to a 5 L round-bottom flask and placed on a rotary evaporator. The temperature is controlled at 45° C., the negative pressure is controlled at −0.10 MPa, and the rotation speed is controlled at 75 rpm to evaporate the solvent.
[0201] (3) The liquid obtained by rotary evaporation of the solvent in step (2) is transferred to a 5 L round-bottom flask and placed on a rotary evaporator. The temperature is controlled at 155° C., the negative pressure is controlled at −0.15 MPa, and the rotation speed is controlled at 80 rpm to rotary evaporate various low-boiling point by-products. The liquid obtained by rotary evaporation is pure THFDM with a purity of up to 99.99%.
[0202] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0203] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases.
[0204] Under the scope of protection of the invention and the claims, all technical modifications made according to the technical solution of the present invention fall within the protection scope of the present invention.
Claims
1. A method for preparing an alkali metal-doped modified Ni / Al2O3 catalyst, characterized in that: include: The alumina carrier is mixed and fully contacted with the nickel salt solution, and then subjected to a first sintering treatment to obtain a Ni / Al2O3 catalyst; Furthermore, the Ni / Al2O3 catalyst is mixed and fully contacted with an alkali metal solution, and then subjected to a second sintering treatment to obtain an alkali metal-doped modified Ni / Al2O3 catalyst.
2. The preparation method according to claim 1, characterized in that: Specifically include: The alumina carrier is fully impregnated in a nickel salt solution, and then the solvent is removed by stirring at 60-90°C, and then a first sintering treatment is performed at 100-600°C for 4-8 hours to obtain a Ni / Al2O3 catalyst; Furthermore, the Ni / Al2O3 catalyst is fully immersed in an alkali metal solution, then stirred at 60-90°C, and then subjected to a second sintering treatment at 100-600°C for 4-8h to obtain an alkali metal-doped modified Ni / Al2O3 catalyst.
3. The preparation method according to claim 2, characterized in that: The nickel salt includes nickel nitrate; And / or, the cations in the alkali metal solution include any one or more combinations of lithium ions, sodium ions, potassium ions, rubidium ions, and cesium ions, preferably sodium ions and / or potassium ions; And / or, the anions in the alkali metal solution include any one or more combinations of chloride ions, nitrate ions, sulfate ions, and carbonate ions, preferably chloride ions and / or nitrate ions; And / or, in the Ni / Al2O3 catalyst, Ni is loaded on an Al2O3 carrier in the form of nanoparticles.
4. The preparation method according to claim 2, characterized in that: The concentration of nickel ions in the nickel salt solution is 0.01-0.2 mol / L; And / or, the Ni content in the Ni / i / Al2O3 catalyst is 5 to 50 wt%; and / or, the concentration of cations in the alkali metal solution is 0.01 to 0.3 mol / L, preferably 0.01 to 0.2 mol / L; And / or, the temperature of the first sintering treatment is 150-550°C; and / or, the temperature of the second sintering treatment is 150-550°C.
5. Alkali metal-doped modified Ni / Al2O3 catalyst prepared by the preparation method according to any one of claims 1 to 4; Preferably, the alkali metal in the alkali metal-doped modified Ni / Al2O3 catalyst is embedded in the surface of the alumina carrier in the form of oxide, and the content of the alkali metal in the alkali metal-doped modified Ni / Al2O3 catalyst is 0.05-0.47wt%.
6. Use of the alkali metal-doped modified Ni / i / Al2O3 catalyst according to claim 5 in catalyzing the preparation of 2,5-tetrahydrofuran dimethanol from 5-hydroxymethylfurfural.
7. A method for preparing 2,5-tetrahydrofuran dimethanol, characterized in that: include: In a hydrogen atmosphere, a reaction system comprising at least 5-hydroxymethylfurfural, a catalyst and a solvent is reacted to produce 2,5-tetrahydrofuran dimethanol; Wherein, the catalyst comprises the alkali metal doped modified Ni / Al2O3 catalyst as described in claim 5.
8. The preparation method according to claim 7, characterized in that: Specifically include: 5-Hydroxymethylfurfural, a catalyst and a solvent are placed in a reaction device, and stirred for reaction for 2 to 12 hours under the conditions of a hydrogen pressure of 1 to 10 MPa and a temperature of 60 to 200° C. to obtain 2,5-tetrahydrofuran dimethanol.
9. The preparation method according to claim 8, characterized in that: The mass ratio of 5-hydroxymethylfurfural to catalyst is 4:1 to 500:1, preferably 10:1 to 100:1; and / or, the hydrogen pressure is 2-6 MPa; and / or, the temperature is 70°C-150°C, preferably 80°C-150°C; And / or, the stirring reaction time is 2 to 8 hours; And / or, the solvent includes any one or more combinations of ethanol, methanol, isopropanol, 1,4-dioxane, and water, preferably methanol.
10. The preparation method according to claim 7, characterized in that: The concentration of 5-hydroxymethylfurfural in the reaction system is 0.01-5 mol / L.