Silicon-aluminum composite oxide catalyst with three-dimensional ordered macroporous structure as well as preparation method and application of silicon-aluminum composite oxide catalyst
Preparation of silicon-aluminum composite oxide catalysts with three-dimensional ordered macroporous structures by sol-gel method, solving the problems of low selectivity and short life of existing acetylene hydrogenation catalysts, achieving efficient acetylene conversion and ethylene selectivity, and extending the The service life of the catalyst.
Patent Information
- Application Number
- CN202411160780.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
The existing acetylene hydrogenation catalysts have problems of low selectivity and short catalyst life during the ethylene conversion process, which leads to excessive hydrogenation and polymerization of ethylene and affects product quality.
The silicon-aluminum composite oxide catalyst with three-dimensional ordered macroporous structures is prepared by sol-gel method. Nickel is used as the active component and zinc is used as the auxiliary agent to form a larger specific surface area and three-dimensional order by controlling the particle size and dispersion. Large pore structure to avoid sintering of active components and excessive hydrogenation of ethylene.
It improves the acetylene conversion rate and ethylene selectivity, extends the service life of the catalyst, avoids excessive hydrogenation and polymerization of ethylene, and significantly improves the stability and efficiency of the catalyst.
Smart Images

Figure BDA0005006340620000151 
Figure BDA0005006340620000161
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of industrial catalysis, and specifically relates to a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure, and a preparation method and application thereof. Background Art
[0002] Ethylene is the basic raw material for synthetic resins, synthetic fibers, synthetic rubber, medicines, dyes, pesticides, new chemical materials and daily chemical products, and its products account for more than 75% of petrochemical products; as the core of the petrochemical industry, the ethylene industry occupies an important position in the national economy. In chemical production, ethylene is mainly produced by steam cracking of hydrocarbons, and the cracking products usually contain 0.1% to 2% acetylene. Since acetylene can easily cause poisoning and deactivation of downstream polyolefin catalysts and affect the quality of polymerization products, acetylene is often converted into ethylene through catalytic selective hydrogenation.
[0003] At present, the methods for converting acetylene into ethylene include catalytic hydrogenation, solvent absorption, distillation, acetylene copper precipitation, complex adsorption, amination and porous material adsorption. The commonly used method in industry is catalytic hydrogenation, which converts acetylene into ethylene from an ethylene-rich stream by catalytic hydrogenation, thereby achieving the purpose of removing acetylene. The existing catalysts are mainly palladium and nickel. Palladium catalysts have the advantages of low start-up temperature, high hydrogenation activity and high space velocity; nickel catalysts have lower hydrogenation activity than palladium catalysts, but their cost is low, so they are also widely used in industry. Both catalysts face problems such as poor C2H4 selectivity caused by excessive hydrogenation of acetylene and short catalyst life caused by coking of unsaturated hydrocarbons and catalyst sintering. Reference 1 (J. Applied Surface Science, 2019, 495, 30: 143495.1-143495.12) reported a palladium nanoparticle catalyst uniformly dispersed in the mesopores of silicon molecular sieve MCM-41 by atomic layer deposition. The Pd nanoparticles are limited by the internal space of the molecular sieve and have a very narrow size distribution, which effectively prevents the particles from sintering during high-temperature treatment. As the reaction temperature increases, the acetylene conversion rate increases but the ethylene selectivity decreases. At the same time, the acetylene conversion rate decreases by about 50% after 10 hours of continuous reaction; Reference 2 (J. New Journal of Chemistry, 2019, 43, 46: 18120-18125) reported an alumina-supported nickel-copper catalyst prepared by coprecipitation. Under the optimal reaction conditions, the acetylene conversion rate is about 100% and the ethylene selectivity is about 71%, but the catalyst life is not mentioned; Reference 3 (J. Industrial And Engineering Chemistry Research, 2019, 58, 45: 20620-20629) reported a series of nickel-based catalysts such as nickel palladium, nickel silver, and nickel gallium. The results showed that the nickel gallium bimetallic catalyst had good catalytic performance. When the reaction temperature reached 280°C, the nickel gallium catalyst had an acetylene conversion rate of nearly 100% and an ethylene selectivity of nearly 80%. The catalyst life was not mentioned. In summary, acetylene hydrogenation catalysts are not ideal. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure in view of the deficiencies of the above-mentioned prior art. The method adopts a sol-gel method to prepare a catalyst with a silicon-aluminum composite oxide with a three-dimensional ordered macroporous structure as a carrier, nickel as an active component, and zinc as an additive. The catalyst has a smaller average particle size of the active component, a higher dispersion, and a larger specific surface area, so the catalytic hydrogenation activity is good, and the three-dimensional ordered macroporous structure of the carrier is conducive to the adsorption and desorption of acetylene and ethylene, avoiding excessive hydrogenation and polymerization of ethylene, and solving the problems of low ethylene selectivity and short catalyst life of the existing acetylene hydrogenation catalyst.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure, characterized in that the catalyst is prepared by a sol-gel method, and the specific process includes the following steps:
[0006] Step 1, dissolving aluminum salt and tetraethyl silicate in anhydrous ethanol and adjusting the pH with hydrochloric acid to obtain a first solution;
[0007] Step 2, dissolving nickel salt and zinc salt in deionized water to obtain a second solution;
[0008] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2 and add a template agent and a silane coupling agent to obtain a third solution, and continuously stir the third solution for aging to obtain a gel precursor;
[0009] Step 4: Dry the gel precursor obtained in step 3 and then calcine it in an oxygen environment to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure.
[0010] The preparation method of the above-mentioned three-dimensional ordered macroporous structure of silicon-aluminum composite oxide catalyst is characterized in that the aluminum salt in step one is aluminum nitrate nonahydrate or aluminum chloride hexahydrate; the nickel salt in step two is nickel nitrate hexahydrate or nickel sulfate hexahydrate, and the zinc salt is zinc nitrate hexahydrate or zinc sulfate heptahydrate; the template agent in step three is polystyrene microspheres or polymethyl methacrylate microspheres, and the silane coupling agent is 3-aminopropyltriethoxysilane or vinyltrimethoxysilane.
[0011] The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure is characterized in that hydrochloric acid is used to adjust the pH to 2-2.5 in step 1. Preferably, the pH is 2. The first solution is obtained by adjusting the pH to 2-2.5 with hydrochloric acid to control the gel time of subsequent aging, so that the catalyst obtains a smaller active component particle size and better dispersion.
[0012] The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure is characterized in that, in the third solution in step 3, the molar fraction is Al:Si:H2O:EtOH:APTES=1:0.5-5:2.5-25:3-15:0.1-1. Preferably, Al:Si:H2O:EtOH:APTES=1:2:6:10:0.4. By controlling the molar fraction ratio of each component in the third solution to control the aging gel formation time and the product silicon-aluminum ratio, a better three-dimensional ordered macroporous silicon-aluminum composite oxide is obtained.
[0013] The above-mentioned method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure is characterized in that the continuous stirring time in step 3 is 2h to 5h, the temperature is 50°C to 70°C; the aging temperature is room temperature, and the time is 2h to 24h. Preferably, the continuous stirring time is 3h, the temperature is 60°C; the aging temperature is 25°C, and the time is 12h.
[0014] The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure is characterized in that the drying temperature in step 4 is 100°C to 120°C, the time is 8h to 24h, and the calcination temperature is 450°C to 550°C, and the time is 3h to 6h. Preferably, the drying temperature is 105°C, the time is 12h; the calcination temperature is 500°C, and the time is 5.5h.
[0015] The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure is characterized in that the mass content of nickel in the catalyst Zn-Ni-SiO2@Al2O3 in step 4 is 0.5% to 20%, and the mass content of zinc is 0.1% to 0.5%. Preferably, the mass content of nickel in the catalyst Zn-Ni-SiO2@Al2O3 is 0.5%, 2%, 5%, 10% or 20%, and more preferably 2%; preferably, the mass content of zinc in the catalyst Zn-Ni-SiO2@Al2O3 is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, and more preferably 0.2%.
[0016] At the same time, the present invention also discloses a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure, which is characterized in that it is prepared by the above method.
[0017] In addition, the present invention also discloses an application of the silicon-aluminum composite oxide catalyst with the three-dimensional ordered macroporous structure as described above, characterized in that the application comprises the following steps:
[0018] Step 1: fix the catalyst in the constant temperature zone of the high pressure fixed bed reactor and check the air tightness of the system;
[0019] Step 2: Heat the high-pressure fixed-bed reactor after inspection in step 1 to 300°C to 400°C under a nitrogen atmosphere, and then introduce a H2 / N2 mixed gas with a H2 volume content of 10% at a flow rate of 0.1L / h to 2L / h under normal pressure to reduce the catalyst;
[0020] Step 3: introducing H2S / H2 mixed gas with a H2S volume content of 0.1% into the high-pressure fixed bed reactor after the reduction in step 2 to sulfide the reduced catalyst;
[0021] Step 4: Cool the catalyst after sulfurization in step 3, and then introduce acetylene mixed raw gas for catalytic hydrogenation reaction, and the space velocity of acetylene mixed raw gas is 2000h -1 ~10000h -1 The reaction temperature of the catalytic hydrogenation reaction is 120°C to 220°C, and the reaction pressure is 1.0MPa to 1.8MPa.
[0022] Preferably, in step 2, the temperature is raised to 300°C to 400°C, and the reduction time is 2h to 6h; more preferably, the temperature is raised to 380°C, and the reduction time is 4h. Preferably, in step 2, the flow rate of the H2 / N2 mixed gas is 1.8L / h.
[0023] Preferably, the space velocity of the acetylene mixed raw gas in step 4 is 2000h -1 , 4000h -1 、6000h -1 、8000h -1 or 10000h -1 ; More preferably 8000h -1 .
[0024] Preferably, the reaction temperature in step 4 is 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C or 220°C; more preferably 170°C.
[0025] Preferably, the reaction pressure in step 4 is 1.0 MPa, 1.1 MPa, 1.2 MPa, 1.3 MPa, 1.4 MPa, 1.5 MPa, 1.6 MPa, 1.7 MPa or 1.8 MPa; more preferably 1.4 MPa.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] 1. The present invention adopts a sol-gel method to prepare a catalyst with a silicon-aluminum composite oxide with a three-dimensional ordered macroporous structure as a carrier, nickel as an active component, and zinc as an additive. The catalyst has a smaller average particle size of the active component, a higher dispersion and a larger specific surface area, so the catalytic hydrogenation activity is good, and the three-dimensional ordered macroporous structure of the carrier is used as a support to provide sufficient space for the adsorption and desorption of acetylene and ethylene. At the same time, the active component nickel is coated in the pore structure and is not easy to sinter and agglomerate, thereby avoiding the phenomenon of excessive hydrogenation and polymerization of ethylene during the catalytic process, so that the non-precious metal catalyst has a higher acetylene conversion rate and ethylene selectivity, and the service life is extended.
[0028] 2. The catalyst of the present invention uses zinc as an auxiliary agent, which plays the dual functions of a structural auxiliary agent and a modulation auxiliary agent. First, by promoting the formation of a three-dimensional ordered macroporous structure, the steric hindrance effect is exerted to avoid the sintering and agglomeration of the active component nickel of the catalyst caused by long-term use. Secondly, the strong acid sites of the zinc-doped catalyst are reduced and the weak acid sites are increased, which reduces the adsorption of ethylene, is beneficial to the ethylene selectivity of the acetylene hydrogenation reaction and improves the service life of the catalyst.
[0029] 3. In the preparation process of the precursor of the present invention, the added 3-aminopropyltriethoxysilane is dispersed between the inorganic and organic interfaces, forming a bonding layer of organic matrix-silane coupling agent-inorganic matrix, which increases the binding force between the template agent polystyrene microspheres and the precursor, and is conducive to obtaining a silicon-aluminum composite oxide carrier with a three-dimensional ordered macroporous structure.
[0030] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION
[0031] The silicon-aluminum composite oxide catalyst with three-dimensional ordered macroporous structure and the preparation method thereof are described in detail through Examples 1 to 9.
[0032] Example 1
[0033] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0034] Step 1: dissolve 37.51 g of aluminum nitrate nonahydrate and 10.42 g of tetraethyl orthosilicate in 11.52 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0035] Step 2: dissolving 0.64 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 2.70 g of deionized water, and stirring to obtain a second solution;
[0036] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.05 g of polystyrene microspheres and 2.21 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:0.5:2.5:3:0.1 by mole fraction;
[0037] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C for 5.5 hours in an air atmosphere to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-1; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.2%.
[0038] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0039] Example 2
[0040] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0041] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0042] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0043] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0044] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C in an air atmosphere for 5.5 hours to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-2; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.2%.
[0045] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0046] Comparative Example 1
[0047] This comparative example comprises the following steps:
[0048] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0049] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0050] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2 and add 4.28 g of polystyrene microspheres to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH=1:2:10:6 in terms of molar fraction;
[0051] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C for 5.5 hours in an air atmosphere to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as PSA-1; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.2%.
[0052] Comparative Example 2
[0053] This comparative example comprises the following steps:
[0054] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0055] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0056] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2 to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH=1:2:10:6 in terms of molar fraction;
[0057] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C for 5.5 hours in an air atmosphere to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as SA-1; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.2%.
[0058] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0059] Example 3
[0060] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0061] Step 1: dissolve 6.88 g of aluminum nitrate nonahydrate and 26.04 g of tetraethyl orthosilicate in 28.79 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0062] Step 2: dissolving 0.70 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 6.76 g of deionized water, and stirring to obtain a second solution;
[0063] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.39 g of polystyrene microspheres and 5.53 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:5:25:15:1 in terms of molar fraction;
[0064] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C in an air atmosphere for 5.5 hours to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-3; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.2%.
[0065] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0066] Example 4
[0067] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0068] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0069] Step 2: dissolving 0.17 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0070] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0071] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C in an air atmosphere for 5.5 hours to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-4; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 0.5%, and the mass content of zinc element is 0.2%.
[0072] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0073] Example 5
[0074] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0075] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0076] Step 2: dissolving 8.33 g of nickel nitrate hexahydrate and 0.08 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0077] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0078] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C for 5.5 hours in an air atmosphere to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-5; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 20%, and the mass content of zinc element is 0.2%.
[0079] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0080] Example 6
[0081] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0082] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0083] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.03 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0084] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0085] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C in an air atmosphere for 5.5 hours to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-6; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.1%.
[0086] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0087] Example 7
[0088] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0089] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0090] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.16 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0091] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 50° C. for 2 h, and age it at room temperature for 2 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0092] Step 4: Dry the gel precursor obtained in step 3 at 100°C for 8h, and then calcine it at 450°C for 3h in an air atmosphere to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-7; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.5%.
[0093] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0094] Example 8
[0095] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0096] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2 with hydrochloric acid to obtain a first solution;
[0097] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.16 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0098] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 70° C. for 5 h, and age it at room temperature of 25° C. for 24 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0099] Step 4: Dry the gel precursor obtained in step 3 at 120°C for 24 hours, and then calcine it at 550°C in an air atmosphere for 6 hours to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-8; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.5%.
[0100] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0101] Example 9
[0102] This embodiment adopts the sol-gel method to prepare the catalyst, and the specific process includes the following steps:
[0103] Step 1: dissolve 18.76 g of aluminum nitrate nonahydrate and 20.83 g of tetraethyl orthosilicate in 23.03 g of anhydrous ethanol, stir evenly, and adjust the pH to 2.5 with hydrochloric acid to obtain a first solution;
[0104] Step 2: dissolving 0.68 g of nickel nitrate hexahydrate and 0.06 g of zinc nitrate hexahydrate in 5.40 g of deionized water, and stirring to obtain a second solution;
[0105] Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2, add 4.28 g of polystyrene microspheres and 4.43 g of 3-aminopropyltriethoxysilane to obtain a third solution, stir the third solution at 60° C. for 3 h, and age it at room temperature of 25° C. for 12 h to obtain a gel precursor; in the third solution, Al:Si:H2O:EtOH:APTES=1:2:10:6:0.4 by mole fraction;
[0106] Step 4: Dry the gel precursor obtained in step 3 at 105°C for 12 hours, and then calcine it at 500°C for 5.5 hours in an air atmosphere to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure, which is granulated for later use and recorded as APSA-9; the mass content of nickel element in the catalyst Zn-Ni-SiO2@Al2O3 is 2%, and the mass content of zinc element is 0.2%.
[0107] The aluminum salt in this embodiment can also be replaced by aluminum chloride hexahydrate, the nickel salt can also be replaced by nickel sulfate hexahydrate, the zinc salt can also be replaced by zinc sulfate heptahydrate, the template agent can also be replaced by polymethyl methacrylate microspheres, and the silane coupling agent can be replaced by vinyl trimethoxy silane.
[0108] The application of the silicon-aluminum composite oxide catalyst with three-dimensional ordered macroporous structure of the present invention is described in detail through Examples 10 to 12.
[0109] Example 10
[0110] The application of this embodiment includes the following steps:
[0111] Step 1, fix 2 g of the catalyst prepared in Example 2 in the constant temperature zone of the reaction tube of the stainless steel high-pressure fixed bed reactor in the order of quartz wool-catalyst-quartz wool, connect the reaction tube and check the air tightness of the system;
[0112] Step 2: Heat the high-pressure fixed-bed reactor checked in step 1 to 300° C. under a nitrogen atmosphere, and then introduce a H2 / N2 mixed gas with a H2 volume content of 10% at a flow rate of 0.1 L / h through a mass flow meter at normal pressure to reduce the catalyst for 2 hours;
[0113] Step 3: introducing a H2S / H2 mixed gas having a H2S volume content of 0.1% into the high-pressure fixed-bed reactor after the reduction in step 2, and sulfurizing the reduced catalyst until the inlet and outlet sulfur contents are equal;
[0114] Step 4: Cool the catalyst after sulfurization in step 3, and then introduce acetylene mixed raw gas for catalytic hydrogenation reaction, and the space velocity of acetylene mixed raw gas is 2000h -1The reaction temperature of the catalytic hydrogenation reaction was 120°C, the reaction pressure was 1.0 MPa, and sampling was performed every 1 hour. The acetylene conversion rate was 99.99% and the ethylene selectivity was 81.43% as determined by gas chromatography.
[0115] Embodiment 11
[0116] The application of this embodiment includes the following steps:
[0117] Step 1, fix 2 g of the catalyst prepared in Example 2 in the constant temperature zone of the reaction tube of the stainless steel high-pressure fixed bed reactor in the order of quartz wool-catalyst-quartz wool, connect the reaction tube and check the air tightness of the system;
[0118] Step 2: Heat the high-pressure fixed-bed reactor checked in step 1 to 380° C. under a nitrogen atmosphere, and then introduce a H2 / N2 mixed gas with a H2 volume content of 10% at a flow rate of 1.8 L / h through a mass flow meter at normal pressure to reduce the catalyst for 4 hours;
[0119] Step 3: introducing a H2S / H2 mixed gas having a H2S volume content of 0.1% into the high-pressure fixed-bed reactor after the reduction in step 2, and sulfurizing the reduced catalyst until the inlet and outlet sulfur contents are equal;
[0120] Step 4: Cool the catalyst after sulfurization in step 3, and then introduce acetylene mixed raw gas for catalytic hydrogenation reaction, and the space velocity of acetylene mixed raw gas is 8000h -1 The reaction temperature of the catalytic hydrogenation reaction was 170°C, the reaction pressure was 1.4 MPa, and sampling was performed every 1 hour. The acetylene conversion rate was 99.99% and the ethylene selectivity was 96.31% as determined by gas chromatography.
[0121] Example 12
[0122] The application of this embodiment includes the following steps:
[0123] Step 1, fix 2 g of the catalyst prepared in Example 2 in the constant temperature zone of the reaction tube of the stainless steel high-pressure fixed bed reactor in the order of quartz wool-catalyst-quartz wool, connect the reaction tube and check the air tightness of the system;
[0124] Step 2: Heat the high-pressure fixed-bed reactor checked in step 1 to 400° C. under a nitrogen atmosphere, and then introduce a H2 / N2 mixed gas with a H2 volume content of 10% at a flow rate of 2.0 L / h through a mass flow meter at normal pressure to reduce the catalyst for 6 hours;
[0125] Step 3: introducing a H2S / H2 mixed gas having a H2S volume content of 0.1% into the high-pressure fixed-bed reactor after the reduction in step 2, and sulfurizing the reduced catalyst until the inlet and outlet sulfur contents are equal;
[0126] Step 4: Cool the catalyst after sulfurization in step 3, and then introduce acetylene mixed raw gas for catalytic hydrogenation reaction, and the space velocity of acetylene mixed raw gas is 10000h -1 The reaction temperature of the catalytic hydrogenation reaction was 220°C, the reaction pressure was 1.8 MPa, and sampling was performed every 1 hour. The acetylene conversion rate was 99.99% and the ethylene selectivity was 93.97% as determined by gas chromatography.
[0127] (I) Catalyst stability evaluation
[0128] The stability of the silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure prepared by the present invention was tested. The specific process is: the catalyst is reduced and sulfurized according to steps 1 to 3 in Example 11, and then the feed system is balanced at 150°C, the temperature is raised to 300°C and acetylene mixed raw material gas is introduced for catalytic hydrogenation reaction for 5 hours, and then the temperature is lowered to 150°C to examine the change in catalyst performance after high-temperature catalytic hydrogenation reaction; then the feed is continuously fed for 500 hours to examine the service life of the catalyst. The results show that after the high-temperature catalytic hydrogenation reaction, the acetylene conversion rate and ethylene selectivity of the catalyst are basically not reduced, and it still has a high catalytic activity; after continuous feeding for 500 hours, the acetylene conversion rate of the catalyst is basically not reduced, and the ethylene selectivity is only reduced by less than 0.2%, which shows that the catalyst of the present invention has good stability.
[0129] (II) Evaluation of catalytic hydrogenation activity
[0130] The stability of the silicon-aluminum composite oxide catalyst Zn-Ni-SiO2@Al2O3 with a three-dimensional ordered macroporous structure prepared by the present invention was tested. The specific process is: the catalysts of Examples 1 to 9 and Comparative Examples 1 to 2 were subjected to the application process in Example 11. The acetylene conversion rate and ethylene selectivity detected by gas chromatography are shown in Table 1 below.
[0131] Table 1
[0132]
[0133]
[0134] As can be seen from Table 1, the acetylene conversion rates of the catalysts prepared in Examples 1 to 8 of the present invention are all above 98%, and the ethylene selectivity is all above 86%. At the same time, compared with the catalyst prepared in Comparative Example 1 without adding a silane coupling agent, the acetylene conversion rate of the catalyst prepared in Example 2 is equivalent, but the ethylene selectivity is improved, indicating that the silane coupling agent added in the present invention is dispersed between the inorganic and organic interfaces, forming a bonding layer of an organic matrix-silane coupling agent-inorganic matrix, increasing the bonding force between the template agent and the precursor, and facilitating the formation of a three-dimensional ordered macroporous structure, thereby improving the ethylene selectivity. Compared with the catalyst prepared in Comparative Example 2 without adding template agent and silane coupling agent, the acetylene conversion rate of the catalyst prepared in Example 2 is equivalent, but the ethylene selectivity is significantly improved, indicating that the catalyst is conducive to obtaining a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure by adding template agent and silane coupling agent. The catalyst is supported by a three-dimensional ordered macroporous structure, which provides sufficient space for the adsorption and desorption of acetylene and ethylene. At the same time, the active components are coated in the pore structure and are not easy to sinter and agglomerate, thereby avoiding the phenomenon of excessive hydrogenation and polymerization of ethylene during the catalytic process, thereby significantly improving the ethylene selectivity.
[0135] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure, It is characterized in that The catalyst is prepared by the sol-gel method, and the specific process includes the following steps: Step 1, dissolving aluminum salt and tetraethyl silicate in anhydrous ethanol and adjusting the pH with hydrochloric acid to obtain a first solution; Step 2, dissolving nickel salt and zinc salt in deionized water to obtain a second solution; Step 3: Mix the first solution obtained in step 1 with the second solution obtained in step 2 and add a template agent and a silane coupling agent to obtain a third solution, and continuously stir the third solution and age it to obtain a gel precursor; Step 4: Dry the gel precursor obtained in step 3 and calcine it in an oxygen environment to obtain a silicon-aluminum composite oxide catalyst Zn-Ni-SiO 2 @Al 2 O 3 .
2. The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure according to claim 1, It is characterized in that The aluminum salt described in step one is aluminum nitrate nonahydrate or aluminum chloride hexahydrate; the nickel salt described in step two is nickel nitrate hexahydrate or nickel sulfate hexahydrate, and the zinc salt is zinc nitrate hexahydrate or zinc sulfate heptahydrate; the template agent described in step three is polystyrene microspheres or polymethyl methacrylate microspheres, and the silane coupling agent is 3-aminopropyltriethoxysilane or vinyltrimethoxysilane.
3. The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure according to claim 1, It is characterized in that In step 1, hydrochloric acid is used to adjust the pH to 2-2.
5.
4. The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure according to claim 1, It is characterized in that In the third solution in step 3, Al:Si:H 2 O:EtOH:APTES=1:0.5~5:2.5~25:3~15:0.1~1.
5. The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure according to claim 1, It is characterized in that The continuous stirring time in step 3 is 2h to 5h, and the temperature is 50°C to 70°C; the aging temperature is room temperature, and the time is 2h to 24h.
6. The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure according to claim 1, It is characterized in that The drying temperature in step 4 is 100° C. to 120° C., and the time is 8 h to 24 h. The calcination temperature is 450° C. to 550° C., and the time is 3 h to 6 h.
7. The method for preparing a silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure according to claim 1, It is characterized in that The catalyst Zn-Ni-SiO 2 @Al 2 O 3 The mass content of nickel element is 0.5% to 20%, and the mass content of zinc element is 0.1% to 0.5%.
8. A silicon-aluminum composite oxide catalyst with a three-dimensional ordered macroporous structure, It is characterized in that The method is prepared by any one of claims 1 to 7.
9. Use of a silicon-aluminum composite oxide catalyst having a three-dimensional ordered macroporous structure as claimed in claim 8, It is characterized in that The application includes the following steps: Step 1: fix the catalyst in the constant temperature zone of the high pressure fixed bed reactor and check the air tightness of the system; Step 2: Heat the high-pressure fixed-bed reactor checked in step 1 to 300°C to 400°C under a nitrogen atmosphere, and then introduce H at a flow rate of 0.1L / h to 2L / h under normal pressure. 2 The volume content of H is 10% 2 / N 2 The mixed gas reduces the catalyst; Step 3: introducing H into the high pressure fixed bed reactor after the reduction in step 2 2 S volume content of 0.1% H 2 S / H 2 Mixed gas, sulfiding the reduced catalyst; Step 4: Cool the catalyst after sulfurization in step 3, and then introduce acetylene mixed raw gas for catalytic hydrogenation reaction, and the space velocity of acetylene mixed raw gas is 2000h -1 ~10000h -1 The reaction temperature of the catalytic hydrogenation reaction is 120°C to 220°C, and the reaction pressure is 1.0MPa to 1.8MPa.