Preparation method of CdSe-CuInSe2 composite material for photocatalytic hydrogen production and synchronous degradation of pollutants
By simplifying the preparation method of CdSe and CuInSe2, combining the high-temperature reaction of precursors of cadmium and selenium and the precursors of Cu and indium, CdSe-CuInSe2 composite materials are prepared, which solves the problems of high production cost and cumbersome steps in the prior art. It has achieved efficient photocatalytic hydrogen production and pollutant degradation capabilities.
Patent Information
- Application Number
- CN202411252808.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
The existing preparation methods of CdSe and CuInSe2 are costly and cumbersome, and are not suitable for large-scale production and application. They lack simple and low-cost composite preparation methods to achieve the ability of photocatalytic hydrogen production to synchronously degrade pollutants.
The precursor of cadmium and selenium source are heated under stirring, then insulated and cooled at high temperatures. The precursor of Cu and the precursor of indium react under the protection of inert gas, and is treated by 3-mercaptopropionic acid and finally dried in vacuum. The CdSe-CuInSe2 composite material was prepared under conditions, which simplified the preparation process and reduced the cost.
The prepared CdSe-CuInSe2 photocatalyst has a high specific surface area, multiple active sites and channels, and exhibits excellent photocatalytic properties. It can effectively degrade rhodamine B while producing hydrogen. The preparation method is simple and low-cost.
Smart Images

Figure CN119034765A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalyst preparation, and specifically relates to a method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and synchronous degradation of pollutants. Background Art
[0002] In recent years, the over-exploitation of fossil minerals and the rapid development of industrialization have caused energy shortages and environmental pollution. Photocatalytic technology converts inexhaustible solar energy into storable chemical energy, providing an effective method to solve the above problems. Hydrogen energy has become one of the alternative energy sources to fossil energy due to its wide source, clean, efficient and environmentally friendly advantages. The use of semiconductor materials for photocatalytic water decomposition to produce hydrogen is one of the effective ways to achieve the conversion of solar energy into light energy. In the photocatalytic reaction, the oxidation and reduction properties are used simultaneously to degrade pollutants while photocatalytically producing hydrogen from water, which has attracted widespread attention. Yu et al. successfully prepared g-C3N4 / BiVO4, which can degrade ofloxacin (OFL) wastewater while producing hydrogen (Separation and Purification Technology 335 (2024) 126201). Semiconductor photocatalytic technology provides a new research idea for alleviating the current energy crisis and environmental pollution.
[0003] The development of highly active and stable photocatalysts is the key to improving photocatalytic activity. At present, a large number of transition metal catalysts have been widely used, such as titanium dioxide, zinc oxide, carbon nitride and cadmium sulfide. Among them, cadmium sulfide has a good driving force for hydrogen evolution reaction and the ability to degrade pollutants due to its suitable band gap and visible light response ability, but its high carrier recombination rate, photocorrosion and instability under light limit its application (Advanced Fiber Materials, 2022, 4(5): 1094-1107). CdSe, as a transition metal selenide, has similar optical properties to cadmium sulfide. However, since sulfur and selenium are in different periods, selenium has a larger atomic radius than sulfur, stronger metallicity than sulfur, and less ionization energy than sulfur. These characteristics make CdSe's photoelectric properties better than CdS. Therefore, the advantages of suitable band gap, excellent photoelectric performance and visible light response ability have made CdSe receive more and more attention in the field of photocatalysis (Journal of Materials Science & Technology, 2023, 137:223-231). CuInSe2 nanoparticles have strong light absorption ability and good photostability (Dalton Transactions, 2020, 6(7): 1543-1559). Using CuInSe2 as a co-catalyst can effectively promote the transfer of photogenerated carriers, inhibit the recombination of photogenerated carriers, provide more photocatalytic active sites and active channels, thereby effectively improving the photocatalytic performance. At present, the preparation methods of CdSe and CuInSe2 include hydrothermal method, vapor deposition method, anion exchange method, two-step hydrothermal calcination method and one-pot solvent thermal method; the preparation methods of composite materials include in-situ composite and post-situ composite. However, the current methods for preparing CdSe and CuInSe2 require high costs and complicated steps, which is not conducive to large-scale production and application. Therefore, it is of great significance to develop a method for preparing CdSe and CuInSe2 nanophotocatalytic materials with simple and low cost, and to composite the two by a simple and easy-to-operate method. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and simultaneous degradation of pollutants. The prepared CdSe-CuInSe2 photocatalyst has excellent photocatalytic hydrogen production and degradation capabilities of Rhodamine B, and has the advantages of low production cost, simple and easy operation, and high material stability.
[0005] The technical solution of the present invention is: a method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and simultaneous degradation of pollutants, characterized in that it comprises the following steps: (1) Add the cadmium precursor and selenium source into a reaction vessel, add 20-45 mL of solvent, and then heat to 50-80 °C with stirring for 40-90 min; (2) Transfer the mixed solution in step (1) into a reaction vessel, keep it at 120-180°C for 10-16 hours, and cool it naturally to room temperature; (3) centrifuging the product in step (2), washing the precipitate with deionized water and ethanol, and then vacuum drying at 40-80° C. for 4-12 h to obtain a CdSe nanosheet photocatalyst; (4) Add Cu precursor, indium precursor and 5-10 ml reaction solvent into the reaction vessel in proportion, and keep the temperature at 60-80 °C for 1-14 h in an inert gas atmosphere; (5) Add the selenium source and 20-35 ml of solvent into the reaction vessel, keep the temperature at 40-70 °C for 5-30 min, then raise the temperature to 260-290 °C and keep the temperature for 25-60 min. The entire reaction is carried out under the protection of inert gas. (6) injecting the mixed solution in step (4) into the mixed solution in step (5), and after the whole reaction temperature drops to 60-80°C, rapidly raising the temperature to 220-270°C and keeping the temperature for 0.5-1.5 h. The whole reaction is carried out under inert gas; (7) The mixed solution in step (6) is post-treated with a 3-mercaptopropionic acid (MPA) aqueous solution, the solution after the reaction is centrifuged, the precipitate is washed with ethanol, and then vacuum dried at 40-80° C. for 4-12 h to obtain a CuInSe2 photocatalyst; (8) Add the CdSe nanosheet photocatalyst prepared in step (3) to 20-60 ml of ethanol, and then add the CuInSe2 photocatalyst prepared in step (7). Stir for 8-24 h and then centrifuge. Wash the precipitate with deionized water and ethanol, and then vacuum dry at 40-80 °C for 4-12 h to obtain a CdSe-CuInSe2 composite material.
[0006] Preferably, the cadmium precursor in step (1) is selected from cadmium acetate, cadmium chloride, and cadmium sulfate, which have stable chemical properties and abundant raw materials; the selenium source can be selected from selenium powder: easy to obtain and widely applicable, sodium selenite: with good stability and solubility, or selenium dioxide: high purity and strong controllability.
[0007] Preferably, the solvent in step (1) is diethylenetriamine or triethylenetetramine, which can not only effectively dissolve and stabilize metal precursors as solvents, but also play an important role as templates and crystal regulation in the synthesis of nanomaterials. They are also environmentally friendly and degradable, which makes them potential in green chemistry and environmentally friendly synthesis.
[0008] Preferably, the solvent in steps (4) and (5) is an alkylamine, which may be oleylamine, dodecylamine or hexadecylamine. Alkylamine has good solubility, structural flexibility, relatively low toxicity and safety, and is a common and valuable choice in many chemical reactions.
[0009] Preferably, the inert gas in steps (4), (5) and (6) is nitrogen or argon. The introduction of the inert gas helps to prevent product oxidation, increase product yield, maintain stable reaction conditions and ensure the safety and stability of the reaction process.
[0010] Preferably, the reaction container in steps (1), (4) and (5) is a three-necked flask or a four-necked flask.
[0011] Preferably, the reactor in step (2) is a Teflon reactor; the Teflon reactor is suitable for reactions in chemical media with high pH, especially in highly corrosive media. At the same time, its temperature resistance range is between -80°C and 200°C, and it has excellent anti-stickiness and high-temperature stability, and is suitable for reactions in harsh environments such as high temperature and high pressure.
[0012] Preferably, in step (4), the Cu precursor, the indium precursor and 5-10 ml of the reaction solvent are added in percentage by mass.
[0013] Preferably, by adjusting the mass percentage of CuInSe2, CdSe-x%CuInSe2 with different ratios is prepared, where x represents the mass percentage of CuInSe2 in the composite material. This method is simple and can effectively increase the number of active sites and active channels, thereby improving the photocatalytic performance.
[0014] The beneficial effects of the present invention are as follows: the preparation method provided by the present invention has the advantages of simple preparation method, low cost and easy control of reaction conditions. The prepared photocatalyst has the characteristics of high specific surface area, more active sites and channels, excellent photocatalytic performance and recyclability. At the same time, during the photocatalytic reaction, oxidation and reduction reactions can be effectively utilized to achieve the degradation of rhodamine B while producing hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1XRD patterns of the CdSe-CuInSe2 catalysts prepared in Examples 1-4 (Example 1 is CdSe-2%CuInSe2, Example 2 is CdSe-5%CuInSe2, Example 3 is CdSe-8%CuInSe2, and Example 4 is CdSe-11%CuInSe2), with the horizontal axis being the 2θ diffraction angle and the vertical axis being the diffraction intensity.
[0016] Figure 2 This is a transmission electron microscope (TEM) image of the CdSe-8%CuInSe2 catalyst prepared in Example 3.
[0017] Figure 3 This is a high resolution electron microscope (HRTEM) image of the CdSe-8%CuInSe2 catalyst prepared in Example 3.
[0018] Figure 4 UV-visible absorption spectra of CdSe, CdSe-CuInSe2, and CuInSe2 catalysts prepared in Example 3.
[0019] Figure 5 The performance diagram of the photocatalytic hydrogen production and synergistic degradation of Rhodamine B by the CdSe-8%CuInSe2 catalyst prepared in Example 3, where the left ordinate is the hydrogen release rate (μmol·g -1 ·h -1 ), the right vertical axis is the degradation rate of Rhodamine B (%). DETAILED DESCRIPTION
[0020] The present invention is further described in detail below in conjunction with specific embodiments. However, the protection scope of the present invention is not limited to the described scope. Example
[0021] A method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and simultaneous degradation of pollutants comprises the following steps: 0.9 mmol cadmium acetate and 0.9 mmol selenium dioxide are dispersed in 38 mL diethylenetriamine by ultrasonic treatment. The mixture is then heated to 5 °C while stirring and maintained for 60 min. The solution is then transferred to a Teflon reactor. The mixture is heated at 140 °C for 15 h and then cooled to room temperature. The resulting product is collected by centrifugation, washed several times with deionized water and ethanol in a ratio of 1:1, and finally dried under vacuum at 6 °C for 8 hours to obtain CdSe nanosheets.
[0022] Weigh 1 mmol of cuprous chloride and 1 mmol of indium chloride into a three-necked flask, add 10 mL of oleylamine, and then transfer to an electric heating mantle and keep it at 80 °C for 4 hours in an argon-filled environment. Weigh 2 mmol of selenium powder into a three-necked flask, add 25 mL of oleylamine, heat to 60 °C and keep it for 10 min, then heat it to 280 °C. After keeping it for 45 min, inject the mixed solution of cuprous chloride and indium chloride into the hot selenium-based solution by hot injection. When the temperature of the entire mixed solution drops to 60 °C, quickly heat it to 240 °C and keep it for 1 h. The entire reaction is carried out under an argon atmosphere. After cooling to room temperature, collect the product, wash it three times with a mixed solution of n-hexane and anhydrous ethanol, and then dry it under vacuum at 60 °C for 8 h. The dried sample was dispersed in 10 mL of toluene and 10 mL of MPA aqueous solution (1 mL of 3-mercaptopropionic acid and 9 mL of pure water), vigorously stirred for 5 h, and then washed three times by centrifugation with ethanol. Finally, it was dried under vacuum at 60 °C for 8 h to obtain CuInSe2 nanoparticles.
[0023] 98 mg of CdSe was weighed and dispersed in 30 mL of ethanol, and then 2 mg of CuInSe2 was added to the suspension and ultrasonicated for 15 min. After strong stirring for 24 h, the precipitate obtained by centrifugation was vacuum dried at 60 °C for 8 h to obtain the CdSe-2%CuInSe2 photocatalyst.
[0024] The performance evaluation method of the catalyst for photocatalytic hydrogen production and photocatalytic degradation of rhodamine B is as follows: 30 mg of the above photocatalyst is dispersed in 60 mL of sacrificial agent solution containing rhodamine B and stirred in the dark for 30 min to reach adsorption-desorption equilibrium. Then it is transferred to the automatic sampling trace gas analysis system, and the reaction system is degassed with a vacuum pump to remove the air in the suspension. The temperature of the suspension is stabilized at 6 °C by circulating cooling water. Subsequently, a 300 W Xe lamp with a 400 nm cutoff filter is used to irradiate vertically at a distance of 3 cm from the bottle mouth for photocatalytic reaction, and the H2 generation rate of the reaction system is automatically determined every 30 min by a gas chromatograph. 2 to 5 ml of the solution is taken out before and after the start of illumination, and the concentration of rhodamine B is determined by UV-visible spectrophotometry, and the degradation rate of rhodamine B by the catalyst is calculated according to the concentration. Figure 1 The X-ray diffraction pattern of CdSe-2%CuInSe2 is shown. Figure 4 Shows the UV-visible absorption spectrum of CdSe-2%CuInSe2 nanophotocatalyst. Example
[0025] A method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and simultaneous degradation of pollutants comprises the following steps: 0.9 mmol cadmium acetate and 0.9 mmol selenium dioxide are dispersed in 38 mL diethylenetriamine by ultrasonic treatment. The mixture is then heated to 5 °C while stirring and maintained for 60 min. The solution is then transferred to a Teflon reactor. The mixture is heated at 140 °C for 15 h and then cooled to room temperature. The resulting product is collected by centrifugation, washed several times with deionized water and ethanol in a ratio of 1:1, and finally dried under vacuum at 6 °C for 8 h to obtain CdSe nanosheets.
[0026] Weigh 1 mmol of cuprous chloride and 1 mmol of indium chloride into a three-necked flask, add 10 mL of oleylamine, then transfer to an electric heating mantle and keep warm at 80 °C for 4 h in an argon-filled environment. Weigh 2 mmol of selenium powder into a three-necked flask, add 25 mL of oleylamine, heat to 60 °C and keep warm for 10 min, then heat to 280 °C, and after keeping warm for 45 min, inject the mixed solution of cuprous chloride and indium chloride into the hot selenium-based solution by hot injection. When the temperature of the entire mixed solution drops to 60 °C, quickly heat to 240 °C and keep warm for 1 h. The entire reaction is carried out under an argon atmosphere. After cooling to room temperature, collect the product, wash it three times with a mixed solution of n-hexane and anhydrous ethanol, and then dry it under vacuum at 60 °C for 8 h. The dried sample was dispersed in 10 mL of toluene and 10 mL of MPA aqueous solution (1 mL of 3-mercaptopropionic acid and 9 mL of pure water), vigorously stirred for 5 h, and then washed three times by centrifugation with ethanol. Finally, it was dried under vacuum at 60 °C for 8 h to obtain CuInSe2 nanoparticles.
[0027] 95 mg of CdSe was weighed and dispersed in 30 mL of ethanol, and then 5 mg of CuInSe2 was added to the suspension and ultrasonicated for 15 min. After strong stirring for 24 h, the precipitate obtained by centrifugation was dried under vacuum at 60 °C for 8 h to obtain the CdSe-2%CuInSe2 photocatalyst.
[0028] The performance evaluation method of the catalyst for photocatalytic hydrogen production and photocatalytic degradation of rhodamine B is as follows: 30 mg of the above photocatalyst is dispersed in 60 mL of sacrificial agent solution containing rhodamine B and stirred in the dark for 30 min to reach adsorption-desorption equilibrium. Then it is transferred to the automatic sampling trace gas analysis system, and the reaction system is degassed with a vacuum pump to remove the air in the suspension. The temperature of the suspension is stabilized at 6 °C by circulating cooling water. Subsequently, a 300 W Xe lamp with a 400 nm cutoff filter is used to irradiate vertically at a distance of 3 cm from the bottle mouth for photocatalytic reaction, and the H2 generation rate of the reaction system is automatically determined every 30 min by a gas chromatograph. 2 to 5 ml of the solution is taken out before and after the start of illumination, and the concentration of rhodamine B is determined by UV-visible spectrophotometry, and the degradation rate of rhodamine B by the catalyst is calculated according to the concentration. Figure 1 The X-ray diffraction pattern of CdSe-5%CuInSe2 is shown. Figure 4 Shows the UV-visible absorption spectrum of CdSe-5%CuInSe2 nanophotocatalyst. Example
[0029] A method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and simultaneous degradation of pollutants comprises the following steps: 0.9 mmol cadmium acetate and 0.9 mmol selenium dioxide are dispersed in 38 mL diethylenetriamine by ultrasonic treatment. The mixture is then heated to 5 °C while stirring and maintained for 60 min. The solution is then transferred to a Teflon reactor. The mixture is heated at 140 °C for 15 h and then cooled to room temperature. The resulting product is collected by centrifugation, washed several times with deionized water and ethanol in a ratio of 1:1, and finally dried under vacuum at 6 °C for 8 h to obtain CdSe nanosheets.
[0030] Weigh 1 mmol of cuprous chloride and 1 mmol of indium chloride into a three-necked flask, add 10 mL of oleylamine, and then transfer to an electric heating mantle and keep it at 80 °C for 4 h in an argon-filled environment. Weigh 2 mmol of selenium powder into a three-necked flask, add 25 mL of oleylamine, heat to 60 °C and keep it for 10 min, then heat to 280 °C, and after keeping it for 45 min, inject the mixed solution of cuprous chloride and indium chloride into the hot selenium-based solution by hot injection. When the temperature of the entire mixed solution drops to 60 °C, quickly heat it to 240 °C and keep it for 1 h. The entire reaction is carried out under an argon atmosphere. After cooling to room temperature, collect the product, wash it three times with a mixed solution of n-hexane and anhydrous ethanol, and then dry it under vacuum at 60 °C for 8 h. The dried sample was dispersed in 10 mL of toluene and 10 mL of MPA aqueous solution (1 mL of 3-mercaptopropionic acid and 9 mL of pure water), vigorously stirred for 5 h, and then washed three times by centrifugation with ethanol. Finally, it was dried under vacuum at 60 °C for 8 h to obtain CuInSe2 nanoparticles.
[0031] 92 mg of CdSe was weighed and dispersed in 30 mL of ethanol, and then 8 mg of CuInSe2 was added to the suspension and ultrasonicated for 15 min. After strong stirring for 24 h, the precipitate obtained by centrifugation was vacuum dried at 60 °C for 8 h to obtain the CdSe-2%CuInSe2 photocatalyst.
[0032] The performance evaluation method of the catalyst for photocatalytic hydrogen production and photocatalytic degradation of rhodamine B is as follows: 30 mg of the above photocatalyst is dispersed in 60 mL of sacrificial agent solution containing rhodamine B and stirred in the dark for 30 min to reach adsorption-desorption equilibrium. Then it is transferred to the automatic sampling trace gas analysis system, and the reaction system is degassed with a vacuum pump to remove the air in the suspension. The temperature of the suspension is stabilized at 6 °C by circulating cooling water. Subsequently, a 300 W Xe lamp with a 400 nm cutoff filter is used to irradiate vertically at a distance of 3 cm from the bottle mouth for photocatalytic reaction, and the H2 generation rate of the reaction system is automatically determined every 30 min by a gas chromatograph. 2 to 5 ml of the solution is taken out before and after the start of illumination, and the concentration of rhodamine B is determined by UV-visible spectrophotometry, and the degradation rate of rhodamine B by the catalyst is calculated according to the concentration. Figure 1 The X-ray diffraction pattern of CdSe-8%CuInSe2 is shown. Figure 2 Shows the microscopic morphology (TEM) of CdSe-8%CuInSe2 nanophotocatalyst. Figure 2 Shows the high-resolution image (HRTEM) of CdSe-8%CuInSe2 nanophotocatalyst. Figure 4 Shows the UV-visible absorption spectrum of CdSe-8%CuInSe2 nanophotocatalyst. Figure 5 The nanophotocatalytic hydrogen production rate of CdSe-8%CuInSe2 nanophotocatalyst and the degradation rate of Rhodamine B are shown. After 2 h of illumination, the hydrogen production rate is 6795.77 μmol·g -1 ·h -1 , the degradation rate of rhodamine was 86%. Example
[0033] A method for preparing a CdSe-CuInSe2 composite material for photocatalytic hydrogen production and simultaneous degradation of pollutants comprises the following steps: 0.9 mmol cadmium acetate and 0.9 mmol selenium dioxide are dispersed in 38 mL diethylenetriamine by ultrasonic treatment. The mixture is then heated to 5 °C while stirring and maintained for 60 min. The solution is then transferred to a Teflon reactor. The mixture is heated at 140 °C for 15 h and then cooled to room temperature. The resulting product is collected by centrifugation, washed several times with deionized water and ethanol in a ratio of 1:1, and finally dried under vacuum at 6 °C for 8 h to obtain CdSe nanosheets.
[0034] Weigh 1 mmol of cuprous chloride and 1 mmol of indium chloride into a three-necked flask, add 10 mL of oleylamine, and then transfer to an electric heating mantle and keep it at 80 °C for 4 h in an argon-filled environment. Weigh 2 mmol of selenium powder into a three-necked flask, add 25 mL of oleylamine, heat to 60 °C and keep it for 10 min, then heat to 280 °C, and after keeping it for 45 min, inject the mixed solution of cuprous chloride and indium chloride into the hot selenium-based solution by hot injection. When the temperature of the entire mixed solution drops to 60 °C, quickly heat it to 240 °C and keep it for 1 h. The entire reaction is carried out under an argon atmosphere. After cooling to room temperature, collect the product, wash it three times with a mixed solution of n-hexane and anhydrous ethanol, and then dry it under vacuum at 60 °C for 8 h. The dried sample was dispersed in 10 mL of toluene and 10 mL of MPA aqueous solution (1 mL of 3-mercaptopropionic acid and 9 mL of pure water), vigorously stirred for 5 h, and then washed three times by centrifugation with ethanol. Finally, it was dried under vacuum at 60 °C for 8 h to obtain CuInSe2 nanoparticles.
[0035] 89 mg of CdSe was weighed and dispersed in 30 mL of ethanol, and then 11 mg of CuInSe2 was added to the suspension and ultrasonicated for 15 min. After strong stirring for 24 h, the precipitate obtained by centrifugation was vacuum dried at 60 °C for 8 h to obtain the CdSe-2%CuInSe2 photocatalyst.
[0036] The performance evaluation method of the catalyst for photocatalytic hydrogen production and photocatalytic degradation of rhodamine B is as follows: 30 mg of the above photocatalyst is dispersed in 60 mL of sacrificial agent solution containing rhodamine B and stirred in the dark for 30 min to reach adsorption-desorption equilibrium. Then it is transferred to the automatic sampling trace gas analysis system, and the reaction system is degassed with a vacuum pump to remove the air in the suspension. The temperature of the suspension is stabilized at 6 °C by circulating cooling water. Subsequently, a 300 W Xe lamp with a 400 nm cutoff filter is used to irradiate vertically at a distance of 3 cm from the bottle mouth for photocatalytic reaction, and the H2 generation rate of the reaction system is automatically determined every 30 min by a gas chromatograph. 2 to 5 ml of the solution is taken out before and after the start of illumination, and the concentration of rhodamine B is determined by UV-visible spectrophotometry, and the degradation rate of rhodamine B by the catalyst is calculated according to the concentration. Figure 1 The X-ray diffraction pattern of CdSe-11%CuInSe2 is shown. Figure 4 Shows the UV-visible absorption spectrum of CdSe-11%CuInSe2 nanophotocatalyst.
Claims
1. A CdSe-CuInSe for Photocatalytic Hydrogen Production and Simultaneous Pollutant Degradation 2 A method for preparing a composite material, It is characterized in that The following steps are involved: (1) Add the cadmium precursor and selenium source into a reaction vessel, add 20-45 mL of solvent, and then heat to 50-80 °C with stirring for 40-90 min; (2) Transfer the mixed solution in step (1) into a reaction vessel, keep it at 120-180°C for 10-16 hours, and cool it naturally to room temperature; (3) centrifuging the product in step (2), washing the precipitate with deionized water and ethanol, and then vacuum drying at 40-80 °C for 4-12 h to obtain a CdSe nanosheet photocatalyst; (4) Add Cu precursor, indium precursor and 5-10 ml reaction solvent into the reaction vessel in proportion, and keep the temperature at 60-80 °C for 1-14 h in an inert gas atmosphere; (5) Add the selenium source and 20-35 ml of solvent into the reaction vessel, keep the temperature at 40-70 °C for 5-30 min, then raise the temperature to 260-290 °C and keep the temperature for 25-60 min. The entire reaction is carried out under the protection of inert gas. (6) injecting the mixed solution in step (4) into the mixed solution in step (5), and after the whole reaction temperature drops to 60-80°C, rapidly raising the temperature to 220-270°C and keeping the temperature for 0.5-1.5 h. The whole reaction is carried out under inert gas; (7) The mixed solution in step (6) is post-treated with an aqueous solution of 3-mercaptopropionic acid (MPA), the solution after the reaction is centrifuged, the precipitate is washed with ethanol, and then vacuum dried at 40-80 °C for 4-12 h; CuInSe is obtained. 2 Photocatalysts; (8) Add the CdSe nanosheet photocatalyst prepared in step (3) to 20-60 ml of ethanol, and then add the CuInSe prepared in step (7). 2 The photocatalyst was stirred for 8-24 h and then centrifuged. The precipitate was washed with deionized water and ethanol and then vacuum dried at 40-80 °C for 4-12 h to obtain CdSe-CuInSe 2 Composite materials.
2. A CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: In the step (1), the cadmium precursor is selected from any one of cadmium acetate, cadmium chloride, cadmium sulfate or a mixture thereof; the selenium source is selected from any one of selenium powder, sodium selenite or selenium dioxide or a mixture thereof.
3. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: The solvent in step (1) is diethylenetriamine or triethylenetetramine.
4. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: The solvent in steps (4) and (5) is alkylamine, oleylamine, dodecylamine or hexadecylamine.
5. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: The inert gas in steps (4), (5) and (6) is nitrogen or argon.
6. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: The reaction container in steps (1), (4) and (5) is a three-necked flask or a four-necked flask.
7. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: The reactor in step (2) is a Teflon reactor.
8. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: In the step (4), the Cu precursor, the indium precursor and 5-10 ml of the reaction solvent are added according to mass percentage.
9. The CdSe-CuInSe for photocatalytic hydrogen production and simultaneous degradation of pollutants according to claim 1 2 A method for preparing a composite material, Features: By adjusting CuInSe 2 The mass ratio of CdSe-x%CuInSe was prepared 2 , x represents CuInSe 2 The mass percentage in the composite material.