Catalyst for synthesizing lubricant base oil and preparation method thereof
Through heteroatom doping of rare earth metals and phosphorus-supported modified Y molecular sieve alkylation catalysts, the problems of catalysts being easily deactivated and environmental pollution in alkylnaphthalene synthesis are solved, and the high selectivity of single-substituted long-chain alkylnaphthalenes is achieved Synthesis and excellent properties, and the catalyst can be recycled.
Patent Information
- Application Number
- CN202411214663.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-02
AI Technical Summary
In the prior art, the synthesis catalyst of alkyl naphthalene has problems such as equipment corrosion, difficulty in separation of products, environmental pollution, easy deactivation of solid acid catalysts, short reaction life and inability to synthesize single-substituted long-chain alkyl naphthalene with high selectivity.
Using a modified Y molecular sieve alkylation catalyst with heteroatom doping rare earth metals and phosphorus-supported phosphorus, the alkylation catalyst with excellent properties was prepared by hydrothermal synthesis and post-treatment modification, and used to synthesize single-substituted long-chain alkyl groups. Naphthalene.
Achieve high selective synthesis of alkyl naphthalene, improve the service life and stability of the catalyst, avoid equipment corrosion and environmental pollution, and improve the thermal oxygen stability and viscosity of the product. The catalyst can be regenerated through simple hydrothermal roasting. .
Smart Images

Figure CN119034793A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lubricant base oil synthesis, and in particular relates to a catalyst for lubricant base oil synthesis and a preparation method thereof. Background Art
[0002] Mineral base oils are widely used in the field of lubricants, accounting for 95% of the lubricant market in China. However, due to their poor thermal stability and oxidation stability, they cannot meet the requirements of the high-end lubricant market. Synthetic base oils are a good supplement to the lubricant market. Common synthetic base oils include Class IV lubricant polyalphaolefins (PAO) and Class V lubricant alkyl naphthalene. Compared with mineral base oils, synthetic base oils have better low-temperature fluidity, higher oxidation stability, thermal stability, lower evaporation loss rate and good additive solubility. As a Class V lubricant, alkyl naphthalene base oil has more outstanding oxidation stability and additive solubility advantages compared to other synthetic base oils. Alkyl naphthalene has broad application prospects. It can be used as a base oil alone or as an additive to mineral oil base oils and other synthetic base oils. It is mainly used in high-end lubricants and greases.
[0003] Long-chain alkylnaphthalene is mainly synthesized by the Friedel-Crafts reaction of naphthalene and long-chain α-olefins. Commonly used catalysts include inorganic acid catalysts and Lewis acid catalysts.
[0004] Long-chain alkylnaphthalene is mainly produced by the alkylation reaction of naphthalene. Commonly used alkylating agents include long-chain α-olefins, halogenated alkanes, alcohols, etc. Using long-chain α-olefins as alkylating agents, the base oil products obtained have better properties. Commonly used alkylation catalysts include inorganic acids (concentrated sulfuric acid, HF, etc.) and Lewis acids (AlCl3, ZnCl2, FeCl3, etc.). These catalysts have problems such as corrosion of equipment, serious environmental pollution, and difficulty in separating products and raw materials.
[0005] U.S. Patent No. 4,714,794 describes that monosubstituted alkylnaphthalene has excellent thermal oxygen stability, low vapor pressure and low flash point, good low temperature fluidity and high heat transfer capacity, and is very suitable for use as a lubricant base oil. U.S. Patent Nos. 4,604,491, 4,211,665, and 4,238,343 describe the use of a mixture of monosubstituted alkylnaphthalene and polysubstituted alkylnaphthalene as a lubricant base oil. The most preferred alkylnaphthalene is monosubstituted alkylnaphthalene, which has the best performance. For example, compared with polysubstituted alkylnaphthalene, monosubstituted alkylnaphthalene has better thermal stability and oxidation stability, and therefore can be used as a better lubricant base oil or additive. Lubricant viscosity that is too high or too low will increase wear between mechanical devices, and having a C 14 ~C 18The kinematic viscosity of monosubstituted alkylnaphthalene at 100°C is 5-8 cst, which is within the optimal range. The currently used alkylation catalysts have poor selectivity and cannot synthesize long-chain monosubstituted alkylnaphthalene with high selectivity.
[0006] US Patent US4604491 uses activated silica alumina as an alkylation catalyst to produce long-chain alkyl naphthalene by alkylation reaction of naphthalene and α-olefin (monoolefin or mixed olefin). The reaction needs to be reacted at 200°C for 6 hours. The reaction time is too long and the reaction temperature is too high, which consumes a lot of energy and is difficult to separate the product. At present, there are many aspects of solid acid catalysts that need to be improved, such as olefin polymerization byproducts that easily block the molecular sieve channels and deactivate the catalyst, and there are also problems such as dark product color, complicated preparation and modification of solid acid catalysts, and insufficient catalyst life. Chinese patent CN1029611C uses loaded heteropolyacids and their salts as alkylation catalysts. The reaction needs to be carried out in a pressurized closed container, which has high requirements for reaction equipment and harsh reaction conditions. Chinese patent CN20151085128 uses gallium trifluoromethanesulfonate as an alkylation catalyst and investigates the performance of alkyl naphthalene base oil, but the preparation price of gallium trifluoromethanesulfonate catalyst is high and the catalyst contains fluorine elements that pollute the environment. Chinese patent CN102965175A uses methanesulfonic acid as a catalyst, and the reaction is subjected to alkaline washing and decolorization treatment. The reaction process is complicated and pollutes the environment, so the synthesis process of alkyl naphthalene and the property analysis and characterization of alkyl naphthalene base oil also need a lot of improvement. Summary of the invention
[0007] Aiming at the problems that inorganic acid catalysts corrode equipment, products are difficult to separate, pollute the environment, and solid acid catalysts are easily deactivated, have a short reaction life, poor activity after regeneration, and cannot synthesize monosubstituted long-chain alkyl naphthalene with high selectivity, the present invention develops a modified Y molecular sieve alkylation catalyst doped with a heteroatom and loaded with phosphorus, adjusts the synthesis process of alkyl naphthalene, and synthesizes a monosubstituted long-chain alkyl naphthalene base oil with more outstanding oxidation stability.
[0008] The synthesized base oil products are all monosubstituted alkylnaphthalenes, that is, the alkylnaphthalenes contain one identical C4~C 22 Alkyl substituents are present, and the ratio of α-alkylnaphthalene to β-alkylnaphthalene in the product is at least 1.5.
[0009] To achieve the above object, the present invention adopts the following technical solution: The present invention develops a method for preparing a modified Y molecular sieve alkylation catalyst doped with a heteroatom and loaded with a rare earth metal, and the method is specifically as follows: The present invention adopts a hydrothermal synthesis method to synthesize zeolite materials. First, a directing agent solution is prepared, and then a certain amount of silicon source is added to a beaker, the directing agent solution is slowly added to the silicon source, the rotation speed is adjusted to make it evenly mixed, and then a certain amount of aluminum source is added, and stirring is maintained for a certain period of time to prepare an intermediate gel, and a heteroatom source is added to the aluminum source solution prepared in advance to prepare a mixed solution, and then the mixed solution is added to the above intermediate gel, and the stirring state is maintained for a period of dynamic aging so that the components of the gel are fully mixed and evenly mixed, and the gel mixture is added to a crystallization kettle lined with polytetrafluoroethylene, and crystallized for a period of time to make it completely crystallized, and the crystallized product is fully filtered with deionized water, washed, and fully dried in a 120°C oven for 18 hours to obtain the prepared heteroatom Y zeolite sample.
[0010] In a specific embodiment of the present invention, the aluminum source for synthesizing heteroatom Y zeolite is at least one of sodium aluminate, aluminum sulfate, aluminum isopropoxide, aluminum hydroxide, pseudo-boehmite, alumina, and aluminum nitrate, and preferably the aluminum source is aluminum nitrate or aluminum sulfate.
[0011] In a specific embodiment of the present invention, the silicon source for synthesizing heteroatom Y zeolite is at least one of white carbon black, silica sol, solid silica gel, ethyl orthosilicate and water glass, and preferably the silicon source is water glass or silica sol.
[0012] In a specific embodiment of the present invention, the heteroatom source for synthesizing heteroatom Y zeolite is at least one of magnesium sulfate, magnesium nitrate, zirconium sulfate, cobalt nitrate, cobalt sulfate, tin nitrate, ferrous sulfate, and nickel nitrate, and preferably the heteroatom source is cobalt nitrate and magnesium sulfate.
[0013] In a specific embodiment of the present invention, the directing agent solution is formed by fully mixing an alkali source, a silicon source, an aluminum source and water, and the molar ratio of each component is Na2O:Al2O3:SiO2:H2O=(5-30):1:(10-25):(250-400), and the preferred molar ratio of each component is Na2O:Al2O3:SiO2:H2O=(10-25):1:(10-20):(350-400).
[0014] In a specific embodiment of the present invention, the alkali source is at least one of sodium hydroxide, potassium hydroxide, sodium oxide and urea, and preferably the alkali source is sodium hydroxide.
[0015] In a specific embodiment of the present invention, the aging temperature of the directing agent is 25-50°C, preferably 30-40°C.
[0016] In a specific embodiment of the present invention, the aging time of the directing agent is 7-24 hours, preferably 15-20 hours.
[0017] In a specific embodiment of the present invention, the aging temperature of the gel is 35-90°C, preferably 45-55°C.
[0018] In a specific embodiment of the present invention, the dynamic aging time of the gel is 2-8 hours, preferably 3-5 hours.
[0019] In a specific embodiment of the present invention, the crystallization temperature of the gel is 80-180°C, preferably 90-120°C.
[0020] In a specific embodiment of the present invention, the molar ratio of the alkali source, aluminum source, heteroatom source, silicon source and water source in the gel mixture is Na2O: (Al2O3 + M2O x ):SiO2:H2O=(2-8):1:(6-12):(150-250), preferably, the molar ratio of the alkali source, aluminum source, silicon source and water source of the gel is Na2O: (Al2O3+M2O x ):SiO2:H2O=(4-6):1:(8-10):(150-200). Wherein M is the heteroatom source, and the molar ratio of the heteroatom in the heteroatom source to the aluminum in the aluminum source (M:Al) is (0.25-0.5).
[0021] In a specific embodiment of the present invention, the mass of the directing agent solution accounts for 20%-30% of the total mass of the gel. Preferably, the directing agent accounts for 20%-25% of the total mass of the gel.
[0022] The heteroatom Y zeolite synthesized by the present invention has a silicon-aluminum ratio of 6.1-6.5, a crystal particle size of 200-600 nm, and a BET specific surface area of 700-850 m 2 / g, external specific surface area is 57~77m 2 / g, total pore volume is 0.38~0.58cm 3 / g, and the mesopore volume is 0.04~0.10cm 3 / g, relative crystallinity 90%~100%, with the characteristics of high silicon-aluminum ratio, small grains and high relative crystallinity.
[0023] In order to achieve the purpose of this technology, the heteroatom Y zeolite also needs post-treatment modification, which requires doping with rare earth metals and loading phosphorus to regulate its acid distribution, acid density and texture properties. The subsequent modification steps are as follows: (a) At 60-95°C, a rare earth metal source is dissolved in water to obtain a first component, a heteroatom Y zeolite is mixed with water to obtain a second component, the first component is slowly added dropwise to the second component and vigorously stirred to mix, i.e., the heteroatom Y zeolite is subjected to rare earth metal ion exchange treatment, and then fully washed with deionized water and filtered to neutrality, and dried at 90-180°C (preferably at 120°C).
[0024] In a specific embodiment of the present invention, the rare earth metal source is at least one of the lanthanide metals, preferably lanthanum chloride, lanthanum nitrate, cerium chloride, and cerium nitrate.
[0025] In a specific embodiment of the present invention, the loading amount of the rare earth metal (calculated as rare earth metal oxide) is 1-16 wt %, preferably 1-8 wt %.
[0026] In a specific embodiment of the present invention, the temperature of rare earth metal ion exchange is 60-95°C, preferably 80-90°C.
[0027] In a specific embodiment of the present invention, the rare earth metal ion exchange time is 0.5 to 4 hours, preferably 1 to 2 hours.
[0028] (b) After rare earth ion exchange, the heteroatom Y zeolite needs to be further subjected to ammonium ion exchange treatment and hydrothermal calcination treatment. Generally, the ammonium exchange and hydrothermal treatment need to be performed multiple times, preferably twice.
[0029] In a specific embodiment of the present invention, the ammonium ion exchange is carried out in the following manner: The heteroatom Y zeolite after rare earth ion exchange is added to a 0.5-2.0 mol / L ammonium chloride aqueous solution and allowed to stand for exchange for 1-3 hours at a temperature generally at 60-120°C (preferably 80-95°C), wherein the mass ratio of the heteroatom Y zeolite to the ammonium chloride aqueous solution is 1:5-20 (preferably 1:10-15).
[0030] In a specific embodiment of the present invention, the hydrothermal roasting treatment is carried out in the following manner: The dried heteroatom Y zeolite powder after rare earth ion exchange and ammonium ion exchange is ground and spread into a crucible, and then placed in a muffle furnace. The temperature of the muffle furnace is generally 400-800°C (preferably 650°C), and 60-100% water vapor (preferably 100% water vapor) is introduced. The hydrothermal roasting time is generally 1-6 hours (preferably 2 hours).
[0031] (c) The modified heteroatom Y zeolite obtained in step (b) needs to be further phosphorus-modified In one specific embodiment of the present invention, phosphorus modification is carried out in the following manner: The Y zeolite obtained in step (b) is dried in an oven at 90-180°C (preferably 120°C) for 12-18 hours (preferably 12 hours), the dried zeolite is ground and spread into a large crucible, the crucible is placed in a muffle furnace, the temperature is generally 450-800°C (preferably 550°C), and calcined for 2-6 hours (preferably 4 hours) to obtain a dry zeolite base. The zeolite is impregnated with an equal volume or excessive amount of diammonium hydrogen phosphate aqueous solution (preferably equal volume impregnation), the impregnated zeolite is activated at 25-90°C (preferably 25°C) for one day and night, and is placed in a muffle furnace for calcination at a temperature of 400-800°C (preferably 550°C), and the high temperature calcination is performed for 2-6 hours (preferably 4 hours) to obtain a modified Y molecular sieve alkylation catalyst.
[0032] In a specific embodiment of the present invention, the loading amount of diammonium hydrogen phosphate (calculated as phosphorus pentoxide) is 1-20 wt %, preferably 1-12 wt %.
[0033] The rare earth ion exchange and isovolume impregnation of diammonium hydrogen phosphate modified heteroatom Y zeolite of the present invention has excellent performance, a framework silicon-aluminum ratio of 18-50, a crystal particle size of 200-600nm, and a BET specific surface area of 620-750m 2 / g, external specific surface area is 100~150m 2 / g, total pore volume is 0.430~0.580cm 3 / g, and the mesopore volume is 0.180~0.300cm 3 / g, relative crystallinity 75%~90%, total acid content 0.200~0.300mmol / g, strong acid content 0.080~0.140mmol / g, acid center strength 0.40~0.52, with high silicon-aluminum ratio, small grains, high relative crystallinity, large specific surface area, high mesopores, low total acid density but high acid center strength, etc.
[0034] The present invention also provides a process for synthesizing a long-chain alkyl naphthalene base oil, wherein the alkyl naphthalene has only one identical C4-C 22 The method comprises the following steps: the catalyst used is the above-mentioned rare earth modified and phosphorus doped heteroatom Y zeolite, naphthalene and a single or mixed C4~C 22 Alkylation of α-olefins produces the long-chain alkylnaphthalenes mentioned above.
[0035] In a specific embodiment of the present invention, the temperature of the alkylation reaction is 100-250° C., preferably 120-205° C., more preferably 120-180° C.; the pressure of the alkylation reaction is 0.1-2.0 atm, preferably 0.8-1.0 atm, more preferably normal pressure; the alkylation reaction is 1-12 hours, preferably 2-6 hours, more preferably 2-4 hours; the alkylation reaction is carried out in an inert atmosphere, and the inert atmosphere is preferably nitrogen.
[0036] In a specific embodiment of the present invention, the steps of the alkylation reaction are as follows: the reaction system is maintained under a nitrogen atmosphere, a solvent is added first, and then naphthalene is added, and the reaction is heated to 90° C. to completely melt the naphthalene, and the naphthalene and the solvent are fully mixed, and then a catalyst is added to the reaction system. After the temperature reaches the target reaction temperature, the α-olefin is slowly added dropwise to the reaction system, and the reaction is carried out for 2 to 4 hours to complete the alkylation reaction.
[0037] In a specific embodiment of the present invention, the α-olefin used is a single olefin or a mixture of several olefins, preferably C6~C 20 α-olefins, more preferably C 10 ~C 16 α-Olefins.
[0038] In a specific embodiment of the present invention, the solvent used is C8~C 16 One or a mixture of normal alkanes, preferably C 12 ~C 16 One or a mixture of normal alkanes.
[0039] In a specific embodiment of the present invention, the molar ratio of naphthalene:olefin is 1:(0.5-2.5), preferably the molar ratio of naphthalene:olefin is 1:(0.8-1.2).
[0040] In a specific embodiment of the present invention, preferably, the mass ratio of solvent: (olefin + naphthalene) is 1: (1-2) In a specific embodiment of the present invention, preferably, the mass ratio of naphthalene to Y zeolite is 1:(0.05-0.15).
[0041] In a specific embodiment of the present invention, after the alkylation reaction is completed, the crude product is subjected to reduced pressure distillation to remove unreacted raw materials and solvent, and then fully centrifuged to collect Y zeolite and obtain a reaction product.
[0042] In a specific embodiment of the present invention, the collected Y zeolite catalyst is hydrothermally calcined and regenerated, and the regenerated catalyst is used to synthesize alkyl naphthalene.
[0043] The present invention also provides the use of the alkyl naphthalene prepared by the above method as a Class V alkyl naphthalene lubricant base oil.
[0044] Compared with the prior art, the present invention has the following advantages: The Y zeolite modified with rare earth and doped with phosphorus in the present invention has excellent properties, does not cause equipment corrosion and does not pollute the environment, and is a green alkylation catalyst. The Y zeolite modified by the present invention has the characteristics of high relative crystallinity, high skeleton silicon-aluminum ratio, large specific surface area, large mesopore volume, strong acid strength but extremely low total acid density, so the catalyst of the present invention is not easy to deposit carbon, has a long service life, and has very good product selectivity. The alkyl naphthalene synthesized in the present invention is all monosubstituted alkyl naphthalene and the alpha-alkyl naphthalene / beta-alkyl naphthalene is at least 1.5, so it has excellent thermal oxygen stability and suitable viscosity. The catalyst of the present invention can be regenerated by simple hydrothermal roasting, and the base oil synthesized by the catalysis after regeneration for 5 times still has excellent properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is the XRD spectrum of the alkylation catalyst; Figure 2 SEM spectra of alkylation catalysts (a~e: catalysts 1~5). DETAILED DESCRIPTION
[0046] The preparation and modification methods of the catalyst of the present invention and the synthesis process of alkyl naphthalene are further described below in conjunction with specific examples. However, the specific implementation methods described herein are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0047] Example 1 At a water bath temperature of 40°C, 60.5g of water glass solution (Na2O: 9.96wt%, SiO2: 31.5wt%) was added to a beaker while maintaining dynamic stirring. Then, 35.6g of sodium aluminate solution (Na2O: 27wt%, Al2O3: 4.5wt%) was added to the beaker. Finally, 25g of deionized water was added to the beaker while maintaining dynamic stirring for 90 minutes. The solution was then allowed to stand and aged for 20 hours to obtain a directing agent solution.
[0048] At a water bath temperature of 60°C, 170g of water glass solution (Na2O: 9.96wt%, SiO2: 31.5wt%) was added to another beaker, and dynamic stirring was maintained. 100g of directing agent solution and 19.78g of sodium aluminate solution (Na2O: 27wt%, Al2O3: 4.5wt%) were slowly poured into the beaker in sequence, and dynamic stirring was maintained for 30 minutes to allow the components to be fully mixed. 79.01g of aluminum sulfate solution (Al2O 3:The mixed solution was slowly added into the above beaker and dynamically aged for 2 hours to obtain a gel mixture, and the gel mixture was added into a polytetrafluoroethylene-lined crystallization kettle. After crystallization at 120°C for 14 hours, the crystallized product was fully filtered with deionized water, washed, and fully dried in an oven at 120°C for 18 hours to obtain a heteroatom Y zeolite sample.
[0049] The heteroatom Y zeolite synthesized in Example 1 has a crystallinity of 88% and a BET specific surface area of 750 m 2 / g, external specific surface area is 47m 2 / g, with a total pore volume of 0.35 cm 3 / g, and the mesopore volume is 0.03cm 3 / g, the framework silicon-aluminum ratio is 5.9, and the grain size is about 350nm.
[0050] Example 2 At a water bath temperature of 34°C, 50g of water glass solution (Na2O: 9.96wt%, SiO2: 31.5wt%) was added to a beaker while maintaining dynamic stirring. Then, 35g of sodium aluminate solution (Na2O: 27wt%, Al2O3: 4.5wt%) was added to the beaker. Finally, 35g of deionized water was added to the beaker while maintaining dynamic stirring for 90 minutes. The solution was then allowed to stand and aged for 20 hours to obtain a directing agent solution.
[0051] At a water bath temperature of 55°C, 150g of water glass solution (Na2O: 9.96wt%, SiO2: 31.5wt%) was added to another beaker, and dynamic stirring was maintained. 100g of directing agent solution and 13.69g of sodium aluminate solution (Na2O: 27wt%, Al2O3: 4.5wt%) were slowly poured into the beaker in sequence, and dynamic stirring was maintained for 30 minutes to allow the components to be fully mixed. 68.85g of aluminum sulfate solution (Al2O 3: 9wt%) and 2.78g MgSO4 were prepared into a mixed solution, the mixed solution was slowly added to the above beaker, dynamically aged for 2 hours to obtain a gel mixture, the gel mixture was added into a polytetrafluoroethylene-lined crystallization kettle, and after crystallization at 120°C for 16 hours, the crystallized product was fully filtered with deionized water, washed, and fully dried in an oven at 120°C for 18 hours to obtain a heteroatom Y zeolite sample.
[0052] The heteroatom Y zeolite synthesized in Example 2 has a crystallinity of 91% and a BET specific surface area of 850 m 2 / g, external specific surface area is 57m 2 / g, and the total pore volume is 0.38cm 3 / g, and the mesopore volume is 0.04cm 3 / g, a framework silicon-aluminum ratio of 6.2, and a crystallite size of about 200nm, which is preferably used as a post-modified zeolite precursor.
[0053] Example 3 The synthesized heteroatom Y zeolite is used as a post-modified zeolite precursor, wherein the rare earth Ce source is selected as CeCl3·7H2O, and the input amount of rare earth Ce relative to the heteroatom Y zeolite is 4wt% (in terms of Ce2O3). Weigh CeCl3·7H2O and add it to a beaker filled with water and stir to dissolve, then add the heteroatom Y zeolite to the beaker, heat exchange in a 90℃ water bath for 1 hour, wash, filter and dry. Then perform two ammonium exchanges and two hydrothermal treatments, the ratio of raw materials in the molecular sieve ammonium exchange is molecular sieve: ammonium chloride: deionized water = 1:1:10 (mass ratio), heat and stir in a 90℃ water bath for 1 hour, and adjust its pH value between 3.0 and 3.3 with 0.2mol / L hydrochloric acid during the water bath process. Then, the sample was washed and filtered with deionized water, and dried in an oven at 120°C. The dried sample was ground and evenly spread on the crucible wall, and then calcined in a muffle furnace at 650°C and 100% water vapor for 2 hours. The same ammonium exchange and hydrothermal calcination process was performed again to obtain the rare earth metal ion-exchanged heteroatom Y zeolite.
[0054] The Y zeolite with heteroatom after rare earth metal ion exchange is used as a phosphorus-modified zeolite precursor, and diammonium hydrogen phosphate is selected as the phosphorus source, and the amount of diammonium hydrogen phosphate relative to the zeolite is 1wt% (in terms of P2O5). The Y zeolite modified by rare earth is placed in a 120°C oven to be fully dried, and then the zeolite sample is placed in a 550°C muffle furnace for calcination for 4 hours to obtain a zeolite dry base. The hetero zeolite dry base is impregnated with an aqueous solution of diammonium hydrogen phosphate in equal volumes, and then the impregnated sample is placed at room temperature for activation for 24 hours, and then the sample is placed in a 550°C muffle furnace for calcination for 4 hours to complete the phosphorus modification of the zeolite.
[0055] The rare earth-modified and phosphorus-modified heteroatom Y zeolite can be used as the alkylation catalyst 1 of the present invention.
[0056] Example 4 The input amount of rare earth Ce to heteroatom Y zeolite is 4 wt% (in terms of Ce2O3). The input amount of diammonium hydrogen phosphate to zeolite is 4 wt% (in terms of P2O5). Other conditions are the same as those in Example 1, which is alkylation catalyst 2.
[0057] Example 5 The input amount of rare earth Ce to heteroatom Y zeolite is 8 wt% (in terms of Ce2O3). The input amount of diammonium hydrogen phosphate to zeolite is 8 wt% (in terms of P2O5). Other conditions are the same as those in Example 1, which is alkylation catalyst 3.
[0058] Example 6 The amount of rare earth Ce added to the heteroatom Y zeolite is 4 wt% (in terms of Ce2O3). The amount of diammonium hydrogen phosphate added to the zeolite is 12 wt% (in terms of P2O5). Other conditions are the same as those in Example 1, which is alkylation catalyst 4.
[0059] Example 7 The amount of rare earth Ce added to the heteroatom Y zeolite is 1 wt% (in terms of Ce2O3). The amount of diammonium hydrogen phosphate added to the zeolite is 16 wt% (in terms of P2O5). Other conditions are the same as those in Example 1, which is alkylation catalyst 5.
[0060] Examples 3 to 7 are methods for preparing the alkylation catalyst of the present invention. The properties of the synthesized alkylation catalyst are as follows: Table 1. Framework properties of alkylation catalysts Table 2. Textural properties of alkylation catalysts Table 3. Characterization of acid properties of alkylation catalysts The alkylation catalyst prepared by the present invention has more excellent acid properties and textural properties than conventional USY zeolite, such as a larger external specific surface area, a larger mesopore volume, a reduced total acid density but a greatly increased B / L and an enhanced acid center strength, so the prepared alkylation catalyst is not prone to carbon deposition and deactivation, has enhanced hydrothermal stability, is easy to regenerate, and has higher alkylation selectivity and catalytic activity.
[0061] The olefins used in the following examples are all straight-chain α-olefins without any branches. The kinematic viscosity of the product at 40°C and 100°C is measured according to ASTM D445, the viscosity index is measured according to ASTM D2270, the flash point is measured according to ASTMD92, the pour point is measured according to GB / T 3535, the acid value is measured according to GB / T 7304-2014, the water content is measured according to GB / T 11146-2009, and the product is qualitatively characterized by nuclear magnetic resonance hydrogen spectrum and GC-MS. The thermal oxidation stability of the product is characterized by the DSC onset oxidation temperature, and the DSC onset oxidation temperature is tested according to SN / T3950-2014.
[0062] Example 8 In a nitrogen inert environment, 34.84g of n-dodecane solvent and 25g of naphthalene were first added to a flask, and then 3.75g of catalyst 5 was added, heated to 160°C, naphthalene and n-dodecane solvent were fully mixed, 32.83g of 1-decene was added dropwise to the flask at a speed of 1 drop per second using a constant pressure dropping funnel, and the alkylation reaction was completed in 4 hours. The material in the flask was subjected to reduced pressure distillation at a temperature of 220°C and a gauge pressure of -0.1Mpa to remove unreacted olefins, naphthalene and n-dodecane solvent to obtain a crude product, and the crude product was fully centrifuged to collect the solid acid catalyst to obtain the final product, the product obtained was a transparent golden yellow, the conversion rate of naphthalene was 95.5%, the selectivity was 99.9%, and the product yield was 95.4%. The product was characterized by GC-MS and H NMR, and it was found that the product was naphthalene with only one decane substituent.
[0063] Example 9 In a nitrogen inert environment, 43.45g of n-dodecane solvent and 28g of naphthalene were first added to a flask, and then 4.20g of catalyst 4 was added, heated to 160°C, naphthalene and n-dodecane solvent were fully mixed, 44.12g of 1-dodecene was added dropwise to the flask at a speed of 1 drop per second using a constant pressure dropping funnel, and the alkylation reaction was completed in 4 hours. The material in the flask was subjected to reduced pressure distillation at a temperature of 220°C and a gauge pressure of -0.1Mpa to remove unreacted olefins, naphthalene and n-dodecane solvent to obtain a crude product, and the crude product was fully centrifuged to collect the solid acid catalyst to obtain the final product, the product obtained was a transparent golden yellow, the conversion rate of naphthalene was 97.5%, the selectivity was 99.9%, and the product yield was 97.3%. The product was characterized by GC-MS and H NMR, and it was found that the product was naphthalene with only one dodecane substituent.
[0064] Example 10 In a nitrogen inert environment, 51.30g of n-dodecane solvent and 30g of naphthalene were first added to a flask, and then 4.50g of catalyst 4 was added, heated to 160°C, naphthalene and n-dodecane solvent were fully mixed, 55.15g of 1-tetradecene was added dropwise to the flask at a speed of 1 drop per second using a constant pressure dropping funnel, and the alkylation reaction was completed in 4 hours by reaction, and the material in the flask was subjected to reduced pressure distillation at a temperature of 220°C and a gauge pressure of -0.1Mpa to remove unreacted olefins, naphthalene and n-dodecane solvent to obtain a crude product, and the crude product was fully centrifuged to collect the solid acid catalyst to obtain the final product, the product obtained was a transparent golden yellow, the conversion rate of naphthalene was 96.5%, the selectivity was 99.9%, and the product yield was 96.4%. The product was characterized by GC-MS and H NMR, and it was found that the product was naphthalene with only one tetradecane substituent.
[0065] Embodiment 11 In a nitrogen inert environment, 56.05g of n-dodecane solvent and 30g of naphthalene were first added to a flask, and then 4.5g of catalyst 4 was added, heated to 160°C, naphthalene and n-dodecane solvent were fully mixed, 63.04g of 1-hexadecene was added dropwise to the flask at a speed of 1 drop per second using a constant pressure dropping funnel, and the alkylation reaction was completed in 4 hours by reaction, and the material in the flask was subjected to reduced pressure distillation at a temperature of 220°C and a gauge pressure of -0.1Mpa to remove unreacted olefins, naphthalene and n-dodecane solvent to obtain a crude product, and the crude product was fully centrifuged to collect the solid acid catalyst to obtain the final product, the product obtained was a transparent golden yellow, the conversion of naphthalene was 96.5%, the selectivity was 99.9%, and the product yield was 96.4%. The product was characterized by GC-MS and H NMR, and it was found that the product was a naphthalene having only one hexadecane substituent.
[0066] Example 12 In nitrogen inert environment, in flask, add 57.08g n-dodecane solvent and 35g naphthalene earlier, then add 5.25g catalyst 5, be heated to 160 ℃, naphthalene and n-dodecane solvent are fully mixed, with constant pressure dropping funnel, 11.49g1-decene, 13.79g 1-dodecene, 16.09g 1-tetradecene, the olefin mixture of 18.39g 1-hexadecene composition is added drop-wise in the flask at the speed of 1 drop per second, reacted 4 hours and completed alkylation reaction, by the material in the flask at 220 ℃ of temperature, gauge pressure is-0.1Mpa under reduced pressure distillation to remove unreacted complete olefin, naphthalene and n-dodecane solvent and obtain thick product, with thick product fully centrifugal collection solid acid catalyst after obtain the finished product, the product obtained is transparent golden yellow, the conversion ratio of naphthalene is 96.7%, and selectivity is 99.9%, and product yield is 96.4%. The product was characterized by GC-MS and H NMR, and it was found that the product was a monosubstituted naphthalene with only one alkyl substituent, and the product was a mixture of naphthalene with a decane substituent, a dodecane substituent, a tetradecane substituent, and a hexadecane substituent.
[0067] Example 13 In a nitrogen inert environment, 51.30g of n-dodecane solvent and 30g of naphthalene were first added to a flask, and then 4.5g of catalyst 5 was added, heated to 130°C, naphthalene and n-dodecane solvent were fully mixed, 55.15g of 1-tetradecene was added dropwise to the flask at a speed of 1 drop per second using a constant pressure dropping funnel, and the alkylation reaction was completed in 4 hours by reaction, the material in the flask was subjected to reduced pressure distillation at a temperature of 220°C, and a gauge pressure of -0.1Mpa to remove unreacted olefins, naphthalene and n-dodecane solvent to obtain a crude product, the crude product was fully centrifuged to collect the solid acid catalyst to obtain the final product, the product obtained was a transparent golden yellow, the conversion of naphthalene was 97.5%, the selectivity was 99.9%, and the product yield was 97.4%. The product was characterized by GC-MS and H NMR, and it was found that the product was a naphthalene having only one tetradecane substituent.
[0068] Embodiment 14 In a nitrogen inert environment, 40.22g of n-dodecane solvent and 30g of naphthalene were first added to a flask, and then 4.5g of catalyst 5 was added, heated to 130°C, naphthalene and n-dodecane solvent were fully mixed, 36.77g of 1-tetradecene was added dropwise to the flask at a speed of 1 drop per second using a constant pressure dropping funnel, and the alkylation reaction was completed in 4 hours by reaction, the material in the flask was subjected to reduced pressure distillation at a temperature of 220°C, and a gauge pressure of -0.1Mpa to remove unreacted olefins, naphthalene and n-dodecane solvent to obtain a crude product, the crude product was fully centrifuged to collect the solid acid catalyst to obtain the final product, the product obtained was a transparent golden yellow, the conversion of naphthalene was 96.7%, the selectivity was 99.9%, and the product yield was 96.4%. The product was characterized by GC-MS and H NMR, and it was found that the product was a naphthalene having only one tetradecane substituent.
[0069] Comparative Example 1 Comparative Example 1 is a commercially available alkyl naphthalene base oil, which has a kinematic viscosity of 29.0 cst at 40°C, a kinematic viscosity of 4.7 cst at 100°C, a viscosity index of 74, a pour point of -39°C, a flash point of 222°C, a water content of <50 ppm, and a total acid value of <50 ppm.
[0070] The properties of the lubricating base oils prepared in Examples 8 to 14 and Comparative Example 1 are shown in Table 4: Table 4. Properties of lubricating base oils prepared in various embodiments and comparative examples As shown in Table 4, the lubricating base oil prepared in the embodiment of the present invention has comparable performance to the commercially available alkyl naphthalene base oil in Comparative Example 1, but has a higher DSC onset oxidation temperature, and thus has more excellent thermal oxidation stability.
[0071] The above embodiments are some preferred embodiments of the present invention and cannot be used as limitations of the present invention. Any changes and modifications made by those skilled in the art to the technical solutions of the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a modified Y molecular sieve alkylation catalyst doped with a heteroatom and loaded with a rare earth metal, characterized in that: The following steps are involved: (1) The zeolite material is synthesized by a hydrothermal synthesis method: first, a directing agent solution is prepared, and then a certain amount of silicon source is added to a beaker, and the directing agent solution is slowly added to the silicon source, and the rotation speed is adjusted to make it evenly mixed, and then a certain amount of aluminum source is added, and stirring is maintained for a certain period of time to prepare an intermediate gel, and the heteroatom source is added to the aluminum source solution prepared in advance to prepare a mixed solution, and then the mixed solution is added to the intermediate gel, and the stirring state is maintained for a period of time to allow the components to be fully mixed and evenly mixed, and the gel mixture is added to a crystallization kettle lined with polytetrafluoroethylene, and crystallized for a period of time to make it completely crystallized, and the crystallized product is fully filtered with deionized water, washed, and fully dried in an oven at 120°C for 18 hours to obtain a heteroatom Y zeolite sample; (2) Rare earth metal doping modification: at 60-95°C, a rare earth metal source is dissolved in water to obtain a first component, and the heteroatom Y zeolite is mixed with water to obtain a second component, and the first component is slowly added dropwise to the second component and vigorously stirred to mix evenly, i.e., the heteroatom Y zeolite is subjected to rare earth metal ion exchange treatment, and then fully washed with deionized water, filtered to neutrality, and dried at 90-180°C; (3) Ammonium ion exchange treatment: Add the Y zeolite after rare earth ion exchange into an aqueous solution of ammonium chloride and allow to stand for exchange at a temperature of 60-120 °C for 1-3 hours; (4) Hydrothermal calcination: Grind the dried Y zeolite powder after rare earth ion exchange and ammonium ion exchange and spread it into a crucible, then put it into a muffle furnace. The temperature of the muffle furnace is 400-800°C, and 60-100% water vapor is introduced. The hydrothermal calcination time is 1-6 hours. (5) Phosphorus modification treatment: Dry the Y zeolite after hydrothermal calcination in an oven at 90-180°C for 12-18 hours, grind the dried zeolite and spread it into a large crucible, place the crucible in a muffle furnace at a temperature of 450-800°C, and calcine for 2-6 hours to obtain a dry zeolite base; impregnate the zeolite with an equal volume of diammonium hydrogen phosphate aqueous solution, activate the impregnated zeolite at 25-90°C for one day and night, place it in a muffle furnace at a temperature of 400-800°C, and calcine at high temperature for 2-6 hours to obtain a modified Y molecular sieve alkylation catalyst.
2. The preparation method according to claim 1, characterized in that: In step (1), the aluminum source is at least one of sodium aluminate, aluminum sulfate, aluminum isopropoxide, aluminum hydroxide, pseudo-boehmite, aluminum oxide, and aluminum nitrate; the silicon source is at least one of white carbon black, silica sol, solid silica gel, ethyl orthosilicate, and water glass; and the heteroatom source is at least one of magnesium sulfate, magnesium nitrate, zirconium sulfate, cobalt nitrate, cobalt sulfate, tin nitrate, ferrous sulfate, and nickel nitrate.
3. The preparation method according to claim 2, characterized in that: The guiding agent solution is prepared by fully mixing an alkali source, a silicon source, an aluminum source and water, and the molar ratio of each component is Na2O:Al2O3:SiO2:H2O=(5-30):1:(10-25):(250-400); wherein the alkali source is at least one of sodium hydroxide, potassium hydroxide, sodium oxide and urea; the aging temperature of the guiding agent is 25-50°C, and the aging time is 7-24 hours.
4. The preparation method according to claim 1, characterized in that: In step (1), the aging temperature of the gel is 35-90°C, the dynamic aging time is 2-8 hours; and the crystallization temperature of the gel is 80-180°C.
5. The preparation method according to claim 1, characterized in that: The molar ratio of the alkali source, aluminum source, heteroatom source, silicon source and water source in the gel mixture in step (1) is Na2O: (Al2O3 + M2O x ):SiO2:H2O=(2-8):1:(6-12):(150-250), wherein M is a heteroatom source, and the molar ratio of the heteroatom in the heteroatom source to the aluminum in the aluminum source (M:Al) is (0.25-0.5).
6. The preparation method according to claim 1, characterized in that: In step (1), the mass of the directing agent solution accounts for 20%-30% of the total mass of the gel mixture.
7. The preparation method according to claim 1, characterized in that: In step (2), the rare earth metal source is one of lanthanum chloride, lanthanum nitrate, cerium chloride and cerium nitrate; and the loading amount of the rare earth metal is 1-16 wt % calculated as rare earth metal oxide.
8. The preparation method according to claim 1, characterized in that: In step (5), the loading amount of diammonium hydrogen phosphate calculated as phosphorus pentoxide is 1-20 wt %.
9. A modified Y molecular sieve alkylation catalyst doped with a rare earth metal and loaded with phosphorus, prepared according to the preparation method of any one of claims 1 to 8.
10. The use of the modified Y molecular sieve alkylation catalyst according to claim 9 in the synthesis of long-chain alkyl naphthalene base oil, characterized in that: The synthesized alkyl naphthalenes are all monosubstituted alkyl naphthalenes and the α-alkyl naphthalene / β-alkyl naphthalene ratio is at least 1.5.
Citation Information
Patent Citations
Hydrocracking catalyst containing Y-type molecular sieve, and preparation method thereof
CN103447073A
Modified Y catalyst containing rare earth and phosphorus
CN106268919A
Y molecular sieve for synthesizing dimethyl carbonate through carbonylation of methyl nitrite, and preparation method thereof
CN110844918A
Molecular sieve catalyst, preparation method thereof and liquefied petroleum gas alkylation reaction method
CN111330630A
Method for preparing alkyl naphthalene lubricant base oil from coal alpha-olefin
CN114790407A
Cited By
Catalyst for synthesizing lubricant base oil and preparation method thereof
CN121314659A