Catalyst composition, method for selectively hydrogenating conjugated diene latex, hydrogenated conjugated diene latex and application of hydrogenated conjugated diene latex
By using catalyst compositions of ruthenium or osmium complexes with specific co-catalysts, problems such as catalyst dispersion and slow reaction rates in the selective hydrogenation of conjugated diene latex have been solved, achieving efficient and gel-free hydrogenation, suitable for a variety of industrial applications.
Patent Information
- Application Number
- CN202410361832.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-29
AI Technical Summary
Existing technologies for preparing hydrogenated diene-based rubber suffer from problems such as poor catalyst dispersion, slow reaction rate, gel formation, and environmental pollution, making it difficult to achieve efficient and rapid selective hydrogenation of conjugated diene latex.
A catalyst composition is formed by using ruthenium complex or osmium complex as the main catalyst and combining it with specific co-catalysts and co-catalysts for the selective hydrogenation of conjugated diene latex, thereby reducing the amount of catalyst used and optimizing the hydrogenation conditions to avoid gel formation.
It achieves highly efficient selective hydrogenation of conjugated diene latex, improves production efficiency, reduces catalyst residue, ensures good performance of vulcanized rubber without gelation problems, and is suitable for applications such as impregnation, adhesives, coatings and composites.
Smart Images

Figure CN119034812A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer hydrogenation modification, and in particular relates to a catalyst composition, a method for selective hydrogenation of conjugated diene latex, hydrogenated conjugated diene latex and applications thereof. Background Art
[0002] The research and development of hydrogenated diene-based rubber products mainly refers to obtaining rubber products with the required performance through formulation design and subsequent processing methods according to the application environment of rubber parts. At present, whether in laboratory or industrial production, hydrogenated diene-based rubber is mainly prepared by three methods. Hydrogenated parent diene-based unsaturated polymers, such as nitrile rubber (also known as NBR) prepared by polymerization of acrylonitrile and butadiene, are well known. Taking NBR as an example, the specific methods are as follows:
[0003] (1) Acrylonitrile-ethylene copolymerization method:
[0004] In the ethylene-acrylonitrile copolymerization reaction, due to the large difference in the reactivity ratio of acrylonitrile and ethylene (acrylonitrile is 0.04, ethylene is 0.8), the input ratio of the reaction raw materials needs to be strictly controlled. In addition, group rearrangement is prone to occur during the copolymerization reaction, and there are many side reactions, resulting in poor randomness of the chain segments, poor performance of the obtained product, and ultimately affecting the processing performance of the product. Therefore, it is still in the research stage.
[0005] (2) Solution hydrogenation method:
[0006] The NBR solution hydrogenation method includes heterogeneous solution hydrogenation method and homogeneous solution hydrogenation method. During the operation, NBR is crushed and dissolved in a suitable organic solvent. The solvents used are mainly cyclohexanone, chlorobenzene, xylene and chloroform. It is placed in a high-temperature and high-pressure reactor and reacts with hydrogen under the action of a precious metal catalyst to selectively hydrogenate and prepare HNBR. The solution hydrogenation method is currently the main method for industrial production of HNBR. During hydrogenation, only the double bonds on the butadiene unit are selectively hydrogenated and reduced to saturated single bonds, and the nitrile group is not hydrogenated. The key to the solution hydrogenation method lies in the selection of catalysts. The NBR solution hydrogenation method can be divided into heterogeneous hydrogenation using Group VIII metals coated on inorganic carriers as catalysts and homogeneous hydrogenation based on rhodium, ruthenium and palladium catalysts. The heterogeneous catalyst used in the heterogeneous solution hydrogenation method is a supported catalyst with palladium, rhodium, ruthenium, etc. as active components and aluminum oxide, silicon oxide, activated carbon, carbon black, alkaline earth metal carbonate, etc. as carriers. After the hydrogenation reaction is completed, the hydrogenation product is directly separated from the catalyst by filtering or centrifugal separation. Japan's Zeon Company first used supported catalysts for NBR hydrogenation in the 1980s. The heterogeneous support catalyst is a palladium / carbon catalyst with carbon as the carrier. The catalyst has high selectivity and the hydrogenation rate is as high as 95.6%. However, in the hydrogenation reaction, carbon easily adsorbs rubber molecules, resulting in agglomeration and agglomeration, which affects the product performance. The main advantage of heterogeneous support catalysts is that the catalyst is easy to separate, but the activity and selectivity of the hydrogenation catalyst are greatly affected by the environment. In addition, most of the active components of the supported catalyst prepared by the traditional method are distributed inside the pores. NBR molecules must diffuse into the pores to carry out the hydrogenation reaction. In order to increase the reaction rate, the reaction must be controlled under high pressure and strong stirring conditions. The reaction time is long and the process energy consumption is high, which leads to the deterioration of polymer properties.
[0007] Diolefin-based unsaturated polymers, for example acrylonitrile-butadiene rubber (also referred to as NBR) prepared by polymerization of acrylonitrile and butadiene, are well known in the art. For example, the copolymerization method of acrylonitrile and butadiene has been described in US3690349, US5770660 and CN102532414. According to the preparation conditions, this type of polymer can be obtained as the latex in the aqueous medium. Diolefin-based unsaturated polymers such as NBR are used for multiple industrial purposes, and the hydrogenation method of this type of unsaturated polymers is also well known in the art.
[0008] The technology of polymer catalytic hydrogenation based on organic solution is very mature, and related patents include US6410657, US6020439, US5705571, US5057581 and US3454644. It is known that the carbon-carbon double bonds in diene-based polymers can be selectively hydrogenated by treating the polymer in organic solution with hydrogen in the presence of a catalyst, thereby preparing their saturated polymers, which have significantly improved end-use properties. Such a method can be selective for the double bonds to be hydrogenated, so that, for example, the double bonds in the aromatic or cycloalkyl groups are not hydrogenated, and the double bonds or triple bonds between carbon and other atoms such as nitrogen or oxygen are not affected. This technical field includes many catalyst examples suitable for such hydrogenation, including catalysts based on cobalt, nickel, rhodium, ruthenium, osmium and iridium. The suitability of the catalyst depends on the desired degree of hydrogenation, the hydrogenation reaction rate and the presence of other groups such as carboxyl and nitrile groups in the polymer.
[0009] US6410657 teaches a method for selectively hydrogenating unsaturated double bonds in conjugated diene units of homopolymers or copolymers in the presence of a homogeneous organic titanium-based catalyst. The use of a catalyst mixture consisting of a substituted or unsubstituted monocyclopentadienyl titanium compound and lithium hydride derived from the reaction of an alkyl lithium with hydrogen in a solution shows a high degree of hydrogenation and hydrogenation reproducibility.
[0010] US6020439 describes a method for hydrogenating a living polymer mainly comprising a conjugated double bond monomer and an aromatic vinyl monomer. A polymer prepared from at least one conjugated diene compound is contacted with hydrogen in the presence of a catalyst. The catalyst is formed from a cyclopentadienyl titanium compound. A cocatalyst is provided in the form of an alkoxy lithium compound. The catalyst system selectively hydrogenates the unsaturated double bonds in the conjugated diene units of the living polymer in solution.
[0011] US5705571 provides a method for the selective hydrogenation of a conjugated diene polymer. The method comprises contacting a conjugated diene polymer with hydrogen in an inert organic solvent in the presence of a hydrogenation catalyst composition comprising a substituted or unsubstituted bis(cyclopentadienyl) Group VIII transition metal compound and an organic lithium compound. It is claimed that hydrogenation can be carried out under mild conditions in the presence of a small amount of the hydrogenation catalyst composition, and that the hydrogenation conversion rate and the selectivity to the conjugated diene unit are both high.
[0012] US5057581 teaches a process for selectively hydrogenating carbon-carbon double bonds of conjugated diene copolymers in the presence of certain divalent ruthenium carbonyl complex catalysts containing phosphine ligands having bulky alkyl substituents in a homogeneous solution in an organic solvent.
[0013] US3454644 teaches the use of a metal complex of ruthenium or osmium bonded to two electronegative species selected from hydrogen and halogen and coordinated to at least two organic stabilizing ligands such as a carbonyl group or a tertiary phosphine as a catalyst to hydrogenate an unsaturated organic compound having 2 to 20 carbon atoms containing at least one moiety selected from ketones, formyls, nitriles, non-aromatic carbon double bonds and carbon-carbon triple bonds in solution.
[0014] In summary, research in this area, namely the hydrogenation of diene-based polymers, has been very successful if the polymer is made soluble in an organic solvent, but dissolving the polymer in an organic solvent has many disadvantages and problems.
[0015] However, many diene-based polymers / copolymers are prepared by emulsion polymerization and are discharged from the polymerization reactor in the form of latex. It is therefore highly desirable to develop a process for directly hydrogenating diene-based polymer latexes.
[0016] (3) Emulsion hydrogenation method:
[0017] Add heavy metal catalyst to nitrile latex for hydrogenation to prepare HNBR. Goodyear of the United States first proposed the process of preparing emulsion HNBR using diimide as a reducing agent in 1984. NBR latex can directly generate HNBR under the action of hydrazine or oxygen or hydrogen peroxide as an oxidant and iron or copper metal ion initiators (related US patent application: US4452950), but this reduction method is easy to produce gel, the utilization rate of hydrazine or hydrogen peroxide is low, and it is not easy to recycle. The advantages of emulsion hydrogenation are that the reaction conditions are milder than solution hydrogenation, the process is simple, no solvent is required, the cost can be reduced, the pollution can be reduced, and the product can be recycled and reused (the product is an emulsion and can be used as a special coating). Therefore, the NBR emulsion hydrogenation method has received more and more attention. The disadvantage is that the unhydrogenated double bonds may undergo cross-linking reactions, resulting in an increase in the viscosity of the system and affecting the later processing. Since the NBR solution hydrogenation method is complex, a solvent is required during the reaction process, and the solvent discharge will cause environmental pollution. NBR emulsion polymerization is prone to gel formation due to the presence of severe cross-linking reactions, which makes it difficult to separate the product. At the same time, the emulsion hydrogenation method has the problem of slow hydrogenation rate and is not suitable for large-scale production.
[0018] Yue Dongmei et al. from Beijing University of Chemical Technology improved the hydrogenation method of NBR latex, reduced the gel content of HNBR latex, and increased the degree of hydrogenation (related Chinese patent applications: CN101486775, CN101704909).
[0019] In recent years, direct hydrogenation of polymer latex has attracted increasing attention. Many efforts have been made to achieve this process as described below.
[0020] US Pat. No. 6,552,132 claims a process for the hydrogenation of polymers composed of diene monomer units and monomer units containing nitrile groups, wherein the hydrogenation is carried out in the presence of hydrazine and an oxidizing compound in the form of an aqueous dispersion.
[0021] US6521694 describes a process for hydrogenating the carbon-carbon double bonds of unsaturated polymers in the form of an aqueous dispersion, to which are added a reducing agent selected from hydrazine and hydrazine-releasing compounds, an oxidizing compound and a catalyst, wherein the catalyst contains an element from Group 13 of the Periodic Table of Elements.
[0022] US5272202 describes a method for selectively hydrogenating the carbon-carbon double bonds of an unsaturated polymer containing nitrile groups with hydrogen in the presence of a hydrogenation catalyst. It relates to an aqueous emulsion of an unsaturated polymer containing nitrile groups. Optionally, an organic solvent capable of dissolving or swelling the polymer is present in a volume ratio of aqueous emulsion to organic solvent in the range of 1:3 to 1:0. A palladium compound is used as a hydrogenation catalyst, and the aqueous emulsion is contacted with gaseous or dissolved hydrogen while maintaining an emulsified state.
[0023] US6403727 discloses a method for selectively hydrogenating ethylenically unsaturated double bonds in polymers. The method comprises reacting the polymers with hydrogen in an aqueous suspension of the polymers in the presence of at least one hydrogenation catalyst selected from salts and complex compounds of rhodium and / or ruthenium. A suitable germanium-containing catalyst is of the formula RhX m L 3 L 4 (L 5 ) n A rhodium phosphine complex wherein X is a halide, an anion of a carboxylic acid, acetylacetonate, an aryl or alkyl sulfonate, a hydride or a diphenyltriazine anion, and L 3 ,L 4 and L 5 are independently CO, olefin, cycloolefin, dibenzophosphol, benzonitrile, PR3 or R2P-A-PR2, m is 1 or 2 and n is 0, 1 or 2, provided that L 3 , L 4 or L 5 At least one of the above phosphorus-containing ligands is one of the formula PR3 or PR2-A-PR2, wherein R is alkyl, alkoxy, cycloalkyl, cycloalkoxy, aryl or aryloxy.
[0024] A study has disclosed an NBR-latex hydrogenation technology, by which rubber latex is directly hydrogenated without pre-treating the latex before hydrogenation. Wilkinson catalyst and its ligand triphenylphosphine (TPP) are used as catalyst and co-catalyst, respectively. In this study, the addition of excess TPP plays a crucial role in the catalyst entering the latex particles. One disadvantage of this system is that the hydrogenation rate is quite slow, which limits the further development of this technology.
[0025] JP02178305 describes a method for hydrogenating nitrile rubber by contacting the emulsion with hydrogen in the presence of a Pd compound and optionally swelling the emulsion in an organic solvent. Thus, 100 ml of a 10% nitrile rubber emulsion (containing 39.4% of units derived from acrylonitrile) was mixed with 63.3 mg of palladium benzoate in 50 ml of benzene and heated at 50° C. for 6 hours under a hydrogen pressure of 30 atm to give a 90.2% hydrogenated emulsion.
[0026] EP1705194A1 discloses a method for directly hydrogenating diene-based polymer latex using an organic metal catalyst and high-pressure gaseous hydrogen. The organic metal catalyst is RhCl(PPh3)3. A 300 ml glass-lined stainless steel autoclave with a temperature control device, an agitator and a hydrogen addition point is used. A butadiene-acrylonitrile polymer latex with a limited acrylonitrile content of about 38% (weight) and a Mooney viscosity (ML1+4@100°C) of about 29 is used. The solid content of the latex is 14.3% (weight). The average diameter of the polymer particles in the latex is about 75 nm. 50 ml of this latex, 100 ml of water, 0.0378 g of catalyst RhCl(PPh3)3 and 0.594 g of PPh3 are charged into the reactor. The latex is then degassed with hydrogen. The temperature is raised to 145°C and the hydrogen pressure is increased to 900 psi (6.1 MPa). After 87 hours, the degree of hydrogenation reaches 92%. No gel was produced and the obtained polymer was soluble in methyl ethyl ketone. The main problem of this technology is that the reaction rate is slow, resulting in a very long time, and the catalytic efficiency of the catalyst is low.
[0027] CN104428325, CN111019018 and CN111690080 provide the selective hydrogenation of carbon-carbon double bonds of nitrile latex by directly adding solid ruthenium or osmium hydrogenation catalyst into latex or mixing the catalyst with latex in batches. The main problem of this series of technologies is that the solid ruthenium or osmium catalyst is non-water-soluble. When directly added into latex, the catalyst has poor dispersion effect and is difficult to enter micelles. The catalyst dosage is large and the catalytic effect is poor.
[0028] CN111479831, CN110627928, CN11303317, CN111905821 and CN112940185 add solid ruthenium or osmium hydrogenation catalyst with the help of emulsifier to carry out selective hydrogenation of carbon-carbon double bonds of latex. The main problem of this series of technologies is that either the solid content of latex needs to be reduced to improve the dispersion effect of catalyst, which affects production efficiency; or a large amount of emulsifier needs to be added to help the catalyst disperse. However, if a large amount of emulsifier is added, the post-processing of latex will be greatly affected, and the residual emulsifier will affect the performance of solid glue. At the same time, the post-processing will generate a large amount of wastewater, polluting the environment.
[0029] In summary, there are two main approaches to the research in the above fields: one approach is similar to traditional solution catalytic hydrogenation, which hydrogenates the polymer in the form of latex; the other approach involves the use of hydrazines, etc., in which the hydrogen source is generated on-site as a result of the redox reaction. At present, both approaches have encountered bottlenecks in order to obtain fast hydrogenation reaction rates, high conversion rates and eliminate gel formation.
[0030] At present, ethylene-acrylonitrile copolymerization and NBR emulsion polymerization are still in the laboratory research stage, and there is no precedent for industrial application. The only industrialized method is the NBR solution hydrogenation method, which is adopted by Arlanxeo, Japan Zoon and Zanan Technology. Due to the differences in the catalytic systems used in the hydrogenation reaction, Japan Zoon mainly uses palladium / silica heterogeneous catalysts with silica as carrier to prepare HNBR; Arlanxeo mainly uses rhodium homogeneous catalysts RhCl(P(C6H5)3)3 to prepare HNBR; Zanan mainly uses ruthenium catalysts to prepare HNBR. Summary of the invention
[0031] In view of this, the object of the present invention is to provide a catalyst composition, a method for selective hydrogenation of conjugated diene latex, hydrogenated conjugated diene latex and application thereof. The catalyst composition provided by the present invention can efficiently carry out selective hydrogenation of carbon-carbon double bonds of conjugated diene latex, can effectively reduce the amount of main catalyst and co-catalyst, has mild hydrogenation conditions, lower co-catalyst residual amount, good vulcanized rubber performance, high production efficiency, and no gel problem.
[0032] The present invention provides a catalyst composition, comprising: a main catalyst and a first co-catalyst, wherein the main catalyst is a ruthenium complex hydrogenation catalyst and / or an osmium complex hydrogenation catalyst, and the chemical structure of the first co-catalyst contains one or more of N, O, a carbon-carbon double bond and a carbon-carbon triple bond.
[0033] Preferably, the chemical structure of the main catalyst is at least one of formula (I), formula (II) and formula (III):
[0034]
[0035] In formula (I), M is ruthenium or osmium; X 1 and X 2 are the same or different anionic ligands; L is an uncharged electron donor; two Rs are the same or different groups independently selected from alkyl, alkyl derivatives, cycloalkyl, cycloalkyl derivatives, alkenyl, alkenyl derivatives, alkynyl, alkynyl derivatives, aryl, aryl derivatives, carboxylate, carboxylate derivatives, alkoxy, alkoxy derivatives, alkenyloxy, alkenyloxy derivatives, alkynyloxy, alkynyloxy derivatives, aryloxy, aryloxy derivatives, alkoxycarbonyl, alkoxycarbonyl derivatives, alkylamino, alkylamino derivatives, thioamino, thioamino derivatives, thioaryl, thioaryl derivatives, alkylsulfonyl, alkylsulfonyl derivatives, alkylsulfinyl or alkylsulfinyl derivatives, and the derivative is a group formed by replacing the corresponding non-derivative group with one or more of alkyl, halogen, alkoxy, aryl and heteroaryl;
[0036]
[0037] In formula (II), M is ruthenium or osmium; X 1 and X 2 are the same or different anionic ligands; L is an uncharged electron donor; Y is selected from O, S, NR 1 or PR 1 ; R 1 R is selected from alkyl, alkyl derivatives, cycloalkyl, cycloalkyl derivatives, alkenyl, alkenyl derivatives, alkynyl, alkynyl derivatives, aryl, aryl derivatives, alkoxy, alkoxy derivatives, alkenyloxy, alkenyloxy derivatives, alkynyloxy, alkynyloxy derivatives, aryloxy, aryloxy derivatives, alkoxycarbonyl, alkoxycarbonyl derivatives, alkylamino, alkylamino derivatives, alkylthio, alkylthio derivatives, arylthio, arylthio derivatives, alkylsulfonyl, alkylsulfonyl derivatives, alkylsulfinyl or alkylsulfinyl derivatives, wherein the derivative is a group formed by replacing the corresponding non-derivative group with one or more of alkyl, halogen, alkoxy, aryl and heteroaryl; R 2 , R 3 , R 4 and R 5 independently selected from hydrogen, halogen, nitro, CF3, C1-C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 Alkylsulfinyl; R 6 is selected from hydrogen, alkyl, alkenyl, alkynyl or aryl;
[0038]
[0039] In formula (III), the dotted line represents a saturated bond or an unsaturated bond, and α and β cannot be unsaturated bonds at the same time; M is ruthenium or osmium; X 1 and X 2 are the same or different anionic ligands; L is an uncharged electron donor; when α is a saturated bond, L 2 NR 7 R 8 , PR 7 R 8 、N=CR 7 R 8 or R 7 C=NR 8 , R 7 and R 8 independently selected from unsubstituted, substituted or heteroatom-containing C1-C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl or C6~C 24 The aromatic group, or R 7 and R 8 are non-aromatic ring structures respectively; when α is a double bond, L 2 NR 7 or PR 7 , R 7 is selected from unsubstituted, substituted or heteroatom-containing C1-C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl or C6~C 24 The aromatic group, or R 7 is a non-aromatic ring structure; A and B are independently selected from hydrocarbons, substituted hydrocarbons, hydrocarbons containing heteroatoms, or hydrocarbons with substituted groups and heteroatoms, or A and B are atoms in an aromatic ring; m represents 0 or 1; n represents 0 or 1; R 6 is selected from hydrogen, alkyl, alkenyl or aryl.
[0040] Preferably, in formula (I), formula (II) and formula (III), M is ruthenium; X 1 and X 2 independently selected from hydrogen, halogen, pseudohalogen, linear or branched C1-C 30 Alkyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C6~C 24 Aryloxy, C3~C 20 Alkyl diketone, C6~C 24 Aryl diketone, C1~C 20 Carboxylates, C6~C 24 Alkyl sulfonate, C6~C 24 Aryl sulfonate, C1~C 20 Alkyl mercaptan, C6~C 24 Aromatic thiols, C1~C 20 Alkylsulfonyl or C1-C 20 -alkylsulfinyl; L is selected from phosphine, sulfonated phosphine, phosphate, hypophosphorous acid, phosphite, phosphonate, arsine, stibine, ether, amine, amide, sulfoxide, carboxyl, nitrite, pyridine, thioether or N-heterocyclic carbene ligand.
[0041] Preferably, in formula (I), formula (II) and formula (III), the X 1 and X 2 Independently selected from chlorine, CF3COO, CH3COO, CFH2COO, (CH3)3CO, (CF3)2(CH3)CO, (CF3)(CH3)2CO, phenoxy, methoxy, ethoxy, toluenesulfonate (p-CH3-C6H4-SO3), methanesulfonic acid (CH3SO3) or trifluoromethylsulfonate (CF3SO3); L is at least one of the structures shown in formula (IV-a) to formula (IV-f):
[0042]
[0043] Among them, R 9 , R 10 , R 11 and R 12 Independently selected from hydrogen, linear or branched C1-C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C7~C 25 Alkyl, C2~C 20 Heterocyclic aromatic group, C2~C 20 Heterocyclic ring, C1~C20 Alkoxy, C2~C 20 Alkenyl, C2~C 20 Alkynyloxy, C6~C 20 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylthio, C6~C 20 R is arylthio, -Si(R')3, -O-Si(R')3, -OC(=O)R', -C(=O)R', -C(=O)N(R')2, -NR-C(=O)-N(R')2, -SO2N(R')2, -S(=O)R', -S(=O)2R', -OS(=O)2R', halogen, nitro or cyano, R' is selected from hydrogen, alkyl, cycloalkyl, alkenyl, alkynyl, aryl or heteroaryl; R 13 , R 14 and R 15 Independently selected from C1 to C 20 of alkyl.
[0044] Preferably, the main catalyst comprises at least one of the following structural complexes:
[0045]
[0046] Preferably, the first co-catalyst is one or more of esters, ethers, ketones, amines, carbamates, olefins and alkynes.
[0047] Preferably, the first co-catalyst is one or more of aliphatic monocarboxylic acid alkyl esters, aromatic monocarboxylic acid alkyl esters, aliphatic polycarboxylic acid alkyl esters, aromatic polycarboxylic acid alkyl esters, polyol alkyl esters, polyol cycloalkyl esters, polyol aryl esters, polyol alkylaryl esters, aliphatic ethers, cycloaliphatic ethers, aliphatic diethers, aliphatic ketones, aliphatic amines, aliphatic diamines, olefins and alkynes.
[0048] Preferably, the first co-catalyst is C1-C 20 Saturated fatty acid alkyl esters, C7~C 24 Aromatic carboxylic acid alkyl esters, C2~C 20 -Diol aromatic ester, C2~C 20 Fatty ethers, C3~C 20 Cyclic ethers, C5~C 20 Aliphatic diethers, C3~C 20 Saturated fatty ketones, C3~C 20 Saturated fatty amines, C3~C 20 Saturated fatty diamines, C2~C 20 Olefins and C2~C 20 One or more of the alkynes.
[0049] Preferably, the molar ratio of the main catalyst to the first co-catalyst is 1:(20-100).
[0050] Preferably, the catalyst composition further comprises a second co-catalyst, and the second co-catalyst is one or more of carboxylates, sulfonates and phosphates.
[0051] Preferably, the second co-catalyst is one or more of non-emulsifier type carboxylates, emulsifier type carboxylates, non-emulsifier type sulfonates, emulsifier type sulfonates, non-emulsifier type phosphate salts and emulsifier type phosphate salts.
[0052] Preferably, the non-emulsified formulation carboxylate is one or more of formates, acetates, propionates, butyrates, valerates, oxalates, malonates, succinates, glutarates, triacrylic acid salts, trisuccinates, triglutarates, maleates, tartrates, fumarates, malates, amino acid salts, cyclopentaneates, alginates, gluconates, crotonates, itaconates, citrates, mesaconic acids, aromatic carboxylates, heteroaromatic ring carboxylates, imidazoline carboxylates, pyruvates, epoxysuccinates, salicylates, fluorenedioates, hydroxypropionates, levulinates, furandicarboxylates, acrylates, methacrylates and trifluoroformates;
[0053] The emulsifier-type carboxylate is one or more of resinate, modified resinate, alkanoyl amino acid salt, fatty acid polypeptide condensate, acyl lactylate and long-chain alkyl carboxylate of C8 or above;
[0054] The non-emulsifier type sulfonate is methanesulfonate, trifluoromethylsulfonate, ethanesulfonate, perfluoroethanesulfonate, propanesulfonate, perfluoropropanesulfonate, hydroxypropanesulfonate, butylsulfonate, perfluorobutylsulfonate, hydroxybutylsulfonate, toluenesulfonate, dinitrotoluenesulfonate, styrenesulfonate, vinylsulfonate, allylsulfonate, methylallylsulfonate, perfluorosulfonic acid polymer, aromatic sulfonate, heteroaromatic ring sulfonate, cycloalkanesulfonate, hydroxybenzoate, One or more of 2-(2-aminoethyl)aminoethanesulfonate, N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate, N-tris(hydroxymethyl)methyl-2-aminoethanesulfonate, aminosulfonate, aminoaromaticsulfonate, ethylenediamineethanesulfonate, chrysinsulfonate, anthraquinonesulfonate, diaminoformylsulfonate, quinocinonesulfonate, thiazolesulfonate, imidazolinesulfonate, allylimidazolinesulfonate, triazolonesulfonate, triazinesulfonate and flavonesulfonate;
[0055] The emulsifier type sulfonate is one or more of alkyl aryl sulfonate, alkyl diphenyl oxide disulfonate, α-hydroxy sulfonate, α-olefin sulfonate, petroleum sulfonate, α-sulfomonocarboxylate, α-sulfomonocarboxylate derivative, fatty acid sulfoalkyl ester salt derivative, fatty acid sulfoalkyl amide salt derivative, succinate sulfonate, lignin sulfonate, alkyl glyceryl ether sulfonate, 2-aminoethanesulfonate, 2-aminoethanesulfonate derivative and C8 or higher long-chain alkyl sulfonate;
[0056] The non-emulsifier type phosphate salt is monomethyl phosphate, monoethyl phosphate, monobutyl phosphate, dimethyl phosphate, diethyl phosphate, dibutyl phosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, monophenyl phosphate, diphenyl phosphate, triphenyl phosphate, mono-p-tolyl phosphate, di-p-tolyl phosphate, tri-p-tolyl phosphate, mono-o-tolyl phosphate, di-o-tolyl phosphate, tri-o-tolyl phosphate, mono-m-tolyl phosphate, di-m-tolyl phosphate, tri-m-tolyl phosphate, mono-p-isopropylphenyl phosphate, di-p-isopropylphenyl phosphate, tri-p-isopropylphenyl phosphate, mono-p-tert-butyl phosphate phenyl ester salt, di-p-tert-butylphenyl phosphate salt, tri-p-tert-butylphenyl phosphate, mono-p-methoxyphenyl phosphate salt, di-p-methoxyphenyl phosphate salt, tri-p-methoxyphenyl phosphate, phenyl dimethyl phosphate, phenyl diethyl phosphate, phenyl dibutyl phosphate, diphenyl methyl phosphate, diphenyl ethyl phosphate, diphenyl butyl phosphate, p-tolyl dimethyl phosphate, p-tolyl diethyl phosphate, p-tolyl dibutyl phosphate, o-tolyl dimethyl phosphate, o-tolyl diethyl phosphate, o-tolyl dibutyl phosphate, m-tolyl dimethyl phosphate, m-tolyl diethyl phosphate, m-tolyl dibutyl phosphate, di-p-tolyl methyl phosphate Ester, di-p-tolyl ethyl phosphate, di-p-tolyl butyl phosphate, di-o-tolyl methyl phosphate, di-o-tolyl ethyl phosphate, di-o-tolyl butyl phosphate, di-m-tolyl methyl phosphate, di-m-tolyl ethyl phosphate, di-m-tolyl butyl phosphate, di-p-isopropylphenyl methyl phosphate, di-p-isopropylphenyl ethyl phosphate, di-p-isopropylphenyl butyl phosphate, di-p-isopropylphenyl dimethyl phosphate, di-p-isopropylphenyl diethyl phosphate, di-p-isopropylphenyl dibutyl phosphate, di-p-isopropylphenyl dimethyl phosphate, di-p-isopropylphenyl diethyl phosphate, di-p-isopropylphenyl dibutyl phosphate, di-p-isopropylphenyl methyl phosphate, di-p-isopropylphenyl ethyl phosphate, phosphorus One or more of di-p-tert-butylphenyl butyl phosphate, phenyl di-p-tolyl phosphate, phenyl di-p-isopropylphenyl phosphate, phenyl di-p-tert-butylphenyl phosphate, p-tolyl diphenyl phosphate, p-tolyl p-diisopropylphenyl phosphate, p-tolyl p-di-tert-butylphenyl phosphate, o-tolyl p-diisopropylphenyl phosphate, o-tolyl p-di-tert-butylphenyl phosphate, m-tolyl p-diisopropylphenyl phosphate, m-tolyl p-di-tert-butylphenyl phosphate, p-isopropylbenzene di-p-tolyl phosphate, p-isopropylbenzene di-o-tolyl phosphate, p-isopropylbenzene di-m-tolyl phosphate, p-isopropylbenzene di-p-phenyl phosphate and p-isopropylbenzene di-p-tert-butylphenyl phosphate;
[0057] The emulsifier type phosphate salt is one or more of fatty alcohol polyvinyl ether phosphate monoester salt, fatty alcohol polyvinyl ether phosphate diester salt, alkylphenol polyoxyethylene ether phosphate monoester salt, alkylphenol polyoxyethylene ether phosphate diester salt, alcohol ether phosphate ester salt, phenol ether phosphate ester salt, long-chain alkyl phosphate monoester salt of C8 or above, and long-chain alkyl phosphate diester salt of C8 or above.
[0058] Preferably, the molar ratio of the main catalyst to the second co-catalyst is 1:(100-10000).
[0059] Preferably, the catalyst composition is in liquid form.
[0060] Preferably, the catalyst composition further comprises a solvent.
[0061] The present invention provides a method for selective hydrogenation of conjugated diene latex, comprising the following steps:
[0062] In the presence of the catalyst composition described in the above technical solution, the conjugated diene latex is selectively hydrogenated to obtain hydrogenated conjugated diene latex.
[0063] Preferably, the polymer in the conjugated diene latex contains at least one repeating unit of a C4-C6 conjugated diene.
[0064] Preferably, the polymer in the conjugated diene latex further contains repeating units of at least one other copolymerizable monomer.
[0065] Preferably, the polymer in the conjugated diene latex is a copolymer of 1,3-butadiene and acrylonitrile.
[0066] Preferably, the main catalyst is used in an amount of 0.001 to 5 wt% of the conjugated diene latex; and the first co-catalyst is used in an amount of 0.01 to 5 wt% of the conjugated diene latex.
[0067] Preferably, when the catalyst composition includes a second co-catalyst, the amount of the second co-catalyst is 0.1 to 10 wt % based on the mass of the conjugated diene latex.
[0068] Preferably, the temperature of the selective hydrogenation is 35 to 200° C.; the time of the selective hydrogenation is 10 min to 24 h; and the hydrogen pressure of the selective hydrogenation is 0.5 to 35 MPa.
[0069] The present invention provides a hydrogenated conjugated diene latex, which is prepared according to the method described in the above technical scheme.
[0070] The present invention provides an application of the hydrogenated conjugated diene latex described in the above technical solution in dipping, adhesive, coating, film formation or preparation of composite materials.
[0071] The present invention provides a shaped product, the components of which include the hydrogenated conjugated diene latex described in the above technical solution.
[0072] Preferably, the shaped article comprises one or more of a sealing strip, a sealing gasket, a belt, a hose, a bearing pad, a baffle, a wellhead seal, a valve seal, a cable jacket, a wheel, a roller, an in-situ gasket and a pipe seal.
[0073] Compared with the prior art, the present invention provides a catalyst composition, a method for selective hydrogenation of conjugated diene latex, hydrogenated conjugated diene latex and its application. The catalyst composition provided by the present invention comprises: a main catalyst and a first co-catalyst, preferably also comprising a second co-catalyst, the main catalyst being a ruthenium complex hydrogenation catalyst and / or an osmium complex hydrogenation catalyst, the chemical structure of the first co-catalyst containing one or more of N, O, carbon-carbon double bonds and carbon-carbon triple bonds, and the second co-catalyst being one or more of carboxylates, sulfonates and phosphates. The catalyst composition provided by the present invention can efficiently carry out selective hydrogenation of carbon-carbon double bonds of conjugated diene latex, can effectively reduce the amount of the main catalyst and co-catalyst, the hydrogenation conditions are mild, the co-catalyst residue is lower, the vulcanized rubber has good performance, high production efficiency, and no gel problem. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0075] Figure 1 is an ultraviolet absorption spectrum of the catalyst composition provided by an embodiment of the present invention;
[0076] Figure 2 This is a sample photo of the catalyst composition provided in the examples of the present invention. DETAILED DESCRIPTION
[0077] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0078] The present invention provides a catalyst composition, comprising: a main catalyst (a) and a first co-catalyst (b), preferably also comprising a second co-catalyst (c), wherein the main catalyst (a) is a ruthenium complex hydrogenation catalyst and / or an osmium complex hydrogenation catalyst, the chemical structure of the first co-catalyst contains one or more of N, O, a carbon-carbon double bond and a carbon-carbon triple bond, and the second co-catalyst is one or more of a carboxylate, a sulfonate and a phosphate.
[0079] In the present invention, the chemical structure of the main catalyst (a) is preferably at least one of formula (I), formula (II) and formula (III):
[0080]
[0081]
[0082] Wherein, M is a Group VIII metal element, preferably ruthenium or osmium.
[0083] X 1 and X 2 are the same or different anionic ligands, preferably, X 1 and X 2 independently selected from hydrogen, halogen, pseudohalogen, linear or branched C1-C 30 Alkyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C6~C 24 Aryloxy, C3~C 20 Alkyl diketone, C6~C 24 Aryl diketone, C1~C 20 Carboxylates, C6~C 24 Alkyl sulfonate, C6~C 24 Aryl sulfonate, C1~C 20 Alkyl mercaptan, C6~C 24 Aromatic thiols, C1~C 20 Alkylsulfonyl or C1~C 20 The above-listed groups may also be further substituted by one or more groups, such as halogen (preferably fluorine), C1~C 10 Alkyl, C1~C 10 Alkoxy or C6~C 24 In addition, the above substituents may be substituted in turn to some extent chemically by one or more substituents, preferably comprising halogen (especially fluorine), C1~C5 alkyl, C1~C5 alkoxy or phenyl.
[0084] In a preferred embodiment of the present invention, X 1 and X 2independently selected from halogen (especially fluorine, chlorine, bromine, iodine), benzoic acid, C1-C5 carboxylate, C1-C5 alkyl, phenoxy, C1-C5 alkoxy, C1-C5 alkylthiol, C6-C 14 Aromatic thiophenols, C6~C 14 Aryl or C1~C5 alkyl sulfonate.
[0085] In a particularly preferred embodiment, X 1 and X 2 independently selected from chlorine, CF3COO, CH3COO, CFH2COO, (CH 3) 3CO, (CF3)2(CH3)CO, (CF3)(CH3)2CO, phenoxy, methoxy, ethoxy, toluenesulfonate (p-CH3-C6H4-SO3), methanesulfonic acid (CH3SO3) or trifluoromethanesulfonate (CF3SO3).
[0086] L represents a ligand, preferably an uncharged electron donor, and the ligand L is preferably selected from one or more of phosphine, sulfonated phosphine, phosphate, hypophosphorous acid, phosphite, phosphonate, arsine, stibine, ether, amine, amide, sulfoxide, carboxyl, nitrite, pyridine, thioether and N-heterocyclic carbene ligands;
[0087] In the present invention, the term "hypophosphorous acid" includes phenyldiphenylphosphorous acid, cyclohexyldicyclohexylphosphorous acid, isopropyldiisopropylphosphorous acid and methyldiphenylphosphorous acid.
[0088] The term "phosphite" includes triphenylphosphite, tricyclohexylphosphite, tri-tert-butylphosphite, triisopropylphosphite and methyldiphenylphosphite.
[0089] The term "antimony" includes: triphenyl Tricyclohexyl and trimethyl
[0090] The term "sulfoxide" includes: (CH3)2S(=O) and (C6H5)2S=O.
[0091] The term "thioether" includes: CH3SCH3, C6H5SCH3, CH3OCH2CH2SCH3 and tetrahydrothiophene.
[0092] The term "pyridyl ligand" is used as a generic term for all ligands based on pyridine or its derivatives.
[0093] The term "pyridyl ligand" includes pyridine itself, methylpyridines (such as α-, β- and γ-methylpyridine), dimethylpyridines (such as 2,3-, 2,4-, 2,5-, 2,6-, 3,4- and 3,5-dimethylpyridine), trimethylpyridine (2,4,6-trimethylpyridine), trifluoromethylpyridine, phenylpyridine, 4-(dimethylamino)-pyridine, chloropyridine, bromopyridine, nitropyridine, quinoline, pyrimidine, pyrrole, imidazole and phenylimidazole.
[0094] In the present invention, L in the general expression (I) (II) or (II) represents phosphine as an electron donor, and its general expression is preferably:
[0095]
[0096] Among them, R 13 , R 14 and R 15 are the same or different, preferably the same, preferably C1 to C 20 The alkyl group is more preferably methyl, ethyl, n-n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, neopentyl, 1-ethylpropyl, n-hexyl, neopentyl, or a C3-C8 cycloalkyl group; the most preferred are cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl or cyclooctyl, C1-C8 20 Alkoxy, substituted or unsubstituted C6~C 20 Aryl; most preferably phenyl, biphenyl, naphthalene, phenanthrene, anthracene, tolyl, 2,6-dimethylphenyl, trifluoromethyl, C6~C 20 an aryloxy group, a C2-C 20 Heteroaryl, C2-C 20 The heterocyclic group may be halogen; the halogen is preferably fluorine.
[0097] If L represents a phosphine of the general formula (IV-f) and the structure shown in formula (I), (II) or formula (III) serves as an electron-donating ligand, such phosphine is preferably PPh3, P(p-Tol)3, P(o-Tol)3, PPh(CH3)2, P(CF3)3, P(p-FC6H4)3, P(p-CF3C6H4)3, P(C6H4-SO3Na)3, P(CH2C6H4-SO3Na)3, P(isopropyl)3, P(CHCH3(CH2CH3))3, P(cyclopentyl)3, P(cyclohexyl)3, P(neopentyl)3 or P(neopentyl)3, wherein Ph represents phenyl and Tol represents tolyl.
[0098] An n-heterocyclic carbene ligand is a cyclic carbene ligand having at least one nitrogen as a heteroatom in the ring. The ring may be substituted in different ways. Preferably, the substitution pattern provides a certain degree of steric crowding.
[0099] In the present invention, the n-heterocyclic carbene ligands (hereinafter referred to as "NHC-ligands") are preferably based on imidazoline or imidazolinidine groups.
[0100] In the present invention, L is preferably an NHC-ligand, usually at least one of the structures shown in formula (IV-a) to formula (IV-e):
[0101]
[0102] Among them, R 8 , R 9 , R 10 , R 11 Independently selected from hydrogen, linear or branched C1-C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C7~C 25 Alkyl, C2~C 20 Heterocyclic aromatic group, C2~C 20 Heterocyclic ring, C1~C 20 Alkoxy, C2~C 20 Alkenyl, C2~C 20 Alkynyloxy, C6~C 20 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylthio, C6~C 20 -S(=O)R', -S(=O)2R', -OS(=O)2R', halogen, nitro or cyano.
[0103] In the above R 8 , R 9 , R 10 and R 11 In the group, R' is the same or different and represents hydrogen, alkyl, cycloalkyl, alkenyl, alkynyl, aryl or heteroaryl.
[0104] In the representative formulas (IV-a) to (IV-e), the carbon atom bonded to the ruthenium metal center is in the form of a carbene.
[0105] Optionally, R 9 , R 10 , R 11 and R 12 One or more of the above may be independently substituted by one or more substituents, wherein the substituents are preferably linear or branched C1-C 10 Alkyl, C3-C8 cycloalkyl, C1-C 10 Alkoxy, C6~C 24 Aryl, C2~C 20 Heteroaryl, C2~C 20 or a group containing hydroxyl, thiol, thioether, ketone, aldehyde, ester, ether, amine, imine, amide, nitro, carboxylic acid, disulfide, carbonate, isocyanate, carbodiimide, alkoxycarbonyl, carbamate or halogen, wherein the above substituents may in turn be substituted to a certain extent chemically by one or more substituents, preferably containing halogen (especially chlorine or bromine groups), C1-C5 alkyl, C1-C5 alkoxy and phenyl.
[0106] For the sake of clarity, it should be added that the NHC-ligand structures of the general formulae (IV-a) and (IV-b) depicted in the present invention are identical to the structures (IVa-(i)) and (IVb-(i)) of such NHC-ligands frequently encountered in the literature, respectively, and the carbene character of the NHC-ligands should be emphasized. The same applies to the further structures (IV-c) to (IV-e) and the preferred structures described below in relation to (IV-c) to (IV-e).
[0107]
[0108] In a preferred NHC-ligand of the catalyst represented by the general expression, R 9 and R 10 are the same or different, they represent hydrogen, C6~C 24 Aryl (preferably phenyl), linear or branched C1-C 10 The alkyl group is more preferably methyl, ethyl, n-propyl, i-propyl, n-butyl, sec-butyl, i-butyl or tert-butyl, or forms a cycloalkyl or aryl structure bound to a carbon atom.
[0109] Preferably and more preferably, R 9 and R 10 One or more of the above may be independently substituted by one or more substituents, wherein the substituents are preferably linear or branched C1-C 10 Alkyl, straight chain or branched C1~C 10 Alkoxy, C3-C8 cycloalkyl, C6-C24 or a group containing hydroxy, thiol, thioether, ketone, aldehyde, ester, ether, amine, imine, amide, nitro, carboxylic acid, disulfide, carbonate, isocyanate, carbodiimide, alkoxycarbonyl, carbamate or halogen, wherein these substituents in turn may be substituted by one or more substituents, preferably containing halogen (especially chlorine or bromine), C1-C5 alkyl, C1-C5 alkoxy or phenyl.
[0110] In a further preferred NHC-ligand of the catalyst represented by the general expression, R 11 and R 12 are the same or different, preferably straight chain or branched C1~C 10 Alkyl (preferably i-propyl or neopentyl), C3~C 10 cycloalkyl (preferably adamantyl), substituted or unsubstituted C6~C 24 an aryl group (preferably phenyl, 2,6-isopropylbenzene, 2,6-xylyl or 2,4,6-trimethylphenyl), a C1-C 10 Alkyl sulfonate or C6-C 10 -sulfonic acid.
[0111] Preferably, R 11 and R 12 It may be substituted by one or more substituents selected from linear or branched C1-C 10 Alkyl, straight chain or branched C1~C 10 Alkoxy, C3-C8 cycloalkyl, C6-C 24 or a group containing hydroxy, thiol, thioether, ketone, aldehyde, ester, ether, amine, imine, amide, nitro, carboxylic acid, disulfide, carbonate, isocyanate, carbodiimide, alkoxycarbonyl, carbamate or halogen, wherein these substituents in turn may be substituted by one or more substituents, preferably containing halogen (especially chlorine or bromine), C1-C5 alkyl, C1-C5 alkoxy or phenyl.
[0112] In a further preferred NHC-ligand of the catalyst represented by the general expression, R 9 and R 10 are the same or different, they represent hydrogen, C6~C 24 Aryl (preferably phenyl), straight chain or branched C1~C 10 The alkyl group is more preferably a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cycloalkyl group or an aryl group structure bound to a carbon atom.
[0113] R 11 and R 12are the same or different, preferably straight chain or branched C1~C 10 Alkyl (preferably i-propyl or neopentyl), C3~C 10 cycloalkyl (preferably adamantyl), substituted or unsubstituted C6~C 24 Aryl (preferably phenyl, 2,6-isopropylphenyl, 2,6-xylyl or 2,4,6-trimethylphenyl), C1-C 10 Alkyl sulfonate or C6~C 10 of sulfonic acid.
[0114] Particularly preferably, the NHC-ligand has the following structures (Va) to (Vu), wherein "Ph" represents in each case a phenyl group, "Bu" represents in each case a butyl group, i.e. any one of n-butyl, tert-butyl, isobutyl or sec-butyl. "Mes" represents in each case a 2,4,6-trimethylphenyl group, "Dipp" represents in all cases a 2,6-diisopropylbenzene, and "Dimp" refers to in each case a 2,6-dimethylphenyl group:
[0115]
[0116]
[0117] NHC-ligands contain not only an "N" (nitrogen) but also an "O" (oxygen) in the ring, which makes R 8 , R 9 , R 10 and / or R 11 The replacement pattern tends to provide a certain degree of spatial crowding.
[0118] (i) For a procatalyst having formula (I):
[0119] Wherein, R is selected from one or more of hydrogen, alkyl, cycloalkyl, alkenyl, alkynyl, aryl, alkoxy, alkenyloxy, alkynyloxy, aryloxy, alkoxycarbonyl, alkylamino, alkylthio, arylthio, alkylsulfonic acid and alkylsulfinyl; these substituents may be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups.
[0120] Preferably, the substituent R is usually hydrogen, C1-C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups.
[0121] (ii) For the procatalyst having formula (II):
[0122] Y is selected from O, S, NR 1 or PR 1 Group, where R 1 One or more selected from alkyl, cycloalkyl, alkenyl, alkynyl, aryl, alkoxy, alkenyloxy, alkynyloxy, aryloxy, alkoxycarbonyl, alkylamino, alkylthio, arylthio, alkylsulfonyl and alkylsulfinyl; these substituents may be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups.
[0123] Preferably, the substituent R 1 Usually C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups.
[0124] R 1 More preferably, C3 to C 20 Cycloalkyl, C6~C 24 aromatic, straight chain or branched C1~C 30The alkyl radical R is an alkyl radical, the latter being interrupted, where appropriate, by one or more double or triple bonds or by one or more heteroatoms, preferably oxygen or nitrogen. 1 Particularly preferred are linear or branched C1-C 12 of alkyl.
[0125] Among them, C3~C 20 The cycloalkyl group includes, for example, one or more of a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group.
[0126] A C1~C 12 The alkyl group of R can be, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, neopentyl, 1-ethylpropyl, n-hexyl, n-heptyl, n-octyl, n-decyl or n-dodecyl. In particular, R 1 It is methyl or isopropyl.
[0127] C6~C 24 The aryl group is an aromatic group having 6 to 24 backbone carbon atoms. As a preferred monocyclic, bicyclic or tricyclic carbocyclic aryl group having 6 to 10 backbone carbon atoms, benzene, biphenyl, naphthalene, phenanthrene, anthracene or anthracene can be used to synthesize.
[0128] In the present invention, R 2 , R 3 , R 4 and R 5 independently selected from hydrogen, organic or inorganic groups;
[0129] In one suitable embodiment, R 2 , R 3 , R 4 , R 5 are the same or different and each can be hydrogen, halogen, nitro, CF3, alkyl, cycloalkyl, alkenyl, alkynyl, aryl, alkoxy, alkenyloxy, alkynyloxy, aryloxy, alkoxycarbonyl, alkylamino, alkylthio, hydroxyethyl aryl sulfide, alkylsulfonyl or alkylsulfinyl, and these substituents can be selectively substituted by one or more alkyl, alkoxy, halogen, aryl or heteroaryl groups.
[0130] Preferably, R 2 , R 3 , R 4 , R 5 are usually the same or different, and each can be hydrogen, halogen (preferably chlorine or bromine), nitro, CF3, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 These substituents may be replaced by one or more C1~C 30 Alkyl, C1~C 20 Alkoxy, halogen, C6~C 24 The aryl or heteroaryl group is optionally substituted.
[0131] In a particularly preferred embodiment, R 2 , R 3 , R 4 , R 5 can be the same or different, each can be a nitro, straight chain or branched C1~C 30 Alkyl, C5~C 20 Cycloalkyl, straight chain or branched C1~C 20 Alkoxy or C6~C 24 aryl (preferably phenyl or naphthyl), wherein C1~C 30 Alkyl and C1~C 20 The alkoxy groups may be substituted by one or more double or triple bonds or by one or more heteroatoms, preferably oxygen or nitrogen.
[0132] In addition, two or more groups R 2 , R 3 , R 4 or R 5 It can also be linked via aliphatic or aromatic structures. 3 , R 4 As well as connecting their carbon atoms on the phenyl ring in the expression, a fused phenyl ring can be formed, and overall, a naphthyl structure is produced.
[0133] According to the present invention, R 6 is one or more selected from hydrogen, alkyl, alkenyl, alkynyl and aryl; R 6 Preferably selected from hydrogen, C1-C 30 Alkyl, C2~C 20 Alkenyl, C2~C 20Alkynyl or C6~C 24 The aryl group; R 6 Hydrogen is particularly preferred.
[0134] (iii) For the procatalyst having formula (III):
[0135] The dotted lines represent saturated bonds or unsaturated bonds, such as double bonds; α and β cannot be double bonds at the same time; A and B are independent linking groups, each from a hydrocarbon, such as C1~C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C5~C 50 Aromatic groups, C6~C 24 Alkyl, C6~C 24 or substituted hydrocarbons, such as C1~C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, substituted C5~C 50 Aromatic groups, C6~C 24 Alkyl, substituted C6~C 24 or hydrocarbons containing heteroatoms, such as C1~C 20 Heteroalkyl, C2~C 20 heteroalkenyl, C2~C 20 Heteroalkynyl, C5~C 50 Heteroaromatic, C6~C 24 Heteroalkylaryl, C6~C 24 or a heteroatom-containing hydrocarbon containing a substituent, such as a C1-C 20 Heteroalkyl, C2~C 20 heteroalkenyl, C2~C 20 Heteroalkynyl, substituted C5~C 50 Heteroaromatic groups, C6~C 24 Heteroalkylaryl, C6~C 24 or -O-, -S-, -NR 8 -or-PR 8 -, R 8 Selected from hydrocarbons, such as C1~C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C5~C 50 Aromatic groups, C6~C 24 Alkyl, C6~C 24or substituted hydrocarbons, such as C1~C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, substituted C5~C 50 Aromatic groups, C6~C 24 Alkyl, substituted C6~C 24 or hydrocarbons containing heteroatoms, such as C1~C 20 Heteroalkyl, C2~C 20 heteroalkenyl, C2~C 20 Heteroalkynyl, C5~C 50 Heteroaromatic, C6~C 24 Heteroalkylaryl, C6~C 24 or a heteroatom-containing hydrocarbon containing a substituent, such as a C1-C 20 Heteroalkyl, C2~C 20 heteroalkenyl, C2~C 20 Heteroalkynyl, substituted C5~C 50 Heteroaromatic groups, C6~C 24 Heteroalkylaryl, C6~C 24 The heteroaryl group.
[0136] The overall structure composed of the A and B organic groups is preferably as shown in (A) to (G):
[0137]
[0138] As a preferred embodiment, when α is a saturated bond, L 2 NR 7 R 8 , PR 7 R 8 、N=CR 7 R 8 or R 7 C=NR 8 , R 7 , R 8 independently selected from unsubstituted, substituted or heteroatom-containing C1-C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl or C5~C 24 The aromatic group, or R 7 and R 8 can be non-aromatic ring structures, such as piperidinyl (including substituted piperidinyl); m represents 0 or 1; n represents 0 or 1; R6 Any one selected from hydrogen, alkyl, alkenyl or aryl.
[0139] As a preferred embodiment, the structural formula of the main catalyst is formula (VI) or formula (VII):
[0140]
[0141] Among them, R 7 and R 8 Independently selected from C1 to C 12 Alkyl or C6~C 12 Preferably, A is -CH2-, -CH2CH2-, or A is -CH2- or -CH2CH2- with a substituent.
[0142] In the main catalyst of the present invention, L, R 6 , R 7 , R 8 , X 1 , X 2 , β are as described above; more preferably R 7 , R 8 C1~C 12 Alkyl or C6~C 12 aryl, such as methyl, isopropyl, tert-butyl, cycloalkyl or phenyl, preferably A is -CH2-, -CH2CH2-, or A is a substituted group; when L2 is NR 7 R 8 or PR 7 R 8 When the main catalyst is used, the structural formula is Formula (VI) or Formula (VII).
[0143] As a preferred embodiment, the structural formula of the main catalyst is formula (VIII) or formula (IX):
[0144]
[0145] In the main catalyst of the present invention, L 2 and B can be connected by an unsaturated bond, and the bond α at the dotted line can represent a double bond or a bond on an aromatic ring; when L 2 Connected to B through an unsaturated bond, L 2 Selected from NR 7 or PR 7 , more preferably NR 7 , R 7 Consistent with the above; when α represents an unsaturated bond, the compound may contain an imine ligand, such as -B=NR 8, or contains a pyridine ring, N and B are contained in a pyridine ring, and the structural formula of the catalyst is formula (VIII) or formula (IX).
[0146] In the present invention, R 1 , R 2 , R 3 , R 4 The optional organic group refers to a substituent group containing C atoms, such as alkyl, alkenyl, alkynyl, ester, alkoxy, alkenyloxy, cycloalkyl, aryl, heterocyclic, heteroaryl, alkylamino, etc. In the present invention, R 1 , R 2 , R 3 , R 4 The optional inorganic group refers to a substituent group that does not contain a C atom, such as a hydroxyl group, a nitro group, a halogen group, a sulfonic acid group, an amino group, a cyano group, etc.; R 1 , R 2 , R 3 , R 4 independently selected from hydrogen, halogen, nitro, CF3, C1-C 30 Alkyl, C3~C 30 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C2~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1-C2 alkylthio, C6-C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 of an alkylsulfinyl group.
[0147] In the present invention, R 1 , R 2 , R 3 , R 4 can be the same or different and are each selected from hydrogen or an organic group or an inorganic group; preferably, R 1 , R 2 , R 3 , R 4 Each is independently selected from hydrogen, halogen, nitro, CF3, alkyl, cycloalkyl, alkenyl, alkynyl, aryl, alkoxy, alkenyloxy, alkynyloxy, aryloxy, alkoxycarbonyl, alkylamino, alkylthio, arylthioether, alkylsulfonyl or alkylsulfinyl.
[0148] More preferably, R1 , R 2 , R 3 , R 4 independently selected from hydrogen, fluorine, chlorine, bromine, nitro, straight or branched C1-C 30 Alkyl, C6~C 24 Cycloalkanes, straight or branched C1~C 20 Alkoxy or C6~C 24 wherein the C1~C 30 Alkyl and C1~C 20 The alkoxy radicals may be substituted by one or more double or triple bonds or by one or more heteroatoms, preferably oxygen or nitrogen.
[0149] In addition, R 1 , R 2 , R 3 , R 4 Two or more of them may also be connected through an aliphatic or aromatic structure; for example, R 3 , R 4 And by connecting their carbon atoms on the phenyl ring in the expression (VIII), a fused phenyl ring can be formed, and overall, a naphthyl structure is produced.
[0150] In the present invention, the above R 1 , R 2 , R 3 , R 4 It may be optionally substituted by one or more alkyl, alkoxy, halogen, aryl or heteroaryl groups or heteroaryl groups; more preferably, it may be substituted by one or more C1-C 30 Alkyl, C1~C 20 Alkoxy, halogen, C6~C 24 Aryl or C6~C 24 The heteroaryl group is optionally substituted.
[0151] In the present invention, R 6 Preferably, it is hydrogen, alkyl, alkenyl, alkynyl or aryl; More preferably, it is hydrogen, C1-C 30 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl or C6~C 24 Preferably, R 6 For hydrogen.
[0152] As a preferred embodiment, the structural formula of the main catalyst is at least one of the following structures:
[0153]
[0154] As another preferred embodiment, the structural formula of the main catalyst is at least one of the following structures:
[0155]
[0156] As another preferred embodiment, the structural formula of the main catalyst is at least one of the following structures:
[0157]
[0158] The present invention does not limit the source of the metal compound based on Group VIII of the above formula (I), formula (II) or formula (II) structure, which can be commercially available or prepared by methods disclosed in the prior art, such as US2002 / 0107138, US2008 / 0064882, US2009 / 0076226, J.Am.Chem.Soc, 2000, 122, 8168-8179, and CN111905821.
[0159] The main catalyst of the present invention is preferably selected from one or more of Grubbs II-III, Hoveda-Grubbs II catalyst, and Grela catalyst, and the structural formula is as follows:
[0160]
[0161] In the present invention, the main catalyst (a) may be water-soluble or water-insoluble. In the present invention, "water-insoluble" means that at 24±2°C, 0.001 or less weight content of the substance can be completely dissolved in 100 equivalents of water. At 24±2°C, if more than 0.5 weight content of the catalyst can be completely dissolved in 100 equivalents of water, the catalyst is considered to be "water-soluble".
[0162] In the present invention, the first co-catalyst (b) is preferably one or more of aliphatic monocarboxylic acid alkyl esters, aromatic monocarboxylic acid alkyl esters, aliphatic polycarboxylic acid alkyl esters, aromatic polycarboxylic acid alkyl esters, polyol alkyl esters, polyol cycloalkyl esters, polyol aryl esters, polyol alkylaryl esters, aliphatic ethers, cycloaliphatic ethers, aliphatic diethers, aliphatic ketones, aliphatic amines, aliphatic diamines, olefins and alkynes.
[0163] More preferably, the first co-catalyst (b) is C1 to C 20 Alkyl esters of saturated fatty carboxylic acids, C7~C 24 Alkyl esters of aromatic carboxylic acids, C2~C 20 Aryl esters of diols, C2~C 20 Fatty ethers, C3~C 20 Cyclic ethers, C5~C 20Aliphatic diethers, C3~C 20 Saturated fatty ketones, C3~C 20 Saturated fatty amines, C3~C 20 Saturated fatty diamines, C3~C 20 Fatty amides, C7~C 24 Aromatic amides, C2~C 20 Olefins and C2~C 20 One or more of the alkynes.
[0164] Most preferably, the first co-catalyst (b) is one or more of methyl formate, ethyl acetate, butyl acetate, diisobutyl phthalate, di-n-butyl phthalate, diisooctyl phthalate, ethyl ether, hexyl ether, tetrahydrofuran, dioxane, acetone, butanone, methyl isobutyl ketone, cyclohexanone, N-methylpyrrolidone and N,N-dimethylformamide.
[0165] In the present invention, the second co-catalyst is preferably one or more of non-emulsifier type carboxylates, emulsifier type carboxylates, non-emulsifier type sulfonates, emulsifier type sulfonates, non-emulsifier type phosphate salts and emulsifier type phosphate salts.
[0166] In the present invention, "non-emulsifier carboxylate" refers to an organic small molecule carboxylate containing a carboxylate group which does not have an emulsifying effect, wherein "salt" can be hydrogen, alkali metal cation, ammonium, alkanolamine or other cations.
[0167] Preferably, the non-emulsified formulation carboxylate can be one or more of formates, acetates, propionates, butyrates, valerates, oxalates, malonates, succinates, glutarates, triacrylic acid salts, trisuccinates, triglutarates, maleates, tartrates, fumarates, malates, amino acid salts, cyclopentaneates, alginates, gluconates, crotonates, itaconates, citrates, mesaconic acids, aromatic carboxylates, heteroaromatic carboxylates, imidazole (line) carboxylates, pyruvates, epoxysuccinates, salicylates, fluorenedioates, hydroxypropionates, levulinates, furandicarboxylates, acrylates, methacrylates and trifluoroformates.
[0168] In the present invention, "emulsifier-type carboxylate" is a surfactant containing a carboxylate group with emulsifying effect, which can be one or more of long-chain alkyl carboxylates of C8 or above, resinates, modified resinates, alkanoyl amino acid salts, fatty acid polypeptide condensates and acyl lactylates.
[0169] In the present invention, the "long-chain alkyl carboxylate of C8 or more" is generally represented by the formula RCOOM (1 / n) , wherein R is hydrogen, C8~C 30 Alkyl, C8~C 20Cycloalkyl, C8~C 20 Alkenyl, C8~C 20 Alkynyl, C8~C 24 Aryl, C8~C 20 Alkoxy, C8~C 20 Alkenyloxy, C8~C 20 Alkynyloxy, C8~C 24 Aryloxy, C8~C 20 Alkoxycarbonyl, C8~C 20 Alkylamino, C8~C 20 Alkylthio, C8~C 24 Arylthio, C8~C 20 Alkylsulfonyl or C8~C 20 The alkylsulfinyl groups may be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0170] In the present invention, "resin acid salt" and "modified resin acid salt" are classified into (1) vinyl resin acid salt, (2) aliphatic resin acid salt, and (3) aromatic resin acid salt according to the chemical structure, and some typical examples are (disproportionated) pimaric acid salt, (disproportionated) neorosin acid salt, (disproportionated) rosin acid salt, (disproportionated) levosin acid salt and (disproportionated) pascal acid salt; "salt" can be hydrogen, alkali metal cation, ammonium, alkanolamine or other cations.
[0171] In the present invention, "alkanoyl amino acid salt" is mainly the condensation product of fatty acid and amino acid, such as alkanoyl amino acid salt, the typical types and general formula of which are as follows:
[0172] Alkanoyl aspartate: RCONHCH(CH2COO M (1 / n) )COO M (1 / n) ;
[0173] Alkanoyl-N-β-hydroxyethyl-glycinate: RCON(CH2 CH2OH ) )CH2COO M (1 / n) ;
[0174] N-Acylsarcosinate (Medialan): RCON(CH3)CH2COO M (1 / n) ;
[0175] N-Alkanoyl Peptide (Lamepon): RCONHR`(CONHR``)COO M (1 / n) ;
[0176] Wherein, R is hydrogen, C1~C30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0177] In the present invention, "fatty acid polypeptide condensate" is obtained by condensing fatty acid chloride with amino acids of protein hydrolysate, and its general formula is RCONH(polypeptide)COOM (1 / n) ; Wherein, R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl group may be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, alkali metal cation, ammonium, alkanolamine or other cation; n is the valence of the ion; the polypeptide chain length ranges from a molecular weight of 150 to 10,000, preferably, a polypeptide with a molecular weight of 350 to 2,000.
[0178] In the present invention, "acyl lactylate" is a salt obtained by esterification and polymerization of fatty acid (RCOOH) and lactic acid (H3CCH(OH)COOH) and neutralization, having the general formula RCO(OCH(CH3)CO) m OM (1 / n) ; Wherein, R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0179] In the present invention, "non-emulsifier type sulfonate" refers to an organic small molecule sulfonate containing a sulfonate group which does not have an emulsifying effect, wherein "salt" can be hydrogen, an alkali metal cation, ammonium, an alkanolamine or other cations.
[0180] Preferably, the non-emulsifier type sulfonic acid salt can be methanesulfonate, trifluoromethylsulfonate, ethanesulfonate, perfluoroethanesulfonate, propanesulfonate, perfluoropropanesulfonate, hydroxypropanesulfonate, butylsulfonate, perfluorobutylsulfonate, hydroxybutylsulfonate, toluenesulfonate, dinitrotoluenesulfonate, styrenesulfonate, vinylsulfonate, allylsulfonate, methylallylsulfonate, perfluorosulfonic acid polymer, aromatic sulfonate, heteroaromatic ring sulfonate, cycloalkanesulfonate, hydroxybenzoate, One or more of sulfonates, 2-(2-aminoethyl)aminoethanesulfonates, N,N-di(2-hydroxyethyl)-2-aminoethanesulfonates, N-tris(hydroxymethyl)methyl-2-aminoethanesulfonates, aminosulfonates, aminoaromaticsulfonates, ethylenediamineethanesulfonates, chrysinsulfonates, anthraquinonesulfonates, diaminoformylsulfonates, quinocinonesulfonates, thiazolesulfonates, imidazolinesulfonates, allylimidazolinesulfonates, triazolonesulfonates, triazinesulfonates and flavonesulfonates.
[0181] In the present invention, "emulsifier-type sulfonate" is a surfactant containing a sulfonate group with an emulsifying effect, which can be one or more of long-chain alkyl sulfonates of C8 or above, alkyl aryl sulfonates, alkyl diphenyl ether disulfonates, α-hydroxy sulfonates and α-olefin sulfonates, petroleum sulfonates, α-sulfonic monocarboxylic acids and derivatives thereof, sulfonalkyl ester derivatives of fatty acids and sulfonalkyl amide derivatives of fatty acids, succinate ester sulfonates, lignin sulfonates, alkyl glyceryl ether sulfonates, 2-aminoethanesulfonates and derivatives thereof.
[0182] In the present invention, "C8 or more long chain alkyl sulfonate" and "alkyl aryl sulfonate" have the general formula RSO3M (1 / n) , where R is C8~C 30 Alkyl, C8~C 20 Cycloalkyl, C8~C 20 Alkenyl, C8~C 20 Alkynyl, C6~C 24 Aryl, C8~C 20 Alkoxy, C8~C 20 Alkenyloxy, C8~C 20 Alkynyloxy, C6~C 24 Aryloxy, C8~C 20 Alkoxycarbonyl, C8~C 20 Alkylamino, C8~C 20 Alkylthio, C6~C 24 Arylthio, C8~C 20 Alkylsulfonyl or C8~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0183] In the present invention, "alkyl diphenyl oxide disulfonate" has the following general formula:
[0184]
[0185] Wherein, R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0186] In the present invention, "α-hydroxysulfonate" has the following general formula:
[0187]
[0188] In the present invention, "α-olefin sulfonate" has the following general formula:
[0189]
[0190] In the above-mentioned general structure of "α-hydroxysulfonate" and "α-olefinsulfonate", R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; n is the valence of the ion; m and p are 0 or positive integers.
[0191] In the present invention, "petroleum sulfonate" is a mixture, the main component of which is complex alkylbenzene sulfonate or alkylnaphthalene sulfonate, and the rest is sulfonates and oxides of aliphatic hydrocarbons and cyclic hydrocarbons; the "salt" therein can be hydrogen, alkali metal cations, ammonium, alkanolamine or other cations.
[0192] In the present invention, "α-sulfonic monocarboxylic acid and its derivatives" refer to various products obtained by replacing the α-position H of fatty acids or esters with sulfonic groups, mainly including the following types: (1) α-sulfonic fatty acid methyl ester mono (sodium) salt, which is a product obtained by sulfonation and neutralization of fatty acid methyl ester as raw material, referred to as MES (methyl ester sulfonate), with the general formula of RCH (SO3M (1 / n) )COOCH3, wherein R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 Alkylsulfinyl, these substituents can be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M can be hydrogen, alkali metal cation, ammonium, alkanolamine or other cations; n is the valence of the ion. (2) α-sulfo-low carbon fatty acid high carbon alcohol esters, such compounds mainly include: ① sulfoacetic acid lauryl ester C 12 H 25 OOCCH2SO3Na, ② Esters formed by sulfoacetic acid and branched alcohols, long-chain alcohols or alcohol ethers.
[0193] In the present invention, the trade name of "sulfonalkyl ester salt derivative of fatty acid" is Igepon A, and its representative substance is sodium oleoyloxyethanesulfonate.
[0194] In the present invention, the trade name of "sulfonylamide salt derivative of fatty acid" is Igepon T, and the general formula is R 1 -CO-N(R 2 )-R 3 -SO3M (1 / n) , its representative is sodium N-oleoyl-N-methyl taurine; wherein, R 1 , R 2 , R 3 are the same or different and are each selected from hydrogen, C1 to C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0195] In the present invention, "succinate ester sulfonate" can be divided into succinic acid monoester sulfonate according to its structure, with the general formula ROOCCH2CH(SO3M (1 / n) COOM (1 / n) ), and succinic acid diester sulfonate, general formula ROOCCH2CH(SO3M (1 / n) COOR). According to the different hydroxyl-containing raw materials used in the esterification reaction, it can be divided into sulfosuccinic acid alkyl ester salt, sulfosuccinic acid fatty alcohol polyoxyethylene ether ester salt, sulfosuccinic acid fatty amide ethyl ester salt, etc. Among them, the typical one is sulfosuccinic acid fatty alcohol polyoxyethylene ether ester disodium salt, which has the general formula RO (CH2CH2O) m OCCH2CH(SO3Na)COONa, ethyl sulfosuccinamide disodium salt, has the general formula RCONH(CH2CH2O) m CH2CH2OOCCH2CH(SO3Na)COONa, disodium sulfosuccinate ethoxylated alkanolamide ester, RCONHCH2CH2OOCCH2CH(SO3Na)COONa, sulfosuccinate siloxane ester salt. Wherein, R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be selectively substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; n is the valence of the ion; and m is 0 or a positive integer.
[0196] In the present invention, "lignin sulfonate" is the main component of the wastewater from the sulfite pulping process of logs in the papermaking industry, and the general formula is as follows:
[0197]
[0198] Lignin sulfonate is a mixture with a rather complex structure. It is generally believed to be a sulfonate of a polymer of guaiacylpropyl, syringylpropyl and p-hydroxyphenylpropyl. It can contain up to 8 sulfonic acid groups and 16 methoxy groups. The sulfonated carbon atom is at the α-position connected to the phenyl group. The molecular weight distribution range of lignin sulfonate is very wide, with a relative molecular mass ranging from 200 to 10,000. The most common lignin sulfonate has an average relative molecular mass of about 4,000.
[0199] In the present invention, "alkyl glyceryl ether sulfonate" has the general formula ROCH2CH(OH)CH2SO3M (1 / n) , wherein R is hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, an alkanolamine, or another cation; and n is the valence of the ion.
[0200] In the present invention, "2-aminoethanesulfonate and its derivatives" are also called taurate and its derivatives, such as methyl taurate CH3NHCH2CH2SO3M (1 / n) Derivatives, N-acyl-N-alkyl taurates RCON(R`)CH2CH2SO3M (1 / n) Wherein, R and R' may be the same or different, each selected from hydrogen, C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation; and n is the valence of the ion.
[0201] In the present invention, "non-emulsifier type phosphate salt" refers to an organic small molecule phosphate salt containing a phosphate group that does not have an emulsifying effect, wherein the "salt" can be hydrogen, an alkali metal cation, ammonium, an alkanolamine or other cations.
[0202] Preferably, the non-emulsifier type phosphate salt can be monomethyl phosphate, monoethyl phosphate, monobutyl phosphate, dimethyl phosphate, diethyl phosphate, dibutyl phosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, monophenyl phosphate, diphenyl phosphate, triphenyl phosphate, mono-p-tolyl phosphate, di-p-tolyl phosphate, tri-p-tolyl phosphate, mono-o-tolyl phosphate, di-o-tolyl phosphate, tri-o-tolyl phosphate, mono-m-tolyl phosphate, di-m-tolyl phosphate, tri-m-tolyl phosphate, mono-p-isopropylphenyl phosphate, di-p-isopropylphenyl phosphate, tri-p-isopropylphenyl phosphate, phosphoric acid Mono-p-tert-butylphenyl ester salt, di-p-tert-butylphenyl phosphate salt, tri-p-tert-butylphenyl phosphate, mono-p-methoxyphenyl phosphate salt, di-p-methoxyphenyl phosphate salt, tri-p-methoxyphenyl phosphate, phenyl dimethyl phosphate, phenyl diethyl phosphate, phenyl dibutyl phosphate, diphenyl methyl phosphate, diphenyl ethyl phosphate, diphenyl butyl phosphate, p-tolyl dimethyl phosphate, p-tolyl diethyl phosphate, p-tolyl dibutyl phosphate, o-tolyl dimethyl phosphate, o-tolyl diethyl phosphate, o-tolyl dibutyl phosphate, m-tolyl dimethyl phosphate, m-tolyl diethyl phosphate, m-tolyl dibutyl phosphate, di-p-tolyl phosphate Phenyl methyl ester, di-p-tolyl ethyl phosphate, di-p-tolyl butyl phosphate, di-o-tolyl methyl phosphate, di-o-tolyl ethyl phosphate, di-o-tolyl butyl phosphate, di-m-tolyl methyl phosphate, di-m-tolyl ethyl phosphate, di-m-tolyl butyl phosphate, di-p-isopropylphenyl methyl phosphate, di-p-isopropylphenyl ethyl phosphate, di-p-isopropylphenyl butyl phosphate, di-p-isopropylphenyl dimethyl phosphate, di-p-isopropylphenyl diethyl phosphate, di-p-isopropylphenyl dibutyl phosphate, di-p-isopropylphenyl dimethyl phosphate, di-p-isopropylphenyl diethyl phosphate, di-p-isopropylphenyl dibutyl phosphate, di-p-isopropylphenyl methyl phosphate, di-p-isopropylphenyl ethyl phosphate, One or more of di-p-tert-butylphenyl butyl phosphate, phenyl di-p-tolyl phosphate, phenyl di-p-isopropylphenyl phosphate, phenyl di-p-tert-butylphenyl phosphate, p-tolyl diphenyl phosphate, p-tolyl p-diisopropylphenyl phosphate, p-tolyl p-di-tert-butylphenyl phosphate, o-tolyl p-diisopropylphenyl phosphate, o-tolyl p-di-tert-butylphenyl phosphate, m-tolyl p-diisopropylphenyl phosphate, m-tolyl p-di-tert-butylphenyl phosphate, p-isopropylbenzene di-p-tolyl phosphate, p-isopropylbenzene di-o-tolyl phosphate, p-isopropylbenzene di-m-tolyl phosphate, p-isopropylbenzene di-p-phenyl phosphate and p-isopropylbenzene di-p-tert-butylphenyl phosphate.
[0203] In the present invention, the "emulsifier type phosphate salt" is a surfactant containing a phosphate group with an emulsifying effect, which can be one or more of a long-chain alkyl phosphate monoester or diester salt of C8 or above, a fatty alcohol polyvinyl ether phosphate monoester or disalter, an alkylphenol polyoxyethylene ether phosphate monoester or disalter, and a phosphate ester salt of an alcohol ether or a phenol ether. Particularly preferred is a phosphate ester salt selected from the following chemical formula:
[0204]
[0205] Among them, R is usually C1~C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 The alkylsulfinyl groups may be optionally substituted by one or more alkyl, halogen, alkoxy, aryl or heteroaryl groups; M may be hydrogen, an alkali metal cation, ammonium, an alkanolamine or another cation.
[0206] In the present invention, the molar ratio of the main catalyst (a), the first co-catalyst (b) and the second co-catalyst (d) in the catalyst composition is preferably 1:(20-100):(100-10000).
[0207] In the present invention, the catalyst composition is preferably present in liquid form. In order to achieve the presence in liquid form, the catalyst composition may also include a solvent, and the solvent can be appropriately selected according to the type of the catalyst composition, based on the ability to dissolve the catalyst composition. Generally, the solvent can be an organic solvent and / or water, preferably an aromatic hydrocarbon solvent and / or water, particularly preferably one or more of toluene, xylene, chlorobenzene and water. The amount of the solvent can be a conventional choice in the art, and will not be described in detail herein.
[0208] The present invention also provides a method for selective hydrogenation of conjugated diene latex, comprising the following steps:
[0209] In the presence of the catalyst composition described in the above technical solution, the conjugated diene latex is selectively hydrogenated to obtain hydrogenated conjugated diene latex.
[0210] In the present invention, the amount of the main catalyst (a) is preferably 0.001 to 5 wt %, more preferably 0.001 to 2 wt %, and most preferably 0.01 to 0.1 wt % based on the mass of the conjugated diene latex.
[0211] In the present invention, the amount of the first cocatalyst (b) is preferably 0.01 to 5 wt %, more preferably 0.01 to 2 wt %, and most preferably 0.05 to 1 wt % based on the mass of the conjugated diene latex.
[0212] In the present invention, the amount of the second cocatalyst (c) is preferably 0-10 wt %, more preferably 0.1-10 wt %, and most preferably 0.5-2 wt % based on the mass of the conjugated diene latex.
[0213] In the present invention, suitable substrates for hydrogenation are in principle all aqueous suspensions based on conjugated diene polymers, which are also referred to as "latexes". Such polymers based on conjugated dienes contain carbon-carbon double bonds. These latexes include suspensions prepared by free radical polymerization of aqueous monomer latexes (primary suspensions) and those suspensions whose polymers have been prepared by any method or route and then converted into aqueous suspension form (secondary suspensions). The term "aqueous suspension" also includes, in principle, suspensions of microcapsules.
[0214] In the present invention, the polymer having carbon-carbon double bonds that can withstand the method of the present invention comprises repeating units based on at least one conjugated diene monomer. The conjugated diene monomer comprises at least one conjugated monomer (a); the conjugated diene monomer (a) is preferably selected from C4 to C6 conjugated dienes, more preferably selected from one or more of 1,3-butadiene, isoprene, 1-methylbutadiene, 2,3-dimethylbutadiene, piperylene and chloroprene, particularly preferably 1,3-butadiene and / or isoprene, and extremely preferably 1,3-butadiene.
[0215] In a further embodiment, a polymer having carbon-carbon double bonds can be subjected to the process of the invention, which comprises not only at least one conjugated diene as monomer (a), but also repeating units of at least one other copolymerizable monomer (b). Examples of suitable monomers (b) are olefins, such as ethylene or propylene. Further examples of suitable monomers (b) are vinyl aromatic monomers, such as styrene, α-methylstyrene, o-chlorostyrene or vinyltoluene, aliphatic or branched C1-C 18 Vinyl esters of monocarboxylic acids, such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl caproate, vinyl 2-ethylhexanoate, vinyl caprate, vinyl laurate or vinyl stearate.
[0216] A preferred polymer to be used in the present invention is a copolymer of 1,3-butadiene and styrene, or a copolymer of 1,3-butadiene and α-methylstyrene, which copolymer may have a random or block type structure.
[0217] Further suitable copolymers have repeating units derived from at least one conjugated diene and from at least one monomer (b) selected from the group consisting of an ethylenically unsaturated mono- or dicarboxylic acid, such as acrylic acid, methacrylic acid, maleic acid, fumaric acid or itaconic acid, and a typically C1-C 12 Alkanols, such as methanol, ethanol, n-propanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, n-hexanol, 2-ethylhexanol or C5~C 10 Esters of cycloalkanols, such as cyclopentanol or cyclohexanol, and preferably esters of acrylic acid and / or methacrylic acid; examples are methyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, n-butyl acrylate, tert-butyl acrylate or 2-ethylhexyl acrylate.
[0218] Suitable other copolymerizable monomers (b) are α,β-unsaturated nitriles. It is possible to use any known α,β-unsaturated nitriles, preferably C3-C5 α,β-unsaturated nitriles, such as acrylonitrile, methacrylonitrile, ethacrylonitrile or mixtures thereof, with acrylonitrile being particularly preferred.
[0219] Suitable copolymers to be used in the present invention are so-called nitrile rubbers (also referred to as "NBR"), which are copolymers having repeating units of at least one conjugated diene, preferably 1,3-butadiene, at least one α,β-unsaturated nitrile, preferably acrylonitrile, and optionally one or more other copolymerizable monomers.
[0220] Thus, a particularly preferred nitrile rubber is a copolymer having repeating units derived from acrylonitrile and 1,3-butadiene.
[0221] In addition to the conjugated diene and the α,β-unsaturated nitrile, the nitrile rubber may include repeating units of one or more other copolymerizable monomers known in the art, for example, α,β-unsaturated (preferably monounsaturated) monocarboxylic acids, their esters or amides, α,β-unsaturated (preferably monounsaturated) dicarboxylic acids, their monoesters or diesters, and the corresponding anhydrides or amides of the α,β-unsaturated dicarboxylic acids.
[0222] As α,β-unsaturated monocarboxylic acids, acrylic acid and / or methacrylic acid are preferred third monomers for such nitrile rubbers.
[0223] Esters of α,β-unsaturated monocarboxylic acids may also be used, specifically alkyl esters, alkoxyalkyl esters, aryl esters, cycloalkyl esters, cyanoalkyl esters, hydroxyalkyl esters or fluoroalkyl esters.
[0224] As alkyl esters, C 1~ C 18 Alkyl esters of C l~C 18 alkyl esters such as methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, n-dodecyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate or 2-ethylhexyl methacrylate.
[0225] As alkoxyalkyl esters of α,β-unsaturated monocarboxylic acids, C2-C 18 Alkoxyalkyl esters are preferably used, more preferably alkoxyalkyl esters of acrylic acid or methacrylic acid, such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate or methoxyethyl (meth)acrylate.
[0226] It is also possible to use aromatic esters, preferably C6-C 14 Aryl esters, more preferably C6~C 10 The aryl esters are preferably aryl esters of acrylates and / or methacrylates.
[0227] In another embodiment, the cycloalkyl ester, preferably C5-C 12 Cycloalkyl esters, more preferably C6~C 12 The cycloalkyl esters of the present invention are preferably cycloalkyl acrylates and / or methacrylates as described above.
[0228] It is also possible to use cyanoalkyl esters, in particular cyanoalkyl acrylates or cyanoalkyl methacrylates, wherein the number of C atoms in the cyanoalkyl group is in the range from 2 to 12, preferably α-cyanoethyl acrylate, β-cyanoethyl acrylate or cyanobutyl methacrylate is used.
[0229] In another embodiment, hydrocarbon alkyl esters are used, in particular hydrocarbon alkyl acrylates and hydroxyalkyl methacrylates, wherein the number of C atoms in the hydroxyalkyl group is in the range of 1 to 12, preferably 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate or 3-hydroxypropyl acrylate.
[0230] It is also possible to use fluorobenzyl esters, in particular fluorobenzyl acrylate or fluorobenzyl methacrylate, preferably trifluoroethyl acrylate and / or tetrafluoropropyl methacrylate. Acrylates and / or methacrylates containing substituted amino groups can also be used, like dimethylaminomethacrylate and / or diethylaminoethylacrylate.
[0231] Various other esters of α,β-unsaturated carboxylic acids can also be used, such as, for example, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, glycidyl (meth)acrylate, epoxy (meth)acrylate, N-(2-hydroxyethyl)acrylamide, N-(2-hydroxymethyl)acrylamide or polyurethane (meth)acrylate.
[0232] It is also possible to use mixtures of all the abovementioned esters of α,β-unsaturated carboxylic acids.
[0233] Further α,β-unsaturated dicarboxylic acids can be used, preferably maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid or mesaconic acid (methylfumaric acid).
[0234] In another embodiment, anhydrides of α,β-unsaturated dicarboxylic acids are used, preferably maleic anhydride, itaconic anhydride, citraconic anhydride or mesaconic anhydride.
[0235] In a further embodiment, monoesters or diesters of α,β-unsaturated dicarboxylic acids may be used. Suitable alkyl esters are, for example, C1-C 10 Suitable alkoxyalkyl esters are, for example, C2-C l2 Alkoxyalkyl esters, preferably C3 to C8 alkoxyalkyl monoesters or diesters. Suitable hydroxyalkyl esters are, for example, C l ~C 12 A hydroxyalkyl ester of C2 to C8, preferably a hydroxyalkyl monoester or diester. Suitable cycloalkyl esters are, for example, C5 to C l0 Cycloalkyl esters, preferably C6 to C 10 Suitable alkylcycloalkyl esters are, for example, C6 to C l0 Alkylcycloalkyl esters, preferably C7-C 10 -alkylcycloalkyl monoester or diester. Suitable aryl esters are, for example, C6-C l4 Aryl ester, preferably C6~C 10 Aromatic monoesters or diesters.
[0236] Specific examples of α,β-ethylenically unsaturated dicarboxylic acid monoester monomers include:
[0237] "monoalkyl maleate", preferably monomethyl maleate, monoethyl maleate, monopropyl maleate or mono-n-butyl maleate;
[0238] "Monocyclic maleic acid alkyl ester", preferably monocyclic maleic acid pentyl ester, monocyclic maleic acid hexyl ester or monocyclic maleic acid heptyl ester;
[0239] "monoalkylcycloalkyl maleate", preferably monomethylcyclopentyl maleate or monoethylcyclohexyl maleate;
[0240] "Maleic acid monoaryl ester", preferably monophenyl maleate;
[0241] "Monobenzyl maleate", preferably monobenzyl maleate;
[0242] "monoalkyl fumarate", preferably monomethyl fumarate, monoethyl fumarate, monopropyl fumarate or mono-n-butyl fumarate;
[0243] "monocycloalkyl fumarate", preferably monocyclopentyl fumarate, monocyclohexyl fumarate or monocycloheptyl fumarate;
[0244] "monoalkylcycloalkyl fumarate", preferably monomethylcyclopentyl fumarate or monoethylcyclohexyl fumarate;
[0245] "Monoaryl fumarate", preferably monophenyl fumarate;
[0246] "Monobenzyl fumarate", preferably monobenzyl fumarate;
[0247] "Monoalkyl citrate", preferably monomethyl citrate, monoethyl citrate, monopropyl citrate or mono-n-butyl citrate;
[0248] "Citraconate monocycloalkyl ester", preferably citraconate monocyclopentyl ester, citraconate monocyclohexyl ester or citraconate monocycloheptyl ester;
[0249] "Monoalkylcycloalkyl citrate", preferably monomethylcyclopentyl citrate or monoethylcyclohexyl citrate;
[0250] "Citraconic acid monoaryl ester", preferably citraconic acid monophenyl ester;
[0251] "Monobenzyl citrate", preferably monobenzyl citrate;
[0252] "Monoalkyl itaconate", preferably monomethyl itaconate, monoethyl itaconate, monopropyl itaconate or mono-n-butyl itaconate;
[0253] "Itaconate monocycloalkyl ester", preferably itaconate monocyclopentyl ester;
[0254] "Monoalkylcycloalkyl itaconate", preferably monomethylcyclopentyl itaconate or monoethylcyclohexyl itaconate;
[0255] "Itaconate monoaryl ester", preferably itaconate monophenyl ester;
[0256] "Monobenzyl itaconate", preferably monobenzyl itaconate.
[0257] As α,β-ethylenically unsaturated dicarboxylic acid diester monomers, analogous diesters based on the monoester monomers mentioned explicitly above can be used, wherein, however, the two organic groups linked to the C═O group via the oxygen atom can be identical or different.
[0258] As further third monomers, vinyl aromatic monomers, like styrene, α-methylstyrene or vinylpyridine, and non-conjugated dienes, like 4-cyanocyclohexene and 4-vinylcyclohexene, and alkynes, like 1- or 2-butyne, can be used.
[0259] As an additional third monomer, a PEG acrylate monomer derived from a PEG acrylate of the general formula (X) may be used:
[0260]
[0261] Wherein, R is hydrogen or a straight or branched C1~C 20 alkyl, preferably methyl, ethyl, butyl or ethylhexyl, n is 1 to 8, preferably 2 to 8, more preferably 2 to 5 and most preferably 3, and R 1 It is hydrogen or CH3-.
[0262] In the context of the present invention, the term "(meth)acrylate" means "acrylate" and "methacrylate". 1 When the group is CH3-, the molecule is a methacrylate. The term "polyethylene glycol" or abbreviation "PEG" refers to both monoethylene glycol segments having one repeating ethylene glycol unit (PEG-1, n=1) and polyethylene glycol segments having 2 to 8 repeating ethylene glycol units (PEG-2 to PEG-8; n=2 to 8). The term 'PEG acrylate' is also abbreviated as PEG-X-(M)A, where "X" represents the number of repeating ethylene glycol units, "MA" represents methacrylate and "A" represents acrylate. Acrylate monomers derived from PEG acrylate of the general formula (X) are referred to as "PEG acrylate monomers.
[0263] Preferred PEG acrylate monomers are selected from the following formulas No. 1 to No. 10, wherein n is 1, 2, 3, 4, 5, 6, 7 or 8, preferably 2, 3, 4, 5, 6, 7 or 8, more preferably 3, 4, 5, 6, 7 or 8 and most preferably 3:
[0264]
[0265]
[0266] Other common names for methoxypolyethylene glycol acrylate (Formula No. 3) are, for example, poly(ethylene glycol) methyl ether acrylate, acryloyl-PEG, methoxy-PEG acrylate, methoxypoly(ethylene glycol) monoacrylate, poly(ethylene glycol) monomethyl ether monoacrylate or mPEG acrylate.
[0267] Particularly preferred is a third monomer selected from the following chemical formula:
[0268]
[0269] Among them, R 1 is hydrogen or a methyl group, and R 2 , R 3 , R 4 , R 5 are the same or different and can represent H, C1~C 12 Alkyl, cycloalkyl, alkoxyalkyl, hydroxyalkyl, oxirane, aryl or heteroaryl.
[0270] As the PEG acrylate termonomer, particularly preferred are methoxy-PEG-1-acrylate (MEA), butyl diglycol methacrylate, (butoxy-PEG-2-MA, BDGMA) or ethyl diglycol methacrylate (ethoxy-PEG-3-MA).
[0271] In the present invention, in the case where the polymer to be subjected to the process of the present invention comprises not only repeating units of one or more conjugated dienes but also repeating units of one or more other copolymerizable monomers, the ratio of the conjugated dienes and the other copolymerizable monomers may vary within a wide range, specifically:
[0272] In the case of NBR polymers used in the process of the invention, the proportion or sum of the proportions of conjugated dienes is generally in the range of 40% to 90% by weight, preferably in the range of 50% to 85% by weight, based on the total polymer. The proportion or sum of the proportions of α,β-unsaturated nitrile is generally in the range of 10% to 60% by weight, preferably in the range of 15% to 50% by weight, based on the total polymer. In each case, the proportions of the monomers add up to 100 by weight. Additional third monomers may optionally be present. If used, they are generally present in an amount of greater than 0% to 40% by weight, preferably 0.1% to 40% by weight, particularly preferably 1% to 30% by weight, based on the total polymer. In this case, the corresponding proportions of conjugated dienes and / or α,β-unsaturated nitrile are replaced by the proportions of the additional third monomers, wherein the proportions of all monomers add up to 100% by weight in each case.
[0273] The preparation of nitrile rubbers by polymerization of the abovementioned monomers is sufficiently known to the person skilled in the art and is comprehensively described in the polymer literature.
[0274] The nitrile rubber used according to the invention has a Mooney viscosity (ML 1+4 at 100° C.) in the range of 25 to 70, preferably in the range of 30 to 50. This corresponds to a weight average molecular weight M in the range of 100,000 to 500,000, preferably in the range of 200,000 to 400,000. w .
[0275] A nitrile rubber having a Mooney viscosity of about 34, for example, has an intrinsic viscosity of about 1.1 dL / g measured in chlorobenzene at 35° C. The nitrile rubber used also has a polydispersity PDI=M w / M n , where M w is the weight average molecular weight, and M n is the number average molecular weight, ranging from 2.0 to 10.0, and preferably ranging from 2.0 to 4.0. The Mooney viscosity is measured according to ASTM standard D 1646.
[0276] If a polymer is used in the present invention, which contains repeating units of one or more conjugated dienes and optionally one or more other copolymerizable monomers such as, for example, styrene or α-methylstyrene, the proportion of the conjugated diene is generally between 15% bw (by weight) and 100% bw, and the proportion or total proportion of the copolymerizable termonomers is between 0% bw and 85% bw. If, as other copolymerizable monomers, styrene or α-methylstyrene is used, the proportion of styrene and / or methylstyrene is preferably between 15% bw and 60% bw, with the remainder to 100% bw being represented by the conjugated diene.
[0277] The carbon-carbon double bond-containing polymer in latex form useful in the present invention can be prepared by any method known to those skilled in the art, such as latex polymerization, solution polymerization or bulk polymerization. Preferably, the carbon-carbon double bond-containing polymer useful in the present invention is prepared by an aqueous latex polymerization method because this method directly produces a polymer in latex form.
[0278] Preferably, according to the present invention, the polymer solid content in the aqueous latex lies in the range of 1 to 75% by weight, more preferably 5 to 50% by weight, based on the total weight of the aqueous latex.
[0279] The preparation of such polymers, which are subjected to the process according to the invention, is known to the person skilled in the art and can in principle be carried out by anionic, free radical or Ziegler-Natta polymerization in solution, in bulk, in suspension or in latex. Depending on the type of reaction, the conjugated dienes are 1,4- and / or 1,2-polymerized. For the hydrogenation process according to the invention, preference is given to using polymers which have been prepared by free radical aqueous latex polymerization of the above-mentioned monomers (a) and (b). These techniques are sufficiently known to the person skilled in the art and are described in detail in the literature, for example in Ullmann's Encyclopedia of Industrial Chemistry, 5 th In the preparation of such polymers, free radical initiators and, if desired, surface-active substances such as emulsifiers and protective colloids are usually used (see, for example, Houben Weyl, Methoden der organischen Chemie, Volumen XIV / 1, Makromolekulare Stoffe, Georg Thieme Verlag, Stuttgart, 1961, pp 192-208).
[0280] Suitable free-radical polymerization initiators include organic peroxides, such as tert-butyl hydroperoxide, benzoyl hydroperoxide or diisopropylbenzoyl peroxide, inorganic peroxides, such as hydrogen peroxide, salts of peroxomono and / or peroxodisulfuric acid, especially ammonium and / or alkali metal peroxodisulfates (persulfates), and azo compounds, particularly preferred are persulfates. Also preferred are combined systems consisting of at least one organic reducing agent and at least one peroxide and / or hydroperoxide, such as tert-butyl hydroperoxide and the sodium salt of hydroxymethanesulfonic acid, or hydrogen peroxide and ascorbic acid (as an electrolyte-free redox initiator system), in combination with systems which additionally comprise small amounts of metal compounds which are soluble in the polymerization medium and whose metal components can be present in a plurality of valence states, such as ascorbic acid / iron(II) sulfate / hydrogen peroxide, it being possible to frequently replace ascorbic acid with hydroxymethanesulfinic acid, sodium sulfite, sodium hydrogensulfate or sodium hydrogensulfite, and to replace hydrogen peroxide with tert-butyl hydroperoxide, alkali metal peroxodisulfates and / or ammonium peroxodisulfate. Instead of water-soluble iron(II) salts, it is also possible to employ combinations of water-soluble Fe / V salts.
[0281] These polymerization initiators are employed in customary amounts, for example in amounts of 0.01% bw to 5% bw, preferably 0.1% bw to 2.0% bw, based on the monomers to be polymerized.
[0282] The monomer mixture can, if desired, be polymerized in the presence of customary regulators such as mercaptans, for example tert-dodecyl mercaptan. These regulators are then used in amounts of 0.01% bw to 5% bw, based on the total amount of the mixture.
[0283] There is no particular limitation on the emulsifiers that can be used. Preferred are neutral emulsifiers such as ethoxylated mono-, di- and tri-alkylphenols (ethylene oxide degree: 3 to 50, alkyl C4 to C9) or ethoxylated fatty alcohols (ethylene oxide degree: 3 to 50, alkyl C4 to C9), and / or anionic emulsifiers such as alkali metal and ammonium salts of fatty acids (alkyl: C 12 To C 24 ), alkyl sulfate (alkyl group: C8 to C 22 ), ethoxylated alkanol (ethylene oxide degree: 4 to 30, alkyl group: C8 to C 22 ) or ethoxylated alkylphenol (ethylene oxide degree: 3 to 50, alkyl group: C4 to C 20 ) sulfuric acid monoesters, alkyl sulfonic acid (alkyl: C8 to C 22 ) or alkyl aryl sulfonic acid (alkyl group: C4 to C 18 ). Further suitable anionic emulsifiers are mono- or di-C4-C 24 Alkali metal or ammonium salts of alkyl derivatives.
[0284] Particularly preferred are the alkali metal and / or ammonium salts, especially the sodium salts, of: alkylarylsulfonic acids, alkylsulfonic acids (e.g., sulfonated C 12 ~C 18 Suitable emulsifiers include paraffin waxes, alkyl sulfates (e.g. sodium lauryl sulfonate) and sulfate monoesters of ethoxylated alkanols (e.g. sulfoxylated ethoxylates of lauryl alcohol with 2 to 3 ethylene oxide units). Further suitable emulsifiers are fatty acids (C 12 -C 23The present invention relates to the use of sodium or potassium salts of polyols (alkyl groups of ...
[0285] The free radical polymerization reaction can be carried out by the full batch initial charge (batch) technique, but is preferably operated according to the feed technique, especially on an industrial scale. In this technique, the major amount (usually 50% to 100% by weight) of the monomers to be polymerized is added to the polymerization vessel, depending on the progress of the polymerization of the monomers already in the polymerization vessel. In this context, the free radical initiator system can either be completely included in the initial charge to the polymerization vessel, or it can be added to the polymerization reaction continuously or in stages, the addition rate being the rate at which it is consumed during the free radical aqueous latex polymerization. In each individual case, this will depend, as is well known, on the chemical nature of the initiator system and on the polymerization temperature. The initiator system is preferably supplied to the polymerization zone at the rate at which it is consumed.
[0286] Polymerization reaction can also be carried out in the presence of aqueous polymer suspension as polymer (seed latex). Such technology is fundamentally known to those skilled in the art, and is described in, for example, DE-A 4213967, DE-A4213968, EP567811, EP 567812 or EP 567819, which are all incorporated herein by reference. In principle, according to the desired characteristics, it is possible to include the seed in the initial charge, or to add it continuously or in stages during the polymerization process. Polymerization is preferably carried out with the seed in the initial charge. Preferably, the amount of seed polymer is based on monomer a) to monomer d) by weight at 0.05% to 5%, preferably 0.1% to 2%, and specifically in the range of 0.2% to 1%. The polymer particles of the seed latex preferably used have a weight average particle size (weight average diameter) ranging from 10 nm to 100 nm, preferably from 20 nm to 60 nm, and specifically about 30 nm. It is preferred to use polystyrene seeds.
[0287] The polymerization reaction is preferably carried out above atmospheric pressure. The polymerization time can vary within a wide range and is generally from 1 hour to 15 hours, preferably from 3 hours to 10 hours. The polymerization temperature is also variable within a wide range and depends on the initiator used, from about 0°C to 110°C.
[0288] The polymer suspensions prepared in this way generally have a solids content of up to 75% by weight. For use in the hydrogenation process of the invention, it is possible to employ suspensions having these solids contents. However, in certain cases it is advisable to dilute the suspension beforehand to an appropriate solids content. The solids content of the suspension employed is preferably in the range of 5 to 50% by weight, based on the total weight of the suspension.
[0289] Typically, surface-active substances are still present in the polymer suspension, and further substances, such as customary polymerization aids used in latex polymerization, do not have a destructive effect on the hydrogenation process according to the invention. However, it is advisable that the polymer suspension is subjected to a chemical or physical deodorization before the hydrogenation. Physical deodorization by stripping residual monomers with steam is known, for example, from EP584458. EP327006 proposes for its part the use of conventional distillation methods. Chemical deodorization is preferably carried out by a postpolymerization process after the main polymerization. Such methods are described, for example, in DE-A 3834734, EP379892, EP327006, DE-A 4419518, DE-A 4435422 and DE-A 4435423.
[0290] Preferably, according to the invention, the content of diene-based polymer in the aqueous suspension lies in the range from 1% to 75% by weight, more preferably from 5% to 50% by weight, based on the total weight of the latex.
[0291] According to the method of the present invention:
[0292] In the present invention, hydrogenation is understood to mean that preferably at least 50% of the residual double bonds (RDB) present in the starting diene-based polymer are hydrogenated, preferably 70-100%, more preferably 80-100%, even more preferably 90-100%, and most preferably 95-100%.
[0293] In the present invention, the temperature of the selective hydrogenation is preferably 35 to 200°C, more preferably 60 to 200°C, most preferably 80 to 180°C, and most preferably 90 to 160°C; the reaction time of the selective hydrogenation is preferably 10 min to 24 h, more preferably 15 min to 20 h, and most preferably 1 to 8 h; the hydrogen pressure of the selective hydrogenation is preferably 0.5 to 35 MPa, more preferably 3 to 10 MPa; the atmosphere of the selective hydrogenation is preferably pure hydrogen.
[0294] In the present invention, before the hydrogenation, the latex system is preferably degassed using a gas; wherein the gas is preferably nitrogen; the degassing pressure is preferably 0.1-6 MPa; the degassing time is preferably 10-300 min, more preferably 20-240 min, most preferably 30-120 min; the degassing temperature is preferably 0-50° C., more preferably 10-30° C., most preferably 25° C. After the degassing is completed, stirring is preferably continued for 30 min-12 h; the stirring speed is preferably 50-800 r / min, more preferably 200-500 r / min.
[0295] In general, the selective hydrogenation process provided by the present invention can be carried out in a suitable reactor equipped with a temperature regulator and a stirring device. According to the present invention, the polymer latex can be fed into the reactor, degassed as required, and then the catalyst composition can be added in the form of pure raw material or in some cases in the form of a solution with a small amount of organic solvent, and then the reactor is pressurized with hydrogen, or in another alternative embodiment, the reactor can be pressurized with hydrogen and the catalyst composition can be added in the form of pure raw material or solution. Alternatively, according to the present invention, the catalyst composition can be added to the reactor in the form of pure raw material, and then the polymer latex can be fed into the reactor and degassed as required.
[0296] Generally, when the hydrogenation (hydrogenation reaction) is complete to the desired extent, the reaction vessel can be cooled and vented. The resulting hydrogenated latex can be used as a latex if desired or can be coagulated and washed to obtain the hydrogenated polymer in solid form.
[0297] The procatalyst (a) used in the inventive method is very effective, so that the catalyst residue in the final hydrogenated polymer product can be low enough to make the catalyst metal removal or recovery step alleviated or even unnecessary. However, when the desired degree is reached, the procatalyst (a) used in the method process of the present invention can be removed. Such removal can be carried out, for example, by using ion exchange resins, as described in EP2072532 A1 and EPA2072533 A1. The reaction mixture obtained after the hydrogenation is completed can be obtained and treated with ion exchange resins at, for example, 100°C under nitrogen for 48 hours, which causes the combination of the procatalyst (a) and the resin, and the reaction mixture can be processed using common final treatment methods simultaneously.
[0298] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.
[0299] In the following examples and comparative examples provided by the present invention, the materials used in the hydrogenation reaction are listed in Table 1.
[0300] Table 1 Basic raw materials of the embodiment
[0301] Material source NBR latex Laboratory-made Grubbs II Catalyst Sigma-Aldrich Grubbs III Catalyst Sigma-Aldrich Hoveda-Grubbs II Catalyst Sigma-Aldrich Other reagents Conventional reagents, analytical grade
[0302] In the following embodiments and comparative examples provided by the present invention, the analysis and testing involved are as follows:
[0303] FT-IR test: the spectrum of the acrylonitrile-butadiene rubber before, during and after the hydrogenation reaction is recorded on the TENSOR II infrared spectrometer of Bruker.The solution of acrylonitrile-butadiene rubber in chlorobenzene is cast on a KBr disk and the film that is dried and formed for testing.Analyze degree of hydrogenation by FT-IR according to the ASTM D5670 method.
[0304] UV test: The UV spectra of the solution and the catalyst composition of the Hoveda-Grubbs II catalyst were recorded by a TU-1901 UV-visible spectrophotometer from Beijing Puxi General Instrument Co., Ltd. The formation of the catalyst composition was determined based on the change in the peak position of the UV absorption spectrum.
[0305] Catalyst composition preparation example:
[0306] Example 1
[0307] 0.03 g of Hoveda-Grubbs II catalyst was dissolved in 10 g of butanone and 2.5 g of water at room temperature to form a light green solution.
[0308] Example 2
[0309] 0.03 g of Hoveda-Grubbs II catalyst and 2 g of potassium oleate were dissolved in 10 g of butanone and 2.5 g of water at room temperature to form a light green solution which then slowly turned purple.
[0310] Example 3
[0311] 0.03 g of Hoveda-Grubbs II catalyst and 2 g of sodium dodecylbenzenesulfonate were dissolved in 10 g of butanone and 2.5 g of water at room temperature to form a light green solution which then slowly turned yellow.
[0312] Example 4
[0313] 0.03 g of Hoveda-Grubbs II catalyst and 2 g of potassium dodecyl phosphate monoester were dissolved in 10 g of butanone and 2.5 g of water at room temperature to form a light green solution which then slowly turned white.
[0314] The products of Examples 1 to 4 were subjected to UV absorption spectrum test, and the results are shown in Table 2 and Figure 1 As shown, Figure 1 It is the ultraviolet absorption spectrum diagram of the catalyst composition provided by the embodiment of the present invention, wherein 1, 2, 3, and 4 correspond to embodiment 1, embodiment 2, embodiment 3, and embodiment 4, respectively.
[0315] Table 2 UV absorption spectrum results
[0316] serial number Components Absorption peak wavelength (nm) Example 1 Hoveda-Grubbs II + butanone + water 374、320、212 Example 2 Hoveda-Grubbs II + butanone + water + potassium oleate 325、211 Example 3 Hoveda-Grubbs II + butanone + water + sodium dodecylbenzenesulfonate 322、211 Example 4 Hoveda-Grubbs II + butanone + water + potassium dodecyl phosphate 324、211
[0317] The products of Examples 1 to 4 were photographed. Figure 2 As shown, Figure 2 These are sample photos of the catalyst composition provided in the examples of the present invention, wherein (a), (b), (c), and (d) correspond to Example 1 (light green), Example 2 (purple), Example 3 (yellow), and Example 4 (white), respectively.
[0318] Combination Figure 1 and 2 It can be seen that the number and position of the absorption peaks of the sample shifted and the color of the dispersion changed, confirming the formation of the catalyst composition.
[0319] Emulsion hydrogenation example
[0320] Example 5
[0321] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Grubbs II, 1 g of tetrahydrofuran and 2 g of sodium butanesulfonate were pre-mixed at room temperature, the color of the mixture changed from red to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0322] The results showed that after 5 hours, the degree of hydrogenation reached 98.0%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0323] Example 6
[0324] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Grubbs III, 1 g of tetrahydrofuran and 2 g of sodium butanesulfonate were pre-mixed at room temperature, and the color of the mixture changed from brown to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0325] The results showed that after 5 hours, the degree of hydrogenation reached 98.2%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0326] Example 7
[0327] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Hoveda-Grubbs II, 1 g of tetrahydrofuran and 2 g of sodium butanesulfonate were pre-mixed, and the color of the mixture changed from green to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0328] The results showed that after 5 hours, the degree of hydrogenation reached 99.1%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0329] Example 8
[0330] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Grubbs II, 1 g of tetrahydrofuran and 2 g of sodium toluenesulfonate were pre-mixed at room temperature, the color of the mixture changed from red to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0331] The results showed that after 5 hours, the degree of hydrogenation reached 98.5%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0332] Example 9
[0333] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Hoveda-Grubbs II, 1 g of tetrahydrofuran and 2 g of sodium toluenesulfonate were pre-mixed, and the color of the mixture changed from green to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0334] The results showed that after 5 hours, the degree of hydrogenation reached 99.0%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0335] Example 10
[0336] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Hoveda-Grubbs II, 1 g of tetrahydrofuran, 2 g of sodium toluenesulfonate and 20 g of toluene were pre-mixed, and the color of the mixture changed from green to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0337] The results showed that after 5 hours, the degree of hydrogenation reached 99.1%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0338] Embodiment 11
[0339] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone and 2 g of sodium allyl sulfonate were pre-mixed, and the color of the mixture changed from green to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0340] The results showed that after 5 hours, the degree of hydrogenation reached 99.5%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0341] Example 12
[0342] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Grubbs II, 1 g of ethyl acetate and 2 g of sodium acetate were pre-mixed at room temperature, and the color of the mixture changed from red to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0343] The results showed that after 5 hours, the degree of hydrogenation reached 97.6%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0344] Embodiment 13
[0345] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Grubbs III, 1 g of ethyl acetate and 2 g of sodium acetate were pre-mixed at room temperature, and the color of the mixture changed from brown to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0346] The results showed that after 5 hours, the degree of hydrogenation reached 97.8%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0347] Embodiment 14
[0348] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Hoveda-Grubbs II, 1 g of ethyl acetate and 2 g of sodium acetate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, and the stirring speed during degassing was 200 rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0349] The results showed that after 5 hours, the degree of hydrogenation reached 98.0%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0350] Embodiment 15
[0351] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Grubbs II, 1 g of ethyl acetate and 1 g of disodium maleate were pre-mixed at room temperature, and the color of the mixture changed from red to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0352] The results showed that after 5 hours, the degree of hydrogenation reached 98.2%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0353] Example 16
[0354] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Hoveda-Grubbs II, 1 g of ethyl acetate and 1 g of disodium maleate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, and the stirring speed during degassing was 200 rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0355] The results showed that after 5 hours, the degree of hydrogenation reached 98.6%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0356] Embodiment 17
[0357] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Hoveda-Grubbs II, 1 g of ethyl acetate, 1 g of disodium maleate and 20 g of toluene were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0358] The results showed that after 5 hours, the degree of hydrogenation reached 98.8%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0359] Embodiment 18
[0360] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.02 g of Hoveda-Grubbs II, 1 g of butanone and 2 g of sodium acrylate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, and the stirring speed during degassing was 200 rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0361] The results showed that after 5 hours, the degree of hydrogenation reached 99.2%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0362] Embodiment 19
[0363] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Grubbs II, 1 g of diisobutyl phthalate and 1 g of monoethyl phosphate were pre-mixed at room temperature, and the color of the mixture changed from red to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0364] The results showed that after 5 hours, the degree of hydrogenation reached 97.4%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0365] Embodiment 20
[0366] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Grubbs III, 1 g of diisobutyl phthalate and 1 g of monoethyl phosphate were pre-mixed at room temperature, and the color of the mixture changed from brown to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0367] The results showed that after 5 hours, the degree of hydrogenation reached 97.8%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0368] Embodiment 21
[0369] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Hoveda-Grubbs II, 1 g of diisobutyl phthalate and 1 g of monoethyl phosphate were pre-mixed, and the color of the mixture changed from green to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0370] The results showed that after 5 hours, the degree of hydrogenation reached 97.9%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0371] Embodiment 22
[0372] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Grubbs II, 1 g of diisobutyl phthalate and 1 g of dibutyl phosphate were pre-mixed at room temperature, and the color of the mixture changed from red to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0373] The results showed that after 5 hours, the degree of hydrogenation reached 97.7%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0374] Embodiment 23
[0375] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Hoveda-Grubbs II, 1 g of diisobutyl phthalate and 1 g of dibutyl phosphate were pre-mixed, and the color of the mixture changed from green to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0376] The results showed that after 5 hours, the degree of hydrogenation reached 98.3%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0377] Embodiment 24
[0378] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.01 g of Hoveda-Grubbs II, 1 g of diisobutyl phthalate, 1 g of dibutyl phosphate and 20 g of toluene were pre-mixed, and the color of the mixture changed from green to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0379] The results showed that after 5 hours, the degree of hydrogenation reached 98.8%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0380] Embodiment 25
[0381] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone and 1 g of triphenyl phosphate were pre-mixed, and the color of the mixture changed from green to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, and the stirring speed during degassing was 200 rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0382] The results showed that after 5 hours, the degree of hydrogenation reached 98.7%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0383] Embodiment 26
[0384] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone, 20 g of water and 2 g of sodium dodecylbenzene sulfonate were pre-mixed, and the color of the mixture changed from green to yellow, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0385] The results showed that after 5 hours, the degree of hydrogenation reached 99.3%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0386] Embodiment 27
[0387] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone, 20 g of water and 2 g of potassium oleate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0388] The results showed that after 5 hours, the degree of hydrogenation reached 99.2%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0389] Embodiment 28
[0390] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone, 20 g of water and 2 g of potassium dodecyl phosphate monoester were pre-mixed, and the color of the mixture changed from green to white, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0391] The results showed that after 5 hours, the degree of hydrogenation reached 99.0%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0392] Embodiment 29
[0393] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of N,N-dimethylformamide and 2 g of sodium acrylate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0394] The results showed that after 5 hours, the degree of hydrogenation reached 99.6%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0395] Embodiment 30
[0396] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of N-methylpyrrolidone and 2 g of sodium acrylate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0397] The results showed that after 5 hours, the degree of hydrogenation reached 99.5%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0398] Embodiment 31
[0399] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of 1-hexene and 2 g of sodium acrylate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, and the stirring speed during degassing was 200 rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0400] The results showed that after 5 hours, the degree of hydrogenation reached 99.5%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0401] Embodiment 32
[0402] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II and 1 g of butanone were pre-mixed and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0403] The results showed that after 5 hours, the degree of hydrogenation reached 96.8%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0404] Embodiment 33
[0405] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II and 1 g of tetrahydrofuran were pre-mixed and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0406] The results showed that after 5 hours, the degree of hydrogenation reached 96.9%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0407] Embodiment 34
[0408] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II and 1 g of N-methylpyrrolidone were pre-mixed and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0409] The results showed that after 5 hours, the degree of hydrogenation reached 95.6%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0410] Embodiment 35
[0411] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II and 1 g of N, N-dimethylformamide were pre-mixed and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0412] The results showed that after 5 hours, the degree of hydrogenation reached 96.1%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0413] Embodiment 36
[0414] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone, 20 g of water, 0.5 g of sodium acetate and 0.5 g of sodium dodecylbenzene sulfonate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0415] The results showed that after 5 hours, the degree of hydrogenation reached 100%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0416] Embodiment 37
[0417] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex was loaded into the reactor, 0.03 g of Hoveda-Grubbs II, 1 g of butanone, 20 g of water, 0.5 g of sodium butanesulfonate and 0.5 g of potassium oleate were pre-mixed, and the color of the mixture changed from green to purple, and then added to the latex. The latex was then degassed with nitrogen, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, the stirring speed during degassing was 200 rpm, and after the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol and then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0418] The results showed that after 5 hours, the degree of hydrogenation reached 100%. No gel was produced during the reaction and the obtained polymer was soluble in xylene.
[0419] Comparative Example 1
[0420] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20wt%. The average diameter of the polymer particles in the latex was about 80nm. 500g of latex and 0.03g of Grubbs II were loaded into the reactor. The latex was then degassed with nitrogen gas, the degassing temperature was 25°C, the degassing pressure was 0.1Mpa, the degassing time was 30min, and the stirring speed during degassing was 200rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200psi, the speed was increased to 500rpm, and the reaction was carried out for 5h. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0421] The results showed that after 5 hours, the degree of hydrogenation reached 65.9%, and the amount of gel produced by the reaction was about 0.1%.
[0422] Comparative Example 2
[0423] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20wt%. The average diameter of the polymer particles in the latex was about 80nm. 500g of latex and 0.03g of Grubbs III were loaded into the reactor. The latex was then degassed with nitrogen gas, the degassing temperature was 25°C, the degassing pressure was 0.1Mpa, the degassing time was 30min, and the stirring speed during degassing was 200rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200psi, the speed was increased to 500rpm, and the reaction was carried out for 5h. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0424] The results showed that after 5 hours, the degree of hydrogenation reached 70.5%, and the amount of gel produced by the reaction was about 0.1%.
[0425] Comparative Example 3
[0426] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20wt%. The average diameter of the polymer particles in the latex was about 80nm. 500g of latex and 0.03g of Hoveda-Grubbs II were loaded into the reactor. The latex was then degassed with nitrogen gas, the degassing temperature was 25°C, the degassing pressure was 0.1Mpa, the degassing time was 30min, and the stirring speed during degassing was 200rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200psi, the speed was increased to 500rpm, and the reaction was carried out for 5h. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0427] The results showed that after 5 hours, the degree of hydrogenation reached 76.8%, and the amount of gel produced by the reaction was about 0.3%.
[0428] Comparative Example 4
[0429] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20wt%. The average diameter of the polymer particles in the latex was about 80nm. 500g of latex, 0.03g of Hoveda-Grubbs II, and 2g of sodium dodecylbenzene sulfonate were loaded into the reactor. The latex was then degassed with nitrogen gas, the degassing temperature was 25°C, the degassing pressure was 0.1Mpa, the degassing time was 30min, and the stirring speed during degassing was 200rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200psi, the speed was increased to 500rpm, and the reaction was carried out for 5h. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0430] The results showed that after 5 hours, the degree of hydrogenation reached 99.2% and no gel was produced during the reaction.
[0431] Comparative Example 5
[0432] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33 wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20 wt%. The average diameter of the polymer particles in the latex was about 80 nm. 500 g of latex, 0.03 g of Hoveda-Grubbs II, and 2 g of potassium oleate were loaded into the reactor. The latex was then degassed with nitrogen gas, the degassing temperature was 25°C, the degassing pressure was 0.1 MPa, the degassing time was 30 min, and the stirring speed during degassing was 200 rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200 psi, the speed was increased to 500 rpm, and the reaction was carried out for 5 hours. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0433] The results showed that after 5 hours, the degree of hydrogenation reached 99.3% and no gel was produced during the reaction.
[0434] Comparative Example 6
[0435] A 1L stainless steel high pressure reactor with a temperature control device, a stirrer and a hydrogen addition point was used. A butadiene-acrylonitrile polymer latex with an acrylonitrile content of about 33wt% and a Mooney viscosity (ML1+4@100°C) of 55 was used. The solid content of the latex was 20wt%. The average diameter of the polymer particles in the latex was about 80nm. 500g of latex, 0.03g of Hoveda-Grubbs II, and 2g of potassium monoester of dodecyl phosphate were loaded into the reactor. The latex was then degassed with nitrogen gas, the degassing temperature was 25°C, the degassing pressure was 0.1Mpa, the degassing time was 30min, and the stirring speed during degassing was 200rpm. After the degassing was completed, the temperature was raised to 120°C, the hydrogen pressure was increased to 1200psi, the speed was increased to 500rpm, and the reaction was carried out for 5h. A small amount of latex was precipitated with ethanol, and the precipitate was then dissolved in chlorobenzene for analysis of the degree of hydrogenation. The degree of hydrogenation was measured using an FT-IR instrument and calculated using standard methods.
[0436] The results showed that after 5 hours, the degree of hydrogenation reached 99.0% and no gel was produced during the reaction.
[0437] The hydrogenation conditions and results of Examples 5 to 37 and Comparative Examples 1 to 6 are summarized in Table 3:
[0438] Table 3 Comparison of hydrogenation effects of catalysts in the embodiments of the present invention
[0439]
[0440]
[0441]
[0442] Note: phr: the mass of solid content in latex is 100phr.
[0443] It can be seen from the comparison of the examples and comparative examples that in the presence of the co-catalyst (b) and the optional co-catalyst (c), the catalyst composition has no gelling problem and a lower amount of co-catalyst than the catalyst alone or the mixture of the catalyst and the emulsifier.
[0444] Evaluation of basic physical properties of latex and vulcanized rubber after treatment with polyvalent inorganic salts:
[0445] Solid synthetic rubber is prepared by emulsion polymerization. In industry, polyvalent inorganic salts, such as calcium chloride, magnesium chloride, calcium sulfate, aluminum sulfate, etc., are usually used as flocculants to demulsify and flocculate the polymer latex, and the flocculated particles are then washed with water to remove the emulsifier.
[0446] The present invention uses calcium chloride as a flocculant to flocculate and demulsify the latex of Example 16, Example 27, Example 34 and Comparative Example 5, and then washes with water to obtain a solid rubber, which is then vulcanized and tested for basic physical properties. The specific implementation method and data are as follows:
[0447] Flocculation and post-treatment process:
[0448] Prepare a 2% aqueous solution of calcium chloride, take a calcium chloride aqueous solution 1 to 2 times the volume of the latex, drop the latex into it at a certain speed, continue stirring and heating to prevent the latex from agglomerating during the flocculation process. After stirring for a certain period of time, wash repeatedly with a large amount of hot water until the washing liquid is transparent and does not bubble. Control the moisture of the rubber particles and dry them at 60-80℃ to constant weight.
[0449] Emulsifier residual test:
[0450] Because the residue of emulsifier calcium chloride after flocculation is dissolved in ethanol, according to the national standard GB / T3516-2006 for the determination of rubber solvent extracts, ethanol is used for reflux and the weight loss after 48 hours is measured to evaluate the residual amount of emulsifier.
[0451] Vulcanized rubber formula, see Table 4:
[0452] Table 4 Vulcanized rubber formula
[0453] raw materials Servings (phr) HNBR 100 ZnO 5 SA 1 N550 50 TOTM 8 MgO 3 F-40 8 TAIC 1 total 176
[0454] Preparation and vulcanization process:
[0455] (1) The mixing process is divided into four parts: the first stage of internal mixing to add the activator, carbon black and plasticizer, the thin sheet is passed through the open mill, and the second stage of internal mixing to add the vulcanization system, and the thin sheet is passed through the open mill.
[0456] The first stage mixing of the rubber compound is carried out in a Harp torque meter. The initial temperature of the mixing chamber is 60°C, the rotor speed is 50rpm, and the mixing process is: HNBR→2min, zinc oxide + stearic acid + magnesium oxide-75 are added→3min, half of N550 is added→4.5min, the other half of N550 and TOTM are added→6min, F-40 + TAIC are added→8min, cleaning→10, rubber removal; the mixed rubber is triangularly wrapped six times with a roller spacing of 0.3mm on the mixing mill, and the sheet is unrolled with a roller spacing of 2.0mm, and parked at room temperature.
[0457] (2) Vulcanization process: The mixed rubber was vulcanized on a flat vulcanizer. The vulcanization conditions for the test piece were 180℃×10min×10MPa, and the vulcanization conditions for the type A compression test specimen were 180℃×15min×10MPa.
[0458] Physical property test:
[0459] The Shore A hardness of the vulcanized rubber was tested according to GB / T 531.1-2008, and the test was performed three times in parallel, and the median was taken; the tensile properties were tested according to GB / T 528-2009. The tensile rate was 500mm / min, and the test was performed five times in parallel, and the median was taken; the tear strength was tested according to GB / T 529-2008. The tensile rate was 500mm / min, and the test was performed three times in parallel, and the average was taken.
[0460] Compression set: The compression set of vulcanized rubber was tested in accordance with GB / T 7759.1-2015, using a blast oven at 150°C for 72h.
[0461] Oil resistance: The oil resistance of the vulcanized rubber is tested in accordance with GB / T1690-2010. The test conditions are 150℃×168h, and the test contents include mass change rate, volume change rate, hardness change and tensile property change.
[0462] The test results are shown in Table 5 and Table 6:
[0463] Table 5 Ethanol extraction weight loss and vulcanized rubber physical properties data
[0464]
[0465] Table 6 Physical and mechanical properties of vulcanized rubber after resistance to 3# oil
[0466]
[0467] It can be seen from the comparison between the examples and the comparative examples that the catalyst composition has less residual emulsifier, higher hardness, tensile strength and tensile strength, and better compression deformation performance and 3# oil resistance than the method using only a mixture of catalyst and emulsifier.
[0468] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A catalyst composition, characterized in that include: A main catalyst and a first co-catalyst, wherein the main catalyst is a ruthenium complex hydrogenation catalyst and / or an osmium complex hydrogenation catalyst, and the chemical structure of the first co-catalyst contains one or more of N, O, a carbon-carbon double bond and a carbon-carbon triple bond.
2. The catalyst composition according to claim 1, characterized in that The chemical structure of the main catalyst is at least one of formula (I), formula (II) and formula (III): In formula (I), M is ruthenium or osmium; X 1 and X 2 are the same or different anionic ligands; L is an uncharged electron donor; two Rs are the same or different groups independently selected from alkyl, alkyl derivatives, cycloalkyl, cycloalkyl derivatives, alkenyl, alkenyl derivatives, alkynyl, alkynyl derivatives, aryl, aryl derivatives, carboxylate, carboxylate derivatives, alkoxy, alkoxy derivatives, alkenyloxy, alkenyloxy derivatives, alkynyloxy, alkynyloxy derivatives, aryloxy, aryloxy derivatives, alkoxycarbonyl, alkoxycarbonyl derivatives, alkylamino, alkylamino derivatives, thioamino, thioamino derivatives, thioaryl, thioaryl derivatives, alkylsulfonyl, alkylsulfonyl derivatives, alkylsulfinyl or alkylsulfinyl derivatives, and the derivative is a group formed by replacing the corresponding non-derivative group with one or more of alkyl, halogen, alkoxy, aryl and heteroaryl; In formula (II), M is ruthenium or osmium; X 1 and X 2 are the same or different anionic ligands; L is an uncharged electron donor; Y is selected from O, S, NR 1 or PR 1 ; R 1 R is selected from alkyl, alkyl derivatives, cycloalkyl, cycloalkyl derivatives, alkenyl, alkenyl derivatives, alkynyl, alkynyl derivatives, aryl, aryl derivatives, alkoxy, alkoxy derivatives, alkenyloxy, alkenyloxy derivatives, alkynyloxy, alkynyloxy derivatives, aryloxy, aryloxy derivatives, alkoxycarbonyl, alkoxycarbonyl derivatives, alkylamino, alkylamino derivatives, alkylthio, alkylthio derivatives, arylthio, arylthio derivatives, alkylsulfonyl, alkylsulfonyl derivatives, alkylsulfinyl or alkylsulfinyl derivatives, wherein the derivative is a group formed by replacing the corresponding non-derivative group with one or more of alkyl, halogen, alkoxy, aryl and heteroaryl; R 2 , R 3 , R 4 and R 5 independently selected from hydrogen, halogen, nitro, CF3, C1-C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C2~C 20 Alkenyloxy, C2~C 20 Alkynyloxy, C6~C 24 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylamino, C1~C 20 Alkylthio, C6~C 24 Arylthio, C1~C 20 Alkylsulfonyl or C1~C 20 Alkylsulfinyl; R 6 is selected from hydrogen, alkyl, alkenyl, alkynyl or aryl; In formula (III), the dotted line represents a saturated bond or an unsaturated bond, and α and β cannot be unsaturated bonds at the same time; M is ruthenium or osmium; X 1 and X 2 are the same or different anionic ligands; L is an uncharged electron donor; when α is a saturated bond, L 2 NR 7 R 8 , PR 7 R 8 、N=CR 7 R 8 or R 7 C=NR 8 , R 7 and R 8 independently selected from unsubstituted, substituted or heteroatom-containing C1-C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl or C6~C 24 The aromatic group, or R 7 and R 8 are non-aromatic ring structures respectively; when α is a double bond, L 2 NR 7 or PR 7 , R 7 is selected from unsubstituted, substituted or heteroatom-containing C1-C 20 Alkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl or C6~C 24 The aromatic group, or R 7 is a non-aromatic ring structure; A and B are independently selected from hydrocarbons, substituted hydrocarbons, hydrocarbons containing heteroatoms, or hydrocarbons with substituted groups and heteroatoms, or A and B are atoms in an aromatic ring; m represents 0 or 1; n represents 0 or 1; R 6 is selected from hydrogen, alkyl, alkenyl or aryl.
3. The catalyst composition according to claim 2, characterized in that In formula (I), formula (II) and formula (III), M is ruthenium; X 1 and X 2 independently selected from hydrogen, halogen, pseudohalogen, C1-C 30 Alkyl, C6~C 24 Aryl, C1~C 20 Alkoxy, C6~C 24 Aryloxy, C3~C 20 Alkyl diketone, C6~C 24 Aryl diketone, C1~C 20 Carboxylates, C6~C 24 Alkyl sulfonate, C6~C 24 Aryl sulfonate, C1~C 20 Alkyl mercaptan, C6~C 24 Aromatic thiols, C1~C 20 Alkylsulfonyl or C1-C 20 -alkylsulfinyl; L is selected from phosphine, sulfonated phosphine, phosphate, hypophosphorous acid, phosphite, phosphonate, arsine, stibine, ether, amine, amide, sulfoxide, carboxyl, nitrite, pyridine, thioether or N-heterocyclic carbene ligand.
4. The catalyst composition according to claim 3, characterized in that In formula (I), formula (II) and formula (III), the X 1 and X 2 Independently selected from chlorine, CF3COO, CH3COO, CFH2COO, (CH3)3CO, (CF3)2(CH3)CO, (CF3)(CH3)2CO, phenoxy, methoxy, ethoxy, toluenesulfonate, methanesulfonic acid or trifluoromethylsulfonate; L is at least one of the structures shown in formula (IV-a) to formula (IV-f): Among them, R 9 , R 10 , R 11 and R 12 independently selected from hydrogen, C1-C 30 Alkyl, C3~C 20 Cycloalkyl, C2~C 20 Alkenyl, C2~C 20 Alkynyl, C6~C 24 Aryl, C7~C 25 Alkyl, C2~C 20 Heterocyclic aromatic groups, C2~C 20 Heterocyclic ring, C1~C 20 Alkoxy, C2~C 20 Alkenyl, C2~C 20 Alkynyloxy, C6~C 20 Aryloxy, C2~C 20 Alkoxycarbonyl, C1~C 20 Alkylthio, C6~C 20 R is arylthio, -Si(R')3, -O-Si(R')3, -OC(=O)R', -C(=O)R', -C(=O)N(R')2, -NR-C(=O)-N(R')2, -SO2N(R')2, -S(=O)R', -S(=O)2R', -OS(=O)2R', halogen, nitro or cyano, R' is selected from hydrogen, alkyl, cycloalkyl, alkenyl, alkynyl, aryl or heteroaryl; R 13 , R 14 and R 15 Independently selected from C1 to C 20 of alkyl.
5. The catalyst composition according to claim 1, characterized in that The main catalyst comprises at least one of the following structural complexes:
6. The catalyst composition according to claim 1, characterized in that The first co-catalyst is one or more of esters, ethers, ketones, amines, carbamates, olefins and alkynes.
7. The catalyst composition according to claim 6, characterized in that The first co-catalyst is one or more of aliphatic monocarboxylic acid alkyl esters, aromatic monocarboxylic acid alkyl esters, aliphatic polycarboxylic acid alkyl esters, aromatic polycarboxylic acid alkyl esters, polyol alkyl esters, polyol cycloalkyl esters, polyol aryl esters, polyol alkylaryl esters, aliphatic ethers, cycloaliphatic ethers, aliphatic diethers, aliphatic ketones, aliphatic amines, aliphatic diamines, olefins and alkynes.
8. The catalyst composition according to claim 7, characterized in that The first co-catalyst is C1-C 20 Saturated fatty acid alkyl esters, C7~C 24 Aromatic carboxylic acid alkyl esters, C2~C 20 -Diol aromatic ester, C2~C 20 Fatty ethers, C3~C 20 Cyclic ethers, C5~C 20 Aliphatic diethers, C3~C 20 Saturated fatty ketones, C3~C 20 Saturated fatty amines, C3~C 20 Saturated fatty diamines, C2~C 20 Olefins and C2~C 20 One or more of the alkynes.
9. The catalyst composition according to claim 1, characterized in that The molar ratio of the main catalyst to the first co-catalyst is 1:(20-100).
10. The catalyst composition according to claim 1, characterized in that The catalyst composition further includes a second co-catalyst, which is one or more of carboxylate, sulfonate and phosphate.
11. The catalyst composition according to claim 10, characterized in that The second co-catalyst is one or more of non-emulsifier carboxylates, emulsifier carboxylates, non-emulsifier sulfonates, emulsifier sulfonates, non-emulsifier phosphates and emulsifier phosphates.
12. The catalyst composition according to claim 11, characterized in that The non-emulsified formulation carboxylate is one or more of formates, acetates, propionates, butyrates, valerates, oxalates, malonates, succinates, glutarates, triacrylic acid salts, trisuccinates, triglutarates, maleates, tartrates, fumarates, malates, amino acid salts, cyclopentaneates, alginates, gluconates, crotonates, itaconates, citrates, mesaconic acids, aromatic carboxylates, heteroaromatic ring carboxylates, imidazoline carboxylates, pyruvates, epoxysuccinates, salicylates, fluorenedioates, hydroxypropionates, levulinates, furandicarboxylates, acrylates, methacrylates and trifluoroformates; The emulsifier-type carboxylate is one or more of resinate, modified resinate, alkanoyl amino acid salt, fatty acid polypeptide condensate, acyl lactylate and long-chain alkyl carboxylate of C8 or above; The non-emulsifier type sulfonate is methanesulfonate, trifluoromethylsulfonate, ethanesulfonate, perfluoroethanesulfonate, propanesulfonate, perfluoropropanesulfonate, hydroxypropanesulfonate, butylsulfonate, perfluorobutylsulfonate, hydroxybutylsulfonate, toluenesulfonate, dinitrotoluenesulfonate, styrenesulfonate, vinylsulfonate, allylsulfonate, methylallylsulfonate, perfluorosulfonic acid polymer, aromatic sulfonate, heteroaromatic ring sulfonate, cycloalkanesulfonate, hydroxybenzoate, One or more of 2-(2-aminoethyl)aminoethanesulfonate, N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate, N-tris(hydroxymethyl)methyl-2-aminoethanesulfonate, aminosulfonate, aminoaromaticsulfonate, ethylenediamineethanesulfonate, chrysinsulfonate, anthraquinonesulfonate, diaminoformylsulfonate, quinocinonesulfonate, thiazolesulfonate, imidazolinesulfonate, allylimidazolinesulfonate, triazolonesulfonate, triazinesulfonate and flavonesulfonate; The emulsifier type sulfonate is one or more of alkyl aryl sulfonate, alkyl diphenyl oxide disulfonate, α-hydroxy sulfonate, α-olefin sulfonate, petroleum sulfonate, α-sulfomonocarboxylate, α-sulfomonocarboxylate derivative, fatty acid sulfoalkyl ester salt derivative, fatty acid sulfoalkyl amide salt derivative, succinate sulfonate, lignin sulfonate, alkyl glyceryl ether sulfonate, 2-aminoethanesulfonate, 2-aminoethanesulfonate derivative and C8 or higher long-chain alkyl sulfonate; The non-emulsifier type phosphate salt is monomethyl phosphate, monoethyl phosphate, monobutyl phosphate, dimethyl phosphate, diethyl phosphate, dibutyl phosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, monophenyl phosphate, diphenyl phosphate, triphenyl phosphate, mono-p-tolyl phosphate, di-p-tolyl phosphate, tri-p-tolyl phosphate, mono-o-tolyl phosphate, di-o-tolyl phosphate, tri-o-tolyl phosphate, mono-m-tolyl phosphate, di-m-tolyl phosphate, tri-m-tolyl phosphate, mono-p-isopropylphenyl phosphate, di-p-isopropylphenyl phosphate, tri-p-isopropylphenyl phosphate, mono-p-tert-butyl phosphate phenyl ester salt, di-p-tert-butylphenyl phosphate salt, tri-p-tert-butylphenyl phosphate, mono-p-methoxyphenyl phosphate salt, di-p-methoxyphenyl phosphate salt, tri-p-methoxyphenyl phosphate, phenyl dimethyl phosphate, phenyl diethyl phosphate, phenyl dibutyl phosphate, diphenyl methyl phosphate, diphenyl ethyl phosphate, diphenyl butyl phosphate, p-tolyl dimethyl phosphate, p-tolyl diethyl phosphate, p-tolyl dibutyl phosphate, o-tolyl dimethyl phosphate, o-tolyl diethyl phosphate, o-tolyl dibutyl phosphate, m-tolyl dimethyl phosphate, m-tolyl diethyl phosphate, m-tolyl dibutyl phosphate, di-p-tolyl methyl phosphate Ester, di-p-tolyl ethyl phosphate, di-p-tolyl butyl phosphate, di-o-tolyl methyl phosphate, di-o-tolyl ethyl phosphate, di-o-tolyl butyl phosphate, di-m-tolyl methyl phosphate, di-m-tolyl ethyl phosphate, di-m-tolyl butyl phosphate, di-p-isopropylphenyl methyl phosphate, di-p-isopropylphenyl ethyl phosphate, di-p-isopropylphenyl butyl phosphate, di-p-isopropylphenyl dimethyl phosphate, di-p-isopropylphenyl diethyl phosphate, di-p-isopropylphenyl dibutyl phosphate, di-p-isopropylphenyl dimethyl phosphate, di-p-isopropylphenyl diethyl phosphate, di-p-isopropylphenyl dibutyl phosphate, di-p-isopropylphenyl methyl phosphate, di-p-isopropylphenyl ethyl phosphate, phosphorus One or more of di-p-tert-butylphenyl butyl phosphate, phenyl di-p-tolyl phosphate, phenyl di-p-isopropylphenyl phosphate, phenyl di-p-tert-butylphenyl phosphate, p-tolyl diphenyl phosphate, p-tolyl p-diisopropylphenyl phosphate, p-tolyl p-di-tert-butylphenyl phosphate, o-tolyl p-diisopropylphenyl phosphate, o-tolyl p-di-tert-butylphenyl phosphate, m-tolyl p-diisopropylphenyl phosphate, m-tolyl p-di-tert-butylphenyl phosphate, p-isopropylbenzene di-p-tolyl phosphate, p-isopropylbenzene di-o-tolyl phosphate, p-isopropylbenzene di-m-tolyl phosphate, p-isopropylbenzene di-p-phenyl phosphate and p-isopropylbenzene di-p-tert-butylphenyl phosphate; The emulsifier type phosphate salt is one or more of fatty alcohol polyvinyl ether phosphate monoester salt, fatty alcohol polyvinyl ether phosphate diester salt, alkylphenol polyoxyethylene ether phosphate monoester salt, alkylphenol polyoxyethylene ether phosphate diester salt, alcohol ether phosphate ester salt, phenol ether phosphate ester salt, long-chain alkyl phosphate monoester salt of C8 or above, and long-chain alkyl phosphate diester salt of C8 or above.
13. The catalyst composition according to claim 10, characterized in that The molar ratio of the main catalyst to the second co-catalyst is 1:(100-10000).
14. The catalyst composition according to claim 1, characterized in that The catalyst composition is in liquid form.
15. The catalyst composition according to claim 1, characterized in that The catalyst composition also includes a solvent.
16. A method for selective hydrogenation of conjugated diene latex, characterized in that: The following steps are involved: In the presence of the catalyst composition according to any one of claims 1 to 15, the conjugated diene latex is selectively hydrogenated to obtain hydrogenated conjugated diene latex.
17. The method according to claim 16, characterized in that The polymer in the conjugated diene latex contains at least one repeating unit of a C4-C6 conjugated diene.
18. The method according to claim 17, characterized in that The polymer in the conjugated diene latex further contains repeating units of at least one other copolymerizable monomer.
19. The method according to claim 18, characterized in that The polymer in the conjugated diene latex is a copolymer of 1,3-butadiene and acrylonitrile.
20. The method according to claim 16, characterized in that The amount of the main catalyst is 0.001-5wt% of the mass of the conjugated diene latex; the amount of the first co-catalyst is 0.01-5wt% of the mass of the conjugated diene latex.
21. The method according to claim 20, characterized in that When the catalyst composition includes a second co-catalyst, the amount of the second co-catalyst used is 0.1 to 10 wt % based on the mass of the conjugated diene latex.
22. The method according to claim 16, characterized in that The temperature of the selective hydrogenation is 35-200° C.; the time of the selective hydrogenation is 10 min-24 h; and the hydrogen pressure of the selective hydrogenation is 0.5-35 MPa.
23. A hydrogenated conjugated diene latex, characterized in that: Prepared according to the method according to any one of claims 16 to 22.
24. Use of the hydrogenated conjugated diene latex according to claim 23 in impregnation, adhesives, coatings, film formation or preparation of composite materials.
25. A molded product, characterized in that: The components of the molded article include the hydrogenated conjugated diene latex described in claim 23.
26. The molded article according to claim 25, characterized in that The shaped articles include one or more of sealing strips, sealing gaskets, belts, hoses, bearing pads, baffles, wellhead seals, valve seals, cable jackets, wheels, rollers, in-situ gaskets and pipeline seals.
Citation Information
Patent Citations
Catalyst compositions and their use for hydrogenation of nitrile rubber
CN103974772A
Method for producing hydrogenated copolymer through hydrogenation of conjugated diene
CN110627928A
Cited By
Catalyst composition, selective hydrogenation method for conjugated diene latex, hydrogenated conjugated diene latex and use thereof
WO2025201384A1