Method for improving uniformity and fine grain effect of refiner
By using a magnetic field outside the pressure chamber furnace to stir the aluminum alloy melt and the refinement agent, the problem of deposition and aggregation of the refinement agent is solved, the uniform distribution of the refinement agent and grain refinement are achieved, and the quality of the casting is improved. Mechanical properties.
Patent Information
- Application Number
- CN202410696361.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-11-29
AI Technical Summary
During the pressure casting process, the refiner particles are prone to settle and aggregation, resulting in unstable refiner effect, reduced casting quality, and increased inclusions and casting defects.
Use magnetic fields (electromagnetic stirring, pulsed magnetic field, alternating magnetic field) outside the pressure chamber furnace to stir the aluminum alloy melt and refining agent to ensure uniform distribution of the refining agent and reduce defects such as loosening, shrinkage and segregation in the castings.
Effectively control grain size, improve casting quality, reduce pores, inclusions and shrinkage, improve strength and plastic properties, and prepare tissue for subsequent processing processes.
Smart Images

Figure CN119035503A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting, and more particularly relates to a method for improving the uniformity and grain refining effect of a refiner. Background Art
[0002] Al-Si alloy is a kind of cast aluminum alloy with light weight, high specific strength and good fluidity. It is the alloy with the most types and the widest application range among cast aluminum alloys. With the development of modern industry and social needs, aluminum alloy as the main lightweight material has been widely used in the automotive industry, shipbuilding and aerospace. In the automotive field, cast aluminum silicon alloy can be made into engine cylinder block, cylinder head, automobile wheel hub and chassis and other parts.
[0003] In Al-Si alloys, low-pressure casting and differential pressure casting are the most commonly used casting methods in industrial production. The quality of castings depends on the solidification process and microstructure control of the alloy. The normal as-cast microstructure includes three classic regions, namely the surface fine grain region, the central equiaxed grain region, and the columnar grain region between the two. Refining the grains during the solidification process can reduce columnar grains and refine equiaxed grains, thereby reducing casting defects such as pores, inclusions, and shrinkage cavities in the castings, improving mechanical properties such as strength and plasticity, and preparing the microstructure for subsequent processing. Adding grain refiners is an effective method to refine the solidification microstructure. The refiner method refers to directly or indirectly adding a phase that can promote heterogeneous nucleation into the liquid metal, so that the metal has a large number of heterogeneous nucleation substrates when it is in the liquid state, which can greatly increase the nucleation rate and reduce the grain size. The traditional way to add refiners is to add them directly into the holding furnace. Due to gravity, the refiner particles will settle and gather at the bottom of the melt during the casting process, resulting in a decrease in the refinement of the casting. At the same time, it will also reduce the refinement effect of the refiner, resulting in the subsequent grain size of the casting being different from the previous one. In addition, due to the sedimentation and aggregation of the refiner particles, these sedimented and aggregated refiners will increase the inclusions in the casting and produce refiner residues, ultimately reducing the quality of the casting. Summary of the invention
[0004] 1. Problems to be solved
[0005] In order to solve the problem in the prior art that the refiner particles are naturally added during the pressure casting process, which causes the refiner particles to settle and aggregate at the bottom of the holding furnace, resulting in the gradual instability of the refiner effect and the reduction of the casting quality, the present application proposes a method of adding a magnetic field (electromagnetic stirring, pulse magnetic field, alternating magnetic field, etc.) outside the pressure chamber furnace body when adding refiner during pressure casting to stir the aluminum alloy melt and the refiner in the furnace body at the same time, so that the refiner is evenly distributed in the aluminum alloy melt, which can effectively reduce the casting defects such as looseness, shrinkage, segregation and hot cracking caused by aluminum alloy pressure casting, so that the subsequent filling, pressurized solidification, pressure-holding shrinkage compensation and pressure-release removal process can be completed smoothly. The improved process effectively controls the grain size and can effectively improve the quality of castings.
[0006] 2. Technical solution
[0007] To solve the above problems, the present invention adopts the following technical solutions.
[0008] A method for improving the uniformity and grain refining effect of a refiner comprises the following steps:
[0009] (1) Before the alloy melt is pressed into the mold cavity through the pouring channel, 0.05-0.3wt% of a commercial refiner is added into the pressure chamber furnace body through the pouring channel, and the alloy melt and the refiner that have not entered the mold cavity are fully stirred by an electromagnetic coil device located outside the pouring channel or outside the pressure chamber, and then the alloy melt that has reached the specified temperature is pressed into the mold cavity for filling, pressurized solidification, pressure-maintaining shrinkage compensation, and pressure-relieving and removing the parts;
[0010] (2) Repeat step (1) until the alloy liquid in the holding furnace reaches the maximum number of strokes that can be used, that is, the alloy liquid in the holding furnace is reduced to a weight that is specified in the process to suspend the casting cycle.
[0011] As a further improvement of the technical solution, after electromagnetic stirring is performed on the melt to which the refiner is added, the volume of the melt to which the refiner is added can ensure that the filling of the casting is completed.
[0012] As a further improvement of the technical solution, for differential pressure and low pressure casting, when casting is completed, the pressure is completely released, that is, consistent with the atmospheric pressure, and then the parts are taken out; or, when casting is completed, the pressure is partially released, so that a certain pressure is still maintained in the holding furnace, so that the alloy melt remains in the pouring channel and continues to be electromagnetically stirred to ensure the next filling.
[0013] As a further improvement of the technical solution, for differential pressure and low pressure casting, if the pressure is completely released when a casting cycle is completed, the parts are taken out. Before the next melt filling, the molten metal is pressed into the area where the electromagnetic stirring coil is located, and a refiner is added for electromagnetic stirring. After the stirring is completed, it is pressed into the mold cavity for casting.
[0014] As a further improvement of the technical solution, for differential pressure and low pressure casting, if a casting cycle is completed, the pressure in the holding furnace is partially released. 保 Calculated by the following formula:
[0015] p 保 =p0+ρ g Δh
[0016] Wherein, p0 is the atmospheric pressure, ρ is the density of the alloy melt, g is the acceleration due to gravity, and Δh is the difference between the liquid level of the alloy melt in the pouring channel and the liquid pool height in the holding furnace.
[0017] 3. Beneficial effects
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention can improve the problem of refiner aggregation at the bottom of the molten pool caused by the traditional refiner addition method, and realize accurate control of the refiner addition amount for parts with different structures; thereby more effectively reducing columnar crystals, refining equiaxed crystals, further reducing casting defects such as pores, inclusions, shrinkage cavities in castings, improving mechanical properties such as strength and plasticity, making organizational preparations for subsequent processing technology, and also reducing subsequent processing steps. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The double-chamber furnace used for differential pressure casting of the present invention has a small pressure chamber extending outside the heat preservation chamber, and a pull-out switch is opened (and a seal is made to facilitate the subsequent passage of aluminum alloy melt), and an external magnetic field is placed on the periphery thereof for stirring;
[0021] Figure 2 In order to apply the present invention to low-pressure casting, a small molten pool is added to the middle tube between the mold cavity and the liquid pool, and a pull-out switch is opened on the top, and an external magnetic field is placed on the periphery for stirring;
[0022] Figure 3 The double-chamber furnace of the present invention is applied to low-pressure casting. A small pressure chamber is extended outside the heat preservation chamber, and a pull-out switch is opened. An external magnetic field is placed on the periphery thereof for stirring.
[0023] Figure 4 In order to apply the present invention to differential pressure casting, a small molten pool is added to the middle tube between the mold cavity and the liquid pool, and a pull-out switch is opened on the top, and an external magnetic field is placed on the periphery for stirring;
[0024] Figure 1In the middle, 1-1 is the upper compressed air inlet, 1-2 is the mold cavity, 1-3 is the liquid riser, 1-4 is the pull-out switch, 1-5 is the pressure chamber, 1-6 is the external magnetic field, 1-7 is the aluminum alloy melt, 1-8 is the lower compressed air inlet, and 1-9 is the holding furnace;
[0025] Figure 2 2-1 is the mold cavity, 2-2 is the liquid riser, 2-3 is the pull-out switch, 2-4 is the external magnetic field, 2-5 is the pressure chamber, 2-6 is the holding furnace, 2-7 is the compressed air inlet, and 2-8 is the aluminum alloy melt;
[0026] Figure 3 3-1 is the mold cavity, 3-2 is the liquid riser, 3-3 is the pull-out switch, 3-4 is the pressure chamber, 3-5 is the external magnetic field, 3-6 is the aluminum alloy melt, 3-7 is the compressed air inlet, and 3-8 is the holding furnace;
[0027] Figure 4 In the middle, 4-1 is the upper compressed air inlet, 4-2 is the mold cavity, 4-3 is the liquid riser, 4-4 is the pull-out switch, 4-5 is the external magnetic field, 4-6 is the pressure chamber, 4-7 is the insulation furnace, 4-8 is the lower compressed air inlet, and 4-9 is the aluminum alloy melt. DETAILED DESCRIPTION
[0028] Exemplary embodiments of the present invention are described in detail below. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments may be implemented and various changes may be made to the present invention without departing from the spirit and scope of the present invention. The more detailed description of the embodiments of the present invention below is not intended to limit the scope of the claimed invention, but is merely for illustration and does not limit the description of the features and characteristics of the present invention, in order to propose the best mode for performing the present invention, and is sufficient to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.
[0029] Example 1
[0030] Dual-chamber differential pressure casting A356 aluminum alloy wheels.
[0031] First, the A356 aluminum alloy is refined at 720℃±10℃, and the refined A356 melt is added to the holding furnace to be kept at 720℃±10℃. Then, the pressure difference between the upper and lower pressure cylinders is used to provide an upward net pressure of 12000Pa, and 120 kg of the metal melt is pressed into the pressure chamber for temporary storage, and then the pull-out switch outside the pressure chamber is opened to add 0.2wt% commercial refiner, and the external magnetic field is turned on to stir the A356 melt and the commercial refiner in the pressure chamber, so that the metal melt stays in the stirring zone for 120s. Finally, after the stirring is completed, pressure is applied again to press the fully stirred A356 melt into the cavity through the riser tube by 15 kg, and the pressure is maintained until the shrinkage is completed. After cooling, the pressure is removed and the wheel hub is taken out. The above process is repeated until the alloy liquid in the holding furnace is reduced to the weight required by the process to suspend the casting cycle.
[0032] In the present application, the power and frequency of the magnetic field are controlled by a microcomputer system, and the magnetic field frequency is 20-50 Hz and the power is 1.7-1.8 kW.
[0033] Example 2
[0034] Low pressure casting A356 aluminum alloy steering knuckle.
[0035] First, the A356 aluminum alloy is refined at 720℃±10℃, and the refined A356 melt is added to the holding furnace and kept at 720℃±10℃. The air is used to apply a net pressure of 12000Pa, and 30 kg of the metal melt is pressed into the pressure chamber for temporary storage. Then, the pull-out switch outside the pressure chamber is opened to add 0.2wt% of commercial refiner, and the external magnetic field is turned on to stir the A356 melt and the commercial refiner in the pressure chamber, so that the metal melt stays in the stirring zone for 120s. Finally, after the stirring is completed, pressure is applied again to press the fully stirred A356 melt into the cavity through the riser tube. The pressure is maintained until the shrinkage is completed. After cooling, the pressure is removed and the wheel hub is taken out. The above process is repeated until the alloy liquid in the holding furnace is reduced to the weight required by the process to suspend the casting cycle.
[0036] Example 3
[0037] Dual-chamber low-pressure casting A356 aluminum alloy wheels.
[0038] First, the A356 aluminum alloy is refined at 720℃±10℃, and the refined A356 melt is added to the holding furnace and kept at 720℃±10℃. The air is used to apply a net pressure of 12000Pa, and 120 kg of the metal melt is pressed into the pressure chamber for temporary storage. Then, the pull-out switch outside the pressure chamber is opened to add 0.2wt% of commercial refiner, and the external magnetic field is turned on to stir the A356 melt and the commercial refiner in the pressure chamber, so that the metal melt stays in the stirring zone for 120s. Finally, after the stirring is completed, pressure is applied again to press the fully stirred A356 melt into the cavity through the riser tube at 15 kg, and the pressure is maintained until the shrinkage is completed. After cooling, the pressure is removed and the wheel hub is taken out. The above process is repeated until the alloy liquid in the holding furnace is reduced to the weight required by the process to suspend the casting cycle.
[0039] Example 4
[0040] Differential pressure casting A356 aluminum alloy steering knuckle.
[0041] First, the A356 aluminum alloy is refined at 720℃±10℃, and the refined A356 melt is added to the holding furnace to be kept at 720℃±10℃. Then, the pressure difference between the upper and lower pressure cylinders is used to provide an upward net pressure of 12000Pa, and 30 kg of the metal melt is pressed into the pressure chamber for temporary storage, and then the pull-out switch outside the pressure chamber is opened to add 0.2wt% commercial refiner, and the external magnetic field is turned on to stir the A356 melt and the commercial refiner in the pressure chamber, so that the metal melt stays in the stirring zone for 120s. Finally, after the stirring is completed, pressure is applied again to press the fully stirred A356 melt into the cavity through the riser tube by 10 kg, and the pressure is maintained until the shrinkage is completed. After cooling, the pressure is removed and the wheel hub is taken out. The above process is repeated until the alloy liquid in the holding furnace is reduced to the weight required by the process to suspend the casting cycle.
[0042] The examples described in the present invention are merely descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made to the technical solutions of the present invention by engineers and technicians in this field should all fall within the protection scope of the present invention.
Claims
1. A method for improving the uniformity and grain refining effect of a refiner, Features: The following steps are involved: (1) Before the alloy melt is pressed into the mold cavity through the pouring channel, 0.05-0.3wt% of a commercial refiner is added into the pressure chamber furnace body through the pouring channel, and the alloy melt and the refiner that have not entered the mold cavity are fully stirred by an electromagnetic coil device located outside the pouring channel or outside the pressure chamber, and then the alloy melt that has reached the specified temperature is pressed into the mold cavity for filling, pressurized solidification, pressure-maintaining shrinkage compensation, and pressure-relieving and removing the parts; (2) Repeat step (1) until the alloy liquid in the holding furnace reaches the maximum number of strokes that can be used, that is, the alloy liquid in the holding furnace is reduced to a weight that is specified in the process to suspend the casting cycle.
2. A method for improving uniformity and grain refining effect of a refiner according to claim 1, Features: After electromagnetic stirring is performed on the melt with the refiner added, the volume of the melt with the refiner added can ensure the complete filling of the casting.
3. A method for improving the uniformity and grain refining effect of a refiner according to claim 1 or 2, Features: For differential pressure and low pressure casting, when casting is completed, the pressure is completely released, that is, it is consistent with atmospheric pressure, and then the parts are taken out; or, when casting is completed, the pressure is partially released, so that a certain pressure is still maintained in the holding furnace, so that the alloy melt remains in the pouring channel and continues to be electromagnetically stirred to ensure the next filling.
4. A method for improving uniformity and grain refining effect of a refiner according to claim 3, Features: For differential pressure and low pressure casting, if the pressure is completely released when a casting cycle is completed, the parts are taken out. Before the next melt filling, the molten metal is pressed into the area where the electromagnetic stirring coil is located, and the refiner is added for electromagnetic stirring. After the stirring is completed, it is pressed into the cavity for casting.
5. A method for improving uniformity and grain refining effect of a refiner according to claim 3, Features: For differential pressure and low pressure casting, if a casting cycle is completed, the pressure in the holding furnace is partially released. 保 Calculated by the following formula: p 保 =p 0 +ρgΔh Among them, p 0 is the atmospheric pressure, ρ is the density of the alloy melt, g is the acceleration of gravity, and Δh is the difference between the liquid level of the alloy melt in the pouring channel and the liquid pool height in the holding furnace.
Citation Information
Cited By