Silver powder with hollow structure and preparation method thereof

By preparing silver powder under ultrasonic conditions, reducing the use of dispersants, and employing redox reactions and controlling pH values, the problems of high cost and insufficient sintering activity of silver powder were solved, achieving the preparation of silver powder with high dispersibility and high sintering activity.

CN119035536APending Publication Date: 2024-11-29HUBEI YINKE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411422277.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In existing technologies, the cost of preparing silver powder is high and the sintering activity is insufficient, making it difficult to meet the photovoltaic industry's need to reduce the consumption per cell.

Method used

Silver powder with a hollow structure was prepared by reducing the use of dispersants in an ultrasonic environment, using a redox reaction and mixing oxidizing and reducing solutions under ultrasonic conditions, and controlling the pH value.

Benefits of technology

It reduces preparation costs, improves the dispersibility and sintering activity of silver powder, and is suitable for photovoltaic silver paste applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035536A_ABST
    Figure CN119035536A_ABST
Patent Text Reader

Abstract

The invention provides silver powder with a hollow structure and a preparation method of the silver powder. The method comprises the steps that oxidation liquid and reduction liquid are prepared respectively; putting the reduction liquid into ultrasonic equipment, and adding the oxidation liquid into the reduction liquid in an ultrasonic state; continuously carrying out ultrasonic treatment for a first preset duration to obtain a suspension reaction solution; and separating and drying the suspension reaction liquid to obtain the target silver powder. According to the preparation method of the silver powder with the hollow structure, the ultrasonic waves are introduced in the reaction process, so that the silver microcrystals have a good dispersion effect in the reaction solution, a dispersing agent is reduced and even does not need to be added, and the silver powder prepared in the mode is good in dispersity and high in sintering activity; and a hollow structure exists in the silver powder, so that the sintering performance of the silver powder can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of new precious metal materials, and in particular to a silver powder with a hollow structure and a preparation method thereof. Background Art

[0002] Photovoltaic silver paste has become the main raw material for printed solar panels due to its excellent rheological and conductive properties. Silver powder, as the main conductive phase in solar cell silver paste, accounts for about 90% of the mass ratio in the silver paste, which plays an important role in the electrical properties and cost of the silver paste. With the development demand of the photovoltaic industry to reduce the unit consumption of solar cells, improving the sintering activity of silver powder and reducing the cost of silver powder are the main research directions of photovoltaic silver powder. Summary of the invention

[0003] The purpose of the present application is to provide a silver powder with a hollow structure and a preparation method thereof, which reduces the use of dispersants by preparing the silver powder under an ultrasonic environment, simplifies the preparation and reduces the cost, and has high sintering activity of the silver powder.

[0004] In a first aspect, the present application provides a method for preparing a silver powder having a hollow structure, comprising:

[0005] preparing an oxidizing solution and a reducing solution respectively;

[0006] placing the reducing liquid in an ultrasonic device, and adding the oxidizing liquid into the reducing liquid in an ultrasonic state;

[0007] After the ultrasonic wave is continuously applied for a first preset time, a suspended reaction liquid is obtained;

[0008] The suspended reaction liquid is separated and dried to obtain the target silver powder.

[0009] In some possible embodiments, after preparing the oxidizing solution and the reducing solution respectively, the method further includes:

[0010] A pH regulator is added to the reducing solution to adjust the pH of the reducing solution to 2.2-10, thereby obtaining a new reducing solution with adjusted pH.

[0011] In some possible embodiments, the pH adjuster is at least one of methylamine, trimethylamine, triethylamine, ammonia water, ammonium carbonate, sodium carbonate, sodium hydroxide or potassium hydroxide.

[0012] In some possible embodiments, the solution temperature of the oxidizing solution and the reducing solution is 25-35°C.

[0013] In some possible embodiments, placing the reducing liquid in an ultrasonic device and adding the oxidizing liquid to the reducing liquid in an ultrasonic state includes:

[0014] placing the reducing liquid in an ultrasonic device, and controlling the ultrasonic device to emit ultrasound at a preset frequency;

[0015] The oxidizing liquid is added into the reducing liquid under ultrasonic state and within a second preset time period.

[0016] In some possible embodiments, the ultrasonic frequency of the ultrasonic device is 2-20KHZ.

[0017] In some possible embodiments, the step of separating and drying the suspended reaction liquid to obtain the target silver powder comprises:

[0018] Precipitating the suspended reaction liquid and separating the precipitate;

[0019] washing the precipitate to obtain initial silver powder;

[0020] The initial silver powder is dried at a preset drying temperature for a third preset time to obtain the target silver powder.

[0021] In some possible embodiments, the prepared silver powder has a hollow structure.

[0022] In some possible embodiments, the prepared silver powder has a particle size of 1-2 μm, a bulk density of 2-4 g / cm3, and a specific surface area of ​​0.2-0.6 m 2 / g.

[0023] In a second aspect, an embodiment of the present application provides a silver powder, which is prepared by a preparation method of a silver powder with a hollow structure as described in any one of the above items.

[0024] The present application provides a silver powder with a hollow structure and a preparation method thereof, the method comprising preparing an oxidizing solution and a reducing solution respectively; placing the reducing solution in an ultrasonic device, and adding the oxidizing solution to the reducing solution in an ultrasonic state; after continuous ultrasonic treatment for a first preset time, a suspended reaction solution is obtained; and the suspended reaction solution is separated and dried to obtain the target silver powder. The preparation method of the silver powder with a hollow structure provided by the present application introduces ultrasound during the reaction process, so that the silver microcrystals are better dispersed in the reaction solution, thereby reducing or even eliminating the need to add a dispersant. The silver powder prepared in this way has good dispersibility and high sintering activity, and the presence of a hollow structure inside the silver powder can effectively improve the sintering performance of the silver powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.

[0026] Figure 1 It is a schematic flow chart of a method for preparing a silver powder with a hollow structure provided in an embodiment of the present application;

[0027] Figure 2 is a scanning electron microscope image of the silver powder prepared in Example 1 of the present application;

[0028] Figure 3 This is a scanning electron microscope image of the silver powder prepared in Example 2 of the present application;

[0029] Figure 4 This is a scanning electron microscope image of the silver powder prepared in Example 3 of the present application;

[0030] Figure 5 This is a scanning electron microscope image of the silver powder prepared in Example 4 of the present application;

[0031] Figure 6 This is a scanning electron microscope image of the silver powder prepared in Comparative Example 1 of the present application;

[0032] Figure 7 A cross-sectional view of the silver powder prepared in Example 1 of the present application;

[0033] Figure 8 A cross-sectional view of the silver powder prepared in Comparative Example 1 of the present application;

[0034] Fig. 9 This is a scanning electron microscope image of the silver powder prepared in Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0035] The present application is further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following examples are only some embodiments of the present application rather than all embodiments, and all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application.

[0036] In the following description of the present application, reference is made to “some embodiments”, which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0037] In the following description of the present application, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged with a specific order or sequence where permitted, so that the embodiments of the present application described here can be implemented in an order other than that illustrated or described here.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0039] The following is a detailed description with reference to specific embodiments. It should be noted that the serial numbers of the following embodiments are not intended to limit the preferred order of the embodiments.

[0040] The method for preparing the silver powder with a hollow structure provided in the present application also utilizes an oxidation-reduction reaction to convert silver ions into silver powder particles. However, unlike the method for preparing the silver powder with a hollow structure in the prior art, the present application improves the specific steps of the method for preparing the silver powder with a hollow structure, which is described in detail below.

[0041] See also Figure 1 , Figure 1 : is a schematic diagram of a method for preparing a silver powder with a hollow structure provided in an embodiment of the present application. The specific process of the preparation method can be as follows:

[0042] 101. Prepare oxidizing solution and reducing solution separately.

[0043] The preparation method of the silver powder with a hollow structure provided in the present application is still mainly to convert silver ions into silver powder particles through an oxidation-reduction reaction, so it is necessary to prepare an oxidizing solution including silver ions and a reducing solution for reducing the silver ions in the oxidizing solution. In some embodiments, the silver nitrate solid can be configured as a silver nitrate solution to obtain an oxidizing solution, and the reducing agent can be configured as a reducing solution. In some embodiments, the reducing agent is selected from at least one of glucose, sodium borohydride, formaldehyde, ascorbic acid, hydrazine hydrate, hydroquinone, alkanolamine or hydrogen peroxide; and the mass of the reducing agent in the present application can be 5-60% of the mass of silver nitrate. In the embodiments of the present application, the specific methods and steps for preparing the oxidizing solution and the reducing solution can refer to the prior art and are not limited here. The solution temperature of the prepared oxidizing solution and the reducing solution can be controlled within the range of 25-35°C; more specifically, the solution temperature of the oxidizing solution and the reducing solution can be controlled within the range of 25-30°C.

[0044] 102. Place the reducing liquid in an ultrasonic device, and add the oxidizing liquid into the reducing liquid in an ultrasonic state.

[0045] 103. After continuing the ultrasound for a first preset time, a suspended reaction liquid is obtained.

[0046] After the oxidizing solution and the reducing solution are prepared separately, the two need to be mixed to carry out an oxidation-reduction reaction. In an embodiment of the present application, the reducing solution can be first placed in an ultrasonic device and the ultrasonic device can be controlled to work to emit ultrasonic waves, and then the oxidizing solution is added to the reducing solution. It should be noted that in the process of adding the oxidizing solution to the reducing solution, it is necessary to control the ultrasonic device to keep working and maintain an ultrasonic state; and continue the ultrasound for the first preset time to ensure that the oxidizing solution and the reducing solution are fully mixed and reacted to obtain a suspended reaction solution. The suspended matter in the suspended reaction solution is mainly silver powder particles obtained by redox reaction.

[0047] 104. The suspended reaction liquid is separated and dried to obtain target silver powder.

[0048] Since the silver powder particles obtained through the redox reaction are suspended in the reaction liquid, the reaction liquid needs to be separated and dried to separate the suspended matter and the silver powder particles in the reaction liquid; the specific separation and drying process will be described in detail in the subsequent content and is not limited here.

[0049] The method for preparing the silver powder with a hollow structure disclosed in the present application comprises preparing an oxidizing solution and a reducing solution separately; placing the reducing solution in an ultrasonic device, and adding the oxidizing solution to the reducing solution in an ultrasonic state; after continuous ultrasonic treatment for a preset time, a suspended reaction solution is obtained; and the suspended reaction solution is separated and dried to obtain the target silver powder. The method for preparing the silver powder with a hollow structure disclosed in the present application controls the nucleation and growth processes of the silver powder to be carried out in an ultrasonic environment, without the need for stirring or adding a dispersant, and the preparation process is simple and the preparation cost is low. At the same time, the prepared silver powder has high sintering activity.

[0050] In the embodiments of the present application, after the oxidizing liquid and the reducing liquid are prepared, a pH adjusting agent needs to be added to the reducing liquid to adjust the pH value of the reducing liquid; the reducing liquid after adjusting the pH value is subsequently used for redox reaction. In some embodiments, the pH value of the reducing liquid can be adjusted to 2.2-10 to obtain a new reducing liquid after adjusting the pH, and then the new reducing liquid is added to the ultrasonic device. In other embodiments, the pH value of the reducing liquid can also be adjusted to 2-7 or 4-8, etc. The specific pH can be determined according to the actual situation and is not limited here. The pH adjusting agent in the aforementioned embodiment can be at least one of methylamine, trimethylamine, triethylamine, ammonia water, ammonium carbonate, sodium carbonate, sodium hydroxide or potassium hydroxide.

[0051] On the basis of the above embodiments, after the oxidizing liquid and the reducing liquid are prepared respectively, the reducing liquid needs to be placed in an ultrasonic device first, and the ultrasonic device is controlled to continuously emit ultrasound at a preset frequency, so that the silver ions dissolved in the reducing liquid can be evenly dispersed; then, under the premise of maintaining the ultrasonic state, the oxidizing liquid is added to the reducing liquid. In the embodiment of the present application, it is usually necessary to control the oxidizing liquid to be completely added to the reducing liquid within the second preset time to ensure the reaction speed and reaction efficiency. At the same time, during the entire process of adding the oxidizing liquid to the reducing liquid, it is necessary to control the ultrasonic device to maintain the ultrasonic state and continuously emit ultrasound, so as to ensure that the oxidizing liquid and the reducing liquid are fully mixed and carry out the redox reaction. In some embodiments, the ultrasonic frequency of the ultrasonic device can be 2-20KHZ; and the second preset time can be 1-20S, more specifically 1-10S; that is, while maintaining the ultrasonic state, the oxidizing liquid is completely added to the reducing liquid within a time of 1-10S.

[0052] The above embodiment describes the process of adding an oxidizing liquid to a reducing liquid. After the oxidizing liquid is added to the reducing liquid, the two will be fully mixed and undergo an oxidation-reduction reaction. During this process, the ultrasonic state needs to be maintained, and after the first preset ultrasonic duration, a suspended reaction liquid is obtained. Among them, the first preset duration can be determined based on the amount of oxidizing liquid and reducing liquid in the actual reaction, and is not limited here. The suspended matter in the suspended reaction liquid is the silver powder obtained through the oxidation-reduction reaction. At this time, the silver powder is dispersed in the reaction liquid, and the suspended reaction liquid needs to be further processed to obtain the final target silver powder.

[0053] In some embodiments, the target silver powder is obtained after separation and drying of the suspended reaction liquid, which may include: precipitating the suspended reaction liquid and separating the precipitate; washing the precipitate to obtain initial silver powder; drying the initial silver powder at a preset drying temperature for a third preset time to obtain the target silver powder. Specifically, it is first necessary to precipitate and separate the suspended reaction liquid to separate the precipitate, that is, the silver powder; but at this time, there are still other impurities on the precipitate, so it is necessary to wash it to obtain the initial silver powder, and the target silver powder can be obtained by drying the initial silver powder. In an embodiment of the present application, the initial silver powder can be dried at a preset drying temperature for a third preset time to obtain the target silver powder according to actual conditions. In some embodiments, the preset drying temperature can be 50-80°C, and the third preset time can be 2-6 hours.

[0054] The silver powder is prepared by the method for preparing the silver powder with a hollow structure. The preparation method is simple and does not require the addition of a dispersant, thereby reducing the preparation cost, which is conducive to industrial mass production. The silver powder prepared by the method for preparing the silver powder with a hollow structure has a hollow structure, a large specific surface area, and high sintering activity. Specifically, the silver powder particle size can reach 1-2 μm, the bulk density is 2-4 g / cm3, and the specific surface area is 0.2-0.6 m 2 / g.

[0055] The preparation process of the method for preparing the silver powder with a hollow structure provided by the present application is described in detail below in conjunction with specific embodiments:

[0056] Embodiment 1:

[0057] Weigh 1.6 kg of silver nitrate solid and prepare it into a silver nitrate solution with a mass fraction of 8%; weigh 0.86 kg of ascorbic acid as a reducing agent and prepare it into a reducing agent solution with a mass concentration of 4.6%, and add 200 g of trimethylamine as a pH adjuster to the reducing solution to obtain a reducing agent solution after adjusting the pH. Keep the temperature of the reaction solution (including the silver nitrate solution and the reducing agent solution after adjusting the pH) at 25°C, place the reducing solution in an ultrasonic device and adjust the ultrasonic frequency to 5KHz, and quickly pour the reducing solution into the oxidizing solution for 2s. Maintain the ultrasonic state so that the silver nitrate solution and the reducing agent solution fully react to obtain a suspended reaction solution. Then let the suspended reaction solution stand and obtain a sediment, and then wash the sediment with deionized water and ethanol to obtain the initial silver powder; dry the initial silver powder at 60°C for 30 minutes, and pass the dried product through a 500-mesh sieve to finally obtain the target silver powder. Figure 2 The figure shows the SEM image of the silver powder prepared in Example 1. The actual particle size D50 of the silver powder obtained in Example 1 is 1.4 μm, and the specific surface area is 0.40 m 2 / g.

[0058] Embodiment 2:

[0059] Weigh 1.6kg of silver nitrate solid and prepare it into a silver nitrate solution with a mass fraction of 8%; weigh 0.86kg of ascorbic acid as a reducing agent and prepare it into a reducing agent solution with a mass concentration of 4.6%, and add 200g of trimethylamine as a pH adjuster to the reducing solution to obtain a reducing agent solution after adjusting the pH; at the same time, add 200g of polyvinyl pyrrolidone to the reducing agent solution as a dispersant. Keep the temperature of the reaction solution (including the silver nitrate solution and the reducing agent solution after adjusting the pH) at 25°C, place the reducing solution in an ultrasonic device and adjust the ultrasonic frequency to 5KHz, and quickly pour the reducing solution into the oxidizing solution for 2s. Maintain the ultrasonic state so that the silver nitrate solution and the reducing agent solution fully react to obtain a suspended reaction solution. Then let the suspended reaction solution stand and obtain a sediment, and then wash the sediment with deionized water and ethanol to obtain the initial silver powder; dry the initial silver powder at 60°C for 30min, and pass the dried product through a 500-mesh sieve to finally obtain the target silver powder. Figure 3 The figure shows the SEM image of the silver powder prepared in Example 2. The actual particle size D50 of the silver powder obtained in Example 2 is 1.38 μm, and the specific surface area is 0.41 m 2 / g.

[0060] Different from Example 1, a small amount of dispersant is added in Example 2 to further improve the reaction process of the redox reaction. That is, the preparation method of the silver powder with a hollow structure provided in the embodiment of the present application can reduce the amount of dispersant used or even completely eliminate the use of dispersant, thereby effectively reducing costs.

[0061] Embodiment 3:

[0062] Weigh 1.6kg of silver nitrate solid and prepare it into a silver nitrate solution with a mass fraction of 8%; weigh 0.86kg of ascorbic acid as a reducing agent and prepare it into a reducing agent solution with a mass concentration of 4.6%, and add 200g of trimethylamine as a pH adjuster to the reducing solution to obtain a reducing agent solution after adjusting the pH; at the same time, add 200g of gum arabic to the reducing agent solution as a dispersant. Keep the temperature of the reaction solution (including the silver nitrate solution and the reducing agent solution after adjusting the pH) at 25°C, place the reducing solution in an ultrasonic device and adjust the ultrasonic frequency to 5KHz, and quickly pour the reducing solution into the oxidizing solution for 2s. Maintain the ultrasonic state so that the silver nitrate solution and the reducing agent solution fully react to obtain a suspended reaction solution. Then let the suspended reaction solution stand and obtain a sediment, and then wash the sediment with deionized water and ethanol to obtain the initial silver powder; dry the initial silver powder at 60°C for 30min, and pass the dried product through a 500-mesh sieve to finally obtain the target silver powder. Figure 4 The figure shows the SEM image of the silver powder prepared in Example 3. The actual particle size D50 of the silver powder obtained in Example 3 is 1.35 μm, and the specific surface area is 0.35 m 2 / g.

[0063] Embodiment 4:

[0064] Weigh 1.6 kg of silver nitrate solid and prepare it into a silver nitrate solution with a mass fraction of 8%; weigh 0.86 kg of ascorbic acid as a reducing agent and prepare it into a reducing agent solution with a mass concentration of 4.6%, and add 400 g of trimethylamine as a pH adjuster to the reducing solution to obtain a reducing agent solution after adjusting the pH. Keep the temperature of the reaction solution (including the silver nitrate solution and the reducing agent solution after adjusting the pH) at 25°C, place the reducing solution in an ultrasonic device and adjust the ultrasonic frequency to 5KHz, and quickly pour the reducing solution into the oxidizing solution for 2s. Maintain the ultrasonic state so that the silver nitrate solution and the reducing agent solution fully react to obtain a suspended reaction solution. Then let the suspended reaction solution stand and obtain a sediment, and then wash the sediment with deionized water and ethanol to obtain the initial silver powder; dry the initial silver powder at 60°C for 30 minutes, and pass the dried product through a 500-mesh sieve to finally obtain the target silver powder. Figure 5 The figure shows the SEM image of the silver powder prepared in Example 4. The actual particle size D50 of the silver powder obtained in Example 4 is 1.32 μm, and the specific surface area is 0.43 m 2 / g.

[0065] It can be seen from the above-mentioned Examples 1-4 that silver powders with different particle sizes and surface areas can be obtained by adjusting the amount of the dispersant and the amount of the pH adjuster.

[0066] The present application also provides two comparative examples to verify the advantages of the method for preparing the silver powder with a hollow structure provided by the present application. The specific examples are as follows:

[0067] The difference between Comparative Example 1 and Example 1 is that ultrasound is not turned on, and the oxidizing solution and the reducing solution are not mixed under ultrasound. Specifically, 1.6 kg of silver nitrate solid is weighed and prepared into a silver nitrate solution with a mass fraction of 8%; 0.86 kg of ascorbic acid is weighed as a reducing agent and prepared into a reducing agent solution with a mass concentration of 4.6%, and 200 g of trimethylamine is added to the reducing solution as a pH adjuster to obtain a reducing agent solution after adjusting the pH. The temperature of the reaction solution (including the silver nitrate solution and the reducing agent solution after adjusting the pH) is maintained at 25°C, and the reducing solution is quickly poured into the oxidizing solution, and the pouring time is 2s. The ultrasonic state is maintained to allow the silver nitrate solution and the reducing agent solution to fully react to obtain a suspended reaction solution. The suspended reaction solution is then allowed to stand and a sediment is obtained, and the sediment is then washed with deionized water and ethanol to obtain the initial silver powder; the initial silver powder is dried at 60°C for 30 minutes, and the dried product is sieved through a 500-mesh sieve to finally obtain the target silver powder. Figure 6 The figure shows the SEM image of the silver powder prepared in Comparative Example 1. The actual particle size D50 of the silver powder obtained in Comparative Example 1 is 1.6 μm, and the specific surface area is 0.3 m2 The specific surface area of ​​the silver powder in Comparative Example 1 is smaller than that of the silver powder in Example 1. The specific surface area of ​​the silver powder can be effectively increased by introducing ultrasound during the reaction process.

[0068] like Figure 7 Shown is a cross-sectional view of the silver powder prepared in Example 1 of the present application; Figure 8 This is a cross-sectional view of the silver powder prepared in Comparative Example 1 of this application. Figure 7 Figure 8 It can be seen that there are a large number of holes in the silver powder obtained by introducing ultrasound in Example 1 of the present application, that is, the silver powder has a hollow structure; while in Comparative Example 1, no ultrasound is introduced and no dispersant is added, and there are no large number of holes in the obtained silver powder. Since the silver powder with a hollow structure has a special spatial structure, it is beneficial to reduce the amount of silver in the electronic paste, improve the rheological properties of the paste, and also have better sintering performance; therefore, the present application can effectively improve the sintering performance of the silver powder by introducing ultrasound during the reaction process.

[0069] The difference between Comparative Example 2 and Example 1 is that no pH adjuster is added. Specifically as follows: weigh 1.6 kg of silver nitrate solid and prepare a silver nitrate solution with a mass fraction of 8%; weigh 0.86 kg of ascorbic acid as a reducing agent and prepare a reducing agent solution with a mass concentration of 4.6%. Keep the temperature of the reaction solution (including the silver nitrate solution and the reducing agent solution) at 25°C, and quickly pour the reducing solution into the oxidizing solution for 2 seconds. Maintain the ultrasonic state to allow the silver nitrate solution and the reducing agent solution to fully react to obtain a suspended reaction solution. The suspended reaction solution is then allowed to stand and a sediment is obtained, which is then washed with deionized water and ethanol to obtain an initial silver powder; the initial silver powder is dried at 60°C for 30 minutes, and the dried product is sieved through a 500-mesh sieve to finally obtain the target silver powder. Fig. 9 The figure shows the SEM image of the silver powder prepared in Comparative Example 2. The actual particle size D50 of the silver powder obtained in Comparative Example 2 is 1.52 μm, and the specific surface area is 0.48 m 2 / g. Although the specific surface area of ​​the silver powder in comparative example 2 is greater than that in example 1, the particle size of the silver powder obtained in comparative example 2 is greater than that in example 1; however, a larger particle size will reduce the performance of the silver powder, so the silver powder in comparative example 2 is not the best silver powder. In the present application, the pH value of the reaction solution is adjusted and ultrasound is introduced during the reaction process, so that a large number of pores can be present in the silver powder while ensuring a reasonable particle size of the silver powder, thereby increasing the specific surface area of ​​the silver powder.

[0070] It can be seen that the present application discloses a simple method for preparing silver powder with a hollow structure, by mixing an oxidizing liquid and a reducing liquid under an ultrasonic state, and controlling the two to undergo an oxidation-reduction reaction under an ultrasonic state, without adding a dispersant, and the cost is low and the preparation is simple; the prepared silver powder has a hollow structure, a large specific surface area, and high sintering activity, and has broad application prospects in the field of photovoltaic silver paste.

[0071] The present application also provides a silver powder, which is prepared by adopting the preparation method of the silver powder with a hollow structure provided by any of the above embodiments, and thus has all the same beneficial effects, and this embodiment will not be described in detail here.

[0072] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0073] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a silver powder having a hollow structure, characterized in that: include: preparing an oxidizing solution and a reducing solution respectively; placing the reducing liquid in an ultrasonic device, and adding the oxidizing liquid into the reducing liquid in an ultrasonic state; After the ultrasonic wave is continuously applied for a first preset time, a suspended reaction liquid is obtained; The suspended reaction liquid is separated and dried to obtain the target silver powder.

2. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: After preparing the oxidizing solution and the reducing solution respectively, the method further comprises: A pH regulator is added to the reducing solution to adjust the pH of the reducing solution to 2.2-10, thereby obtaining a new reducing solution with adjusted pH.

3. The method for preparing the silver powder with a hollow structure according to claim 2, characterized in that: The pH regulator is at least one of methylamine, trimethylamine, triethylamine, ammonia water, ammonium carbonate, sodium carbonate, sodium hydroxide or potassium hydroxide.

4. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: The solution temperature of the oxidizing solution and the reducing solution is 25-35°C.

5. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: The step of placing the reducing liquid in an ultrasonic device and adding the oxidizing liquid to the reducing liquid in an ultrasonic state comprises: placing the reducing liquid in an ultrasonic device, and controlling the ultrasonic device to emit ultrasound at a preset frequency; The oxidizing liquid is added into the reducing liquid under ultrasonic state and within a second preset time period.

6. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: The ultrasonic frequency of the ultrasonic device is 2-20KHZ.

7. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: The method of separating and drying the suspended reaction liquid to obtain the target silver powder comprises: Precipitating the suspended reaction liquid and separating the precipitate; washing the precipitate to obtain initial silver powder; The initial silver powder is dried at a preset drying temperature for a third preset time to obtain the target silver powder.

8. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: The prepared silver powder has a hollow structure.

9. The method for preparing the silver powder with a hollow structure according to claim 1, characterized in that: The silver powder prepared has a particle size of 1-2 μm, a bulk density of 2-4 g / cm3, and a specific surface area of ​​0.2-0.6 m 2 / g.

10. A silver powder, characterized in that: The silver powder is prepared by the method for preparing a silver powder with a hollow structure as described in any one of claims 1 to 9, wherein the silver powder has a hollow structure.