Molybdenum-rhenium alloy and niobium-zirconium alloy connecting method and connector
By using PdNi foil as an intermediate layer in a vacuum brazing furnace, the Nb element diffusion of Ni element and niobium zirconium alloy is used to form eutectic structure, which solves the problem of difficulty in connecting molybdenum rhenium alloy and niobium zirconium alloy, and achieves high performance and reduces oxide content and cost.
Patent Information
- Application Number
- CN202411196096.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art lacks an effective connection method to connect molybdenum rhenium alloys with niobium zirconium alloys, and the traditional melt welding method causes the joints to generate a large amount of oxygen-containing compounds at high temperatures, affecting performance.
Using PdNi foil as the intermediate layer, brazing is performed in a vacuum brazing furnace at a temperature of 1200°C to 1300°C. The Ni element and the Nb element in the niobium zirconium alloy are diffused to form an eutectic liquid phase to control the distribution of the brittle phase , forming eutectic structures of NiNb and (Pd,Ni)2Nb to achieve metallurgical bonding between molybdenum rhenium alloy and niobium zirconium alloy.
The obtained joints have a high room temperature average tensile strength and good mechanical properties, and the generated joints contain less oxygen compounds and are low in cost, avoiding damage to the performance of the base material at high temperatures.
Smart Images

Figure CN119035683A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of brazing technology, and in particular to a connection method and joint of a molybdenum-rhenium alloy and a niobium-zirconium alloy. Background Art
[0002] Molybdenum-rhenium alloy (Mo5Re) is used as a structural material in the nuclear field because of its excellent high-temperature mechanical properties such as high strength and toughness, excellent fatigue resistance, creep resistance, good radiation resistance, compatibility with nuclear fuel and alkali metal coolants, neutron characteristics and other nuclear physical properties, good thermal conductivity, corrosion resistance and biocompatibility.
[0003] The zirconium added to niobium-zirconium alloy (Nb1Zr) can refine the grains and significantly improve the room temperature strength without reducing the plasticity of niobium. At the same time, due to the strong affinity between zirconium and oxygen, it can protect the niobium matrix. The zirconium element in niobium has both precipitation strengthening and solid solution strengthening effects. Niobium-zirconium alloy has excellent high-temperature mechanical properties, oxidation resistance and corrosion resistance, and is also widely used.
[0004] Since both molybdenum-rhenium alloy and niobium-zirconium alloy are refractory alloys, there is currently no suitable connection method to connect molybdenum-rhenium alloy and niobium-zirconium alloy together. Summary of the invention
[0005] In view of the above, it is necessary to propose a connection method and joint of molybdenum-rhenium alloy and niobium-zirconium alloy, and the obtained joint has better mechanical properties.
[0006] The embodiment of the present application provides a method for connecting a molybdenum-rhenium alloy and a niobium-zirconium alloy, comprising the following steps:
[0007] Grinding of niobium-zirconium alloy and molybdenum-rhenium alloy to be welded;
[0008] Cleaning the PdNi foil and the polished niobium-zirconium alloy and the molybdenum-rhenium alloy;
[0009] Placing the molybdenum-rhenium alloy, the PdNi foil and the niobium-zirconium alloy in order from top to bottom to obtain a welded part, and applying a preset pressure to a side of the molybdenum-rhenium alloy away from the PdNi foil;
[0010] The workpiece to be welded is placed in a vacuum brazing furnace, and the vacuum degree in the vacuum brazing furnace reaches 2×10 ~3 Pa~5.0×10 ~3 Pa, turn on the heating, and keep the brazing temperature at 1200℃~1300℃ for 1min~30min to obtain the joint.
[0011] In some possible embodiments, the molybdenum-rhenium alloy includes Mo5Re, and the niobium-zirconium alloy includes Nb1Zr.
[0012] In some possible embodiments, the step of grinding the niobium-zirconium alloy and the molybdenum-rhenium alloy to be welded includes:
[0013] The parts to be welded of the molybdenum-rhenium alloy and the niobium-zirconium alloy are polished with SiC sandpapers of 400 mesh, 800 mesh, 1200 mesh and 2000 mesh in sequence.
[0014] In some possible embodiments, the mass fraction of the Pd element in the PdNi foil is 55%-65%, and the mass fraction of the Ni element is 35%-45%.
[0015] In some possible embodiments, the step of cleaning the PdNi foil and the polished niobium-zirconium alloy and the molybdenum-rhenium alloy comprises:
[0016] The PdNi foil and the polished niobium-zirconium alloy and the molybdenum-rhenium alloy are immersed in acetone, ultrasonically cleaned for 10 to 30 minutes and then dried, and then placed in an ethanol solution for ultrasonic cleaning for 10 to 20 minutes and then dried.
[0017] In some possible embodiments, the PdNi foil has a thickness of 50 μm to 150 μm.
[0018] In some possible embodiments, the brazing heating rate is 5° C. / min to 20° C. / min.
[0019] In some possible embodiments, the step of keeping the temperature at 1200° C. to 1300° C. for 1 to 30 minutes further includes:
[0020] The welded parts are cooled to room temperature after being kept warm.
[0021] In some possible embodiments, the cooling rate of the workpiece to be welded is 5° C. / min to 10° C. / min.
[0022] A second aspect of an embodiment of the present application provides a connector, which is prepared by the connection method described in any one of the above items.
[0023] The connection method and joint of the molybdenum-rhenium alloy and the niobium-zirconium alloy are characterized by using PdNi foil as the intermediate layer of brazing. During the process of heating to 1200°C to 1300°C, the Ni element in the PdNi foil and the Nb element in the niobium-zirconium alloy parent material diffuse with each other to form a eutectic liquid phase, thereby realizing the metallurgical bonding of the molybdenum-rhenium alloy and the niobium-zirconium alloy at a brazing temperature below 1240°C. In this process, the parent material niobium-zirconium alloy will dissolve into the brazing seam, and the growth and aggregation of the brittle phase can be controlled by controlling the vacuum degree and the brazing temperature. However, when the brazing temperature is lower than 1200°C, the dissolution of niobium in the niobium-zirconium alloy is limited, and a dense and defect-free joint cannot be obtained. When the brazing temperature is higher than 1300°C, the molybdenum-rhenium alloy and the niobium-zirconium alloy parent materials on both sides will dissolve into the brazing seam in large quantities, and a higher brazing temperature means a longer high temperature residence time, which is not conducive to the performance of the molybdenum-rhenium alloy and the niobium-zirconium alloy parent materials themselves. After cooling, a eutectic structure of NiNb and (Pd, Ni)2Nb is formed in the interface and evenly distributed in the weld, so that the joint has good performance. Therefore, the connection method of the present application is simple, the cost is low, the resulting joint contains less oxygen compounds, the obtained molybdenum-rhenium alloy / PdNi / niobium-zirconium alloy joint has a high room temperature average tensile strength, and the mechanical properties of the joint are better. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A flow chart of a method for connecting a molybdenum-rhenium alloy and a niobium-zirconium alloy provided in an embodiment of the present application.
[0025] Figure 2 yes Figure 1 Schematic diagram of the structure of the workpiece to be welded as described in .
[0026] Figure 3 This is a backscattered photograph of the joint obtained in this application. DETAILED DESCRIPTION
[0027] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0028] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the various specific processes and material examples provided by the present application, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.
[0029] The embodiments of the present application are further described below in conjunction with the accompanying drawings.
[0030] At present, rhenium is a rare metal with high price. The overall production and processing cost of molybdenum-rhenium alloy is high. In addition, due to the presence of many impurities in the molybdenum-rhenium alloy base material, a large number of pores will inevitably appear in the joints when using fusion welding. Both molybdenum-rhenium alloy and niobium-zirconium alloy are refractory alloys. The traditional fusion welding method requires a high welding temperature to melt the base material. At high temperatures, it has a greater affinity with oxygen, and the joints generate more oxygen-containing compounds, which is not good for the joint performance. In addition, considering the problem of reducing damage to the base material itself, brazing is more suitable. Brazing is a connection method in which the brazing filler metal melts the base material but does not melt it. The process is simple and easy to implement. Selecting a suitable brazing filler metal can achieve reliable connection between alloys at a lower temperature, and vacuum brazing can avoid problems such as oxygen embrittlement of molybdenum-rhenium alloy and niobium-zirconium alloy at high temperatures.
[0031] To do this, see Figure 1 The present application embodiment provides a method for connecting a molybdenum-rhenium alloy and a niobium-zirconium alloy, comprising the following steps:
[0032] S10, grinding of niobium-zirconium alloy and molybdenum-rhenium alloy to be welded.
[0033] Among them, the molybdenum-rhenium alloy includes Mo5Re. The mass fraction of rhenium element is between 4.5% and 5.2%, and the content of other impurities is less than 0.0001%. The molybdenum-rhenium alloy with this composition reduces the ductile-brittle transition temperature of molybdenum, can improve the plastic toughness and processing performance of the matrix, and can improve the weldability of the material to a certain extent. The niobium-zirconium alloy includes Nb1Zr, in which the mass fraction of zirconium element is between 0.8% and 1.2%, and the content of other impurities is less than 0.0005%. The niobium-zirconium alloy with this composition has excellent oxidation resistance and toughness.
[0034] It is understood that the niobium-zirconium alloy and the molybdenum-rhenium alloy may have other compositions, but are not limited thereto.
[0035] Among them, the mass fraction of Pd element in PdNi foil is 55%-65%, and the mass fraction of Ni element is 35%-45%. Preferably, the mass fraction of Pd element in PdNi foil is 60%, and the mass fraction of Ni element is 40%. According to the Pd-Ni binary phase diagram, Pd and Ni are infinitely miscible. The lowest melting point of the Pd-Ni binary system is about 1240°C when the Pd content is about 60wt.% and the Ni content is 40wt.%, and the solid-liquid phase temperature range is the narrowest. Using this composition of PdNi solder for brazing can, to a certain extent, avoid the damage to the performance of the base material itself caused by keeping the base material at high temperature for too long.
[0036] The step of grinding the niobium-zirconium alloy and the molybdenum-rhenium alloy to be welded includes:
[0037] The parts to be welded of the molybdenum-rhenium alloy and the niobium-zirconium alloy were polished with SiC sandpapers of 400 mesh, 800 mesh, 1200 mesh and 2000 mesh in turn.
[0038] S20, cleaning the PdNi foil and the polished niobium-zirconium alloy and molybdenum-rhenium alloy.
[0039] The steps of cleaning the PdNi foil and the polished niobium-zirconium alloy and molybdenum-rhenium alloy include:
[0040] The PdNi foil and the polished niobium-zirconium alloy and molybdenum-rhenium alloy are immersed in acetone, ultrasonically cleaned for 10 to 30 minutes and then dried, and then placed in an ethanol solution for ultrasonic cleaning for 10 to 20 minutes and then dried.
[0041] S30, placing the molybdenum-rhenium alloy, the PdNi foil and the niobium-zirconium alloy in order from top to bottom to obtain the welded parts, such as Figure 2 As shown, a preset pressure is applied to the side of the molybdenum-rhenium alloy facing away from the PdNi foil.
[0042] Wherein, the thickness of the PdNi foil is 50 μm to 150 μm.
[0043] S40, place the parts to be welded in a vacuum brazing furnace, and the vacuum degree in the vacuum brazing furnace reaches 2×10 ~3 Pa~5.0×10 ~3 Pa, turn on the heating, and keep the brazing temperature at 1200℃~1300℃ for 1min~30min to obtain the joint.
[0044] Among them, the brazing heating rate is 5℃ / min~20℃ / min.
[0045] In some possible embodiments, the steps after the brazing temperature is 1200° C. to 1300° C. and the temperature is kept at 1 min to 30 min further include:
[0046] Cool the welded parts to room temperature after heat preservation.
[0047] Among them, the cooling rate of the welded parts is 5°C / min to 10°C / min.
[0048] A second aspect of an embodiment of the present application provides a connector, which is prepared by any of the connection methods described above.
[0049] The above-mentioned connection method and joint of molybdenum-rhenium alloy and niobium-zirconium alloy, by using PdNi foil as the intermediate layer of brazing, during the process of heating to 1200℃~1300℃, please refer to Figure 3 , the Ni element in the PdNi foil and the Nb element in the niobium-zirconium alloy base material diffuse with each other to form a eutectic liquid phase, and then the metallurgical bonding of the molybdenum-rhenium alloy and the niobium-zirconium alloy can be achieved at a brazing temperature below 1240°C. In this process, the base material niobium-zirconium alloy will dissolve into the brazing seam, and the growth and aggregation of the brittle phase can be controlled by controlling the vacuum degree and the brazing temperature. After cooling, a eutectic structure of NiNb and (Pd, Ni)2Nb is formed at the interface, which is evenly distributed in the weld, making the joint performance good. Therefore, the connection method of the present application is simple and low in cost, the resulting joint contains less oxygen compounds, the obtained molybdenum-rhenium alloy / PdNi / niobium-zirconium alloy joint has a higher room temperature average tensile strength, and the mechanical properties of the joint are better.
[0050] The technical solution of the present application is not limited to the specific implementation modes given below, but also includes any combination of the specific implementation modes.
[0051] Example 1
[0052] This embodiment provides a method for connecting a molybdenum-rhenium alloy and a niobium-zirconium alloy, comprising the following steps:
[0053] Step 1: Grind the parts to be welded of the molybdenum-rhenium alloy and the niobium-zirconium alloy with SiC sandpapers of 400 mesh, 800 mesh, 1200 mesh and 2000 mesh in sequence.
[0054] Step 2: immerse a PdNi foil with a thickness of 75 μm and a Pd mass fraction of 60% in acetone, ultrasonically clean it for 10 minutes, and then dry it. Then, put it in an ethanol solution, ultrasonically clean it for 10 minutes, and then blow it dry with a hair dryer or dry it.
[0055] Step 3: Place the molybdenum-rhenium alloy, PdNi foil and niobium-zirconium alloy in order from top to bottom to obtain the welded parts, and apply a pressure of 0.5×10 3 The Pa graphite block is pressed onto the side of the molybdenum-rhenium alloy facing away from the PdNi foil.
[0056] Step 4: Place the workpiece to be welded in a vacuum brazing furnace and place it in a vacuum furnace at a degree of 5.0×10 ~3The joint was obtained by heating to 1220°C in a Pa environment at a heating rate of 15°C / min and keeping the temperature for 10 minutes. After brazing, the joint was cooled to room temperature at a cooling rate of 5°C / min to obtain a joint. The average tensile strength of the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment was 135 MPa at room temperature.
[0057] Example 2
[0058] The difference between this embodiment and embodiment 1 is that the rhenium content in the molybdenum-rhenium alloy matrix used in step 1 is different. The other steps are the same as those in the specific embodiment. The average room temperature tensile strength of the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment is 120 MPa.
[0059] Example 3
[0060] The difference between this embodiment and embodiment 1 is that the thickness of the PdNi foil in step 2 is 150 μm. The other steps are the same as those in the specific embodiment. The average tensile strength of the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment is 68 MPa at room temperature.
[0061] Embodiment 4:
[0062] The difference between this embodiment and embodiment 1 is that in step 2, the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment has an average room temperature tensile strength of 128 MPa after ultrasonic cleaning in acetone solution for 30 minutes and drying, and then ultrasonic cleaning in ethanol solution for 10 minutes and drying with a hair dryer.
[0063] Embodiment 5:
[0064] The difference between this embodiment and embodiment 1 is that in step 3, the pressure applied to the assembly to be welded is 2.5×10 3 Pa graphite block, other steps are the same as those in specific embodiment 1. The average tensile strength of the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment is 114 MPa at room temperature.
[0065] Embodiment 6:
[0066] The difference between this embodiment and embodiment 1 is that in step 4, the brazing process heating rate is 10°C / min, the brazing temperature is 1260°C, the holding time is 1min, and the other steps are the same as those in embodiment 1. The room temperature average tensile strength of the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment is 48MPa.
[0067] Embodiment 7:
[0068] The difference between this embodiment and embodiment 1 is that in step 4, the brazing process parameters are a heating rate of 20°C / min, a brazing temperature of 1220°C, and a holding time of 30min. The average room temperature tensile strength of the molybdenum-rhenium / PdNi / niobium-zirconium joint obtained in this embodiment is 96MPa.
[0069] From the above content, it can be seen that the connection method of the present invention is simple, and the obtained molybdenum-rhenium / PdNi / niobium-zirconium alloy joint has a high room temperature average tensile strength, the optimal room temperature average tensile strength can reach 135 MPa, and the mechanical properties are better.
[0070] It is obvious to those skilled in the art that the present application is not limited to the details of the exemplary embodiments described above, and that the present application can be implemented in other specific forms without departing from the spirit or essential features of the present application. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present application is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present application.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the preferred embodiments, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.
Claims
1. A method for connecting a molybdenum-rhenium alloy and a niobium-zirconium alloy, characterized in that: The steps include: Grinding of niobium-zirconium alloy and molybdenum-rhenium alloy to be welded; Cleaning the PdNi foil and the polished niobium-zirconium alloy and the molybdenum-rhenium alloy; Placing the molybdenum-rhenium alloy, the PdNi foil and the niobium-zirconium alloy in order from top to bottom to obtain a welded part, and applying a preset pressure to a side of the molybdenum-rhenium alloy away from the PdNi foil; The workpiece to be welded is placed in a vacuum brazing furnace, and the vacuum degree in the vacuum brazing furnace reaches 2×10 ~3 Pa~5.0×10 ~3 Pa, turn on the heating, and keep the brazing temperature at 1200℃~1300℃ for 1min~30min to obtain the joint.
2. The connection method according to claim 1, characterized in that: The molybdenum-rhenium alloy includes Mo5Re, and the niobium-zirconium alloy includes Nb1Zr.
3. The connection method according to claim 1, characterized in that: The step of grinding the niobium-zirconium alloy and the molybdenum-rhenium alloy to be welded comprises: The parts to be welded of the molybdenum-rhenium alloy and the niobium-zirconium alloy are polished with SiC sandpapers of 400 mesh, 800 mesh, 1200 mesh and 2000 mesh in sequence.
4. The connection method according to claim 1, characterized in that: The mass fraction of the Pd element in the PdNi foil is 55%-65%, and the mass fraction of the Ni element is 35%-45%.
5. The connection method according to claim 1, characterized in that: The steps of cleaning the PdNi foil and polishing the niobium-zirconium alloy and the molybdenum-rhenium alloy include: The PdNi foil and the polished niobium-zirconium alloy and the molybdenum-rhenium alloy are immersed in acetone, ultrasonically cleaned for 10 to 30 minutes and then dried, and then placed in an ethanol solution for ultrasonic cleaning for 10 to 20 minutes and then dried.
6. The connection method according to claim 1, characterized in that: The thickness of the PdNi foil is 50 μm to 150 μm.
7. The connection method according to claim 1, characterized in that: The brazing heating rate is 5°C / min to 20°C / min.
8. The connection method according to claim 1, characterized in that: The step of keeping the temperature at 1200° C. to 1300° C. for 1 to 30 minutes further comprises: The welded parts are cooled to room temperature after being kept warm.
9. The connection method according to claim 8, characterized in that: The cooling rate of the workpiece to be welded is 5°C / min to 10°C / min.
10. A joint, characterized in that: The method is prepared by the connection method described in any one of claims 1 to 9.
Citation Information
Cited By
Manual helium arc welding method for niobium-zirconium alloy welding seam
CN121847892A