Method and equipment for laser cutting of semiconductor material
Through laser invisible cutting technology, semiconductor materials are heated and modified layers are formed, combining temperature difference and external force fracture, which solves the problems of edge collapse and surface damage in traditional cutting methods, and achieves high-efficiency and low-cost high-quality cutting.
Patent Information
- Application Number
- CN202411352801.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-16
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing semiconductor material cutting technology has problems of edge collapse, layering and surface damage, and traditional laser cutting methods are difficult to control in heat-affected areas and have high equipment costs, making it difficult to achieve efficient and low-cost high-quality cutting.
The laser invisible cutting method is used to heat the semiconductor material and form a modified layer inside the material. The temperature difference and external force assist the fracture, combined with a three-dimensional displacement platform, laser and cooling device, to ensure cutting accuracy and efficiency.
It significantly improves the cutting quality and efficiency, avoids edge collapse and surface damage, reduces production costs, and achieves high-quality and efficient semiconductor material cutting.
Smart Images

Figure CN119035801A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor material processing, and more specifically, to a method and device for laser cutting semiconductor materials. Background Art
[0002] Third-generation semiconductor materials such as silicon carbide (SiC), due to their unique physical and chemical properties, have shown irreplaceable advantages in the application fields of high frequency, high voltage, high power, optoelectronics, radiation resistance and microwave electronic devices, especially in aerospace, nuclear energy and other fields under extreme environments. SiC has excellent properties such as wide band gap, high breakdown voltage, high thermal conductivity, high chemical inertness and high temperature resistance, which make SiC a key material in modern high-tech industries. In the manufacturing process of semiconductor material wafers, wafer cutting is one of the key links in the production of semiconductor power devices. The cutting method and cutting quality directly affect the roughness, size and production cost of the wafer, which in turn has a significant impact on the performance and cost of the final power device.
[0003] In the early days, the more mature method for cutting SiC was the wire saw process of diamond wire cutting. However, this cutting method has obvious defects, such as contact cutting, which is prone to edge collapse, delamination and heating; slow slicing speed and high cutting cost; large gap width and serious cutting loss of about 50%; and the surface is prone to damage and wire marks after cutting, which requires expensive subsequent processes (such as grinding, mechanical polishing and chemical polishing) to repair, greatly increasing production costs.
[0004] With the development of non-contact laser processing technology and mechanical automation technology, a variety of laser cutting technologies have emerged, including laser ablation cutting, laser thermal cracking cutting, water-conducting laser cutting and laser hidden cutting. Laser ablation cutting is to focus a high-energy laser beam on the surface of the sample, causing the material in the processing area to melt or form a high-temperature and high-pressure plasma to separate from the sample, and to form a slit that penetrates the upper and lower surfaces of the sample by controlling the focus to move up and down to achieve the purpose of cutting. However, a large heat-affected zone is generated during the sample processing process, which seriously affects the processing accuracy, and slag is easily left on the surface around the slit, reducing the surface quality; laser thermal cracking cutting is to irradiate the sample surface with a laser beam, generate local high temperature, change the internal stress of the sample and produce micro-thermal cracks, and further control the movement trajectory of the laser, so that the thermal cracks expand according to the predetermined shape, and finally achieve the cutting of the sample. Although this method has the characteristics of a small heat-affected zone and high cutting accuracy, the expansion direction of the thermal cracks is difficult to control during the processing, and often deviates from the laser processing trajectory, resulting in serious edge collapse.
[0005] Water-guided laser cutting is achieved by coupling the laser beam into a water jet and then acting on the sample surface. Since water has a certain cooling effect and impact force, water-guided laser reduces thermal damage to the material when processing the sample, improves the uniformity of the cutting edge, and can protect the optical device from thermal damage under the cooling effect of water. The impact force can even effectively clean the detached material filler in the cutting area, avoiding the impact of the detached material generated during cutting on the cutting surface. Although water-guided laser cutting has more advantages than traditional laser cutting, it is difficult to couple the laser beam with the water beam, and requires high precision in the design of the water jet nozzle, resulting in high equipment preparation costs for water-guided laser cutting, and high equipment maintenance costs, requiring a certain amount of capital investment.
[0006] Laser invisible cutting is a cutting technology that does not damage the upper and lower surfaces of the sample. The working principle is to focus the laser beam inside the sample. Under the high temperature of the laser, a photochemical reaction occurs inside the sample to form a modified layer, and microcracks are formed in the longitudinal direction of the modified layer. Then, with the help of external force, the modified layer is accurately separated along the laser scanning path, which solves the problems of thermal damage to the material, wide cutting seams, surface contamination, etc. during the cutting process. However, in the subsequent splitting process, the upper and lower surfaces of the sample are often not cut, which makes splitting difficult. Summary of the invention
[0007] In order to solve the above problems, the present application provides a method and device for laser cutting semiconductor materials, which are applicable to materials such as silicon (Si), silicon oxide SiO2, silicon nitride (Si3N4), gallium arsenide, germanium, gallium arsenide phosphide and silicon carbide.
[0008] The present application provides a method for laser cutting semiconductor materials, which adopts the following technical solution: A method for laser cutting semiconductor materials comprises heating the semiconductor material as a whole to improve the machinability of the material; then, using laser to perform invisible cutting on the inside of the semiconductor material, forming a modified layer inside the material by focusing the laser without damaging the surface of the material; after the cutting is completed, stopping the heating and cooling the surface corresponding to the modified layer, using the thermal stress generated by the temperature difference to assist the fracture; finally, applying external force at the modified layer to make the semiconductor material break precisely along the modified layer to form independent grains.
[0009] Through the above technical solutions, the problems of edge collapse, delamination and surface damage in traditional cutting methods are effectively avoided, and the cutting quality and efficiency are significantly improved.
[0010] Furthermore, the present application limits the heating temperature to 50-70°C.
[0011] This temperature range can ensure that the material will not be damaged due to excessive temperature during the heating process, and can effectively improve the material's machinability, creating favorable conditions for subsequent laser cutting.
[0012] Further, the laser wavelength when the laser performs invisible cutting inside the semiconductor material is 1064nm or 1030nm; and / or, the laser pulse duration is 270fs-150ps; and / or, the laser frequency is 50kHz-20MHz; and / or, the maximum power of the laser is 5W-120W; and / or, the maximum pulse energy of the laser is 50μJ-190μJ; and / or, the beam quality of the laser is M 2 <2.
[0013] The precise control of these parameters ensures the energy stability and processing accuracy during the laser cutting process, thus achieving high-quality and efficient invisible cutting.
[0014] Furthermore, by ensuring that the laser focus is located inside the semiconductor material and not less than 10 μm from the surface.
[0015] Through the above technical solution, there are no cracks on the surface of the semiconductor material, so it is not easy to undergo oxidation reactions with oxygen, water vapor, etc. under high temperature conditions, which reduces the possibility of oxidation of the semiconductor material. At the same time, it ensures the uniform formation of the modified layer inside the material, providing a solid foundation for subsequent fracture.
[0016] Furthermore, a cold air flow is introduced during the laser cutting process to scan along the processing area.
[0017] The above scheme not only reduces the temperature of the local area of the modified layer, but also makes the temperature of the areas on both sides of the modified layer higher, resulting in a higher temperature gradient and large stress at the junction of the local modified layer and the unprocessed areas on both sides. When the stress is greater than the splitting threshold of the semiconductor material, it is beneficial to the separation of semiconductor grains, reducing the heat-affected zone, and improving the cutting quality to a certain extent, protecting the equipment from high-temperature damage.
[0018] Furthermore, the cooling range is limited to within 5 μm from the edge of the modified layer. This precise control ensures the maximum cooling effect while avoiding unnecessary energy loss and additional processing costs as well as the generation of thermal stress in other locations within the semiconductor material. By cooling the modified layer area in a targeted manner, the present application further promotes the generation and accumulation of stress, which is conducive to the smooth progress of subsequent fracture operations.
[0019] Furthermore, when force is applied to the modified layer, the semiconductor material is suspended below a position corresponding to the modified layer.
[0020] This design reduces the constraints and obstructions of the material during the fracture process, which is conducive to the neatness of the fracture surface and the smooth progress of the fracture process.
[0021] Furthermore, a splitter is used to apply force to the surface of the modified layer where the semiconductor is located. The splitter only applies force to the surface of the semiconductor material, which reduces the contamination of the cross section of the semiconductor cut by the splitter, makes the fracture operation more precise and controllable, and improves the fracture efficiency and success rate.
[0022] Furthermore, before the heating step, the semiconductor material is thoroughly cleaned and air-dried.
[0023] This pretreatment step ensures the cleanliness and flatness of the material surface, provides a good basic condition for subsequent laser cutting, and reduces processing defects caused by surface contamination or residues.
[0024] The present application also provides a device specifically used for laser cutting of semiconductor materials, which integrates multiple functional modules such as a three-dimensional displacement platform, a laser, a cooling device, and a splitter. The three-dimensional displacement platform has a heating function, which is used to heat the semiconductor material; the laser is responsible for emitting a laser beam and focusing it into the material for invisible cutting; the cooling device sprays cold air after the laser invisible cutting of the wafer to generate a temperature difference between hot and cold to induce stress to produce auxiliary fracture; the splitter plays a role in the final fracture step. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a step diagram of a method for laser cutting semiconductor materials in an embodiment of the present application.
[0026] Figure 2 This is an optical microscopic picture of SiC after laser invisible cutting in one embodiment of the present application.
[0027] Figure 3 This is an optical microscopic picture of a SiC surface after laser thermal cracking cutting in one embodiment of the present application.
[0028] Figure 4 This is a three-dimensional surface morphology and surface roughness of a cross section measured by a laser confocal scanner after laser stealth cutting of SiC in an embodiment of the present application.
[0029] Figure 5 In one embodiment of the present application, the linear roughness in the lateral direction of the cross section is measured based on a laser confocal scanner after laser stealth cutting of SiC.
[0030] Figure 6 In one embodiment of the present application, the linear roughness in the longitudinal direction of the cross section is measured based on a laser confocal scanner after laser stealth cutting of SiC.
[0031] Figure 7 yes Figure 2 Optical micrograph of the cross section of a SiC fragment at magnification.
[0032] Figure 8 yes Figure 3 Optical micrograph of the cross section of SiC fragments cut by laser thermal cracking at magnification. DETAILED DESCRIPTION
[0033] The present application is further described below by way of examples. The following examples are only written to help those skilled in the art better understand the present application and are not intended to limit the scope of protection of the present application. Example 1
[0034] Reference Figure 1 , a method for laser cutting semiconductor material, comprising the following steps: S1: The entire semiconductor material is heated.
[0035] First, the semiconductor material to be cut is placed in a heating furnace for overall heating treatment. The heating temperature is controlled within the range of 50-70°C, specifically 50°C, 55°C, 60°C or 65°C. This temperature range can effectively improve the processability of the semiconductor material without damaging the semiconductor material, creating favorable conditions for subsequent laser invisible cutting.
[0036] The heating time varies according to the size and shape of the semiconductor material, and is usually controlled within 5-10 minutes. For example, a piece of semiconductor material with a diameter of 100 mm and a thickness of 500 μm can achieve the desired effect by heating it at 55°C for 5 minutes.
[0037] The reason for choosing this temperature range for heating is mainly based on the following considerations: when the heating temperature is lower than 50℃, the temperature difference between hot and cold generated by the subsequent injection of cold air is relatively small, and the induced stress is difficult to assist in splitting; and when the temperature exceeds 70℃, the excessively high temperature may cause problems such as surface oxidation and thermal stress damage of semiconductor materials, which in turn affects the cutting quality. Therefore, 50-70℃ is the best temperature range that takes into account both material properties and processing efficiency.
[0038] Table 1 lists the changes in the machinability parameters of semiconductor materials at different heating temperatures. It can be seen that within the range of 50-70℃, the fracture toughness, hardness and other parameters of semiconductor materials decrease significantly, which means that they are easier to cut and process; while electrical parameters such as carrier concentration and mobility are basically unaffected, indicating that moderate heating will not change the semiconductor properties of semiconductor materials. Therefore, 50-70℃ is the best temperature range that takes into account both the machinability and performance stability of semiconductor materials.
[0039] Table 1 Temperature(℃) <![CDATA[Fracture toughness (MPa·m 1 / 2 )]]> Vickers hardness(GPa) <![CDATA[Carrier concentration (cm -3 )]]> <![CDATA[Mobility (cm 2 / V·s)]]> 25 3.5 30 <![CDATA[5×10 15 ]]> 500 40 3.2 28 <![CDATA[5×10 15 ]]> 495 55 2.9 26 <![CDATA[5×10 15 ]]> 490 70 2.7 25 <![CDATA[5×10 15 ]]> 485 S2: Use laser to perform invisible cutting inside the semiconductor material to produce a modified layer.
[0040] A picosecond laser with a wavelength of 1064nm, a pulse width of 5ps, a frequency of 200kHz, a maximum power of 100W, and a beam quality of M²<1.5 is selected to focus on the inside of the semiconductor material for invisible cutting. During the laser cutting process, the laser focus is always kept within a depth range of 10-30μm from the surface of the semiconductor material. As the cutting track moves inside the semiconductor material, a longitudinal modified layer is formed between the upper and lower surfaces of the semiconductor material.
[0041] Laser invisible cutting is a cutting technology that does not damage the upper and lower surfaces of the sample. The working principle is to focus the laser beam inside the sample. On the laser transmission path, the photon number density is low at the unfocused position, and the electrons in the SiC material cannot absorb photons to make the electrons obtain energy and transition from the valence band to the conduction band. At this position, the SiC material is transparent to the laser; the photon number density is very high at the focus point, and the electrons in the SiC material can absorb multiple photons at the same time to obtain energy greater than its bandgap width, and transition from the valence band to the conduction band. At this time, the laser and the material interact. At the focus position, a photochemical reaction occurs inside the laser under the high temperature to form a modified layer, and microcracks are formed in the longitudinal direction of the modified layer. Therefore, the selection of laser cutting parameters directly determines the quality of the modified layer. Among them, the laser wavelength and pulse width are the two most critical parameters. In order to make the laser penetrate the material for invisible cutting, the material must be transparent to the laser wavelength and not absorb linearly. 1064nm or 1030nm is the wavelength where SiC semiconductor materials absorb laser energy poorly, so invisible cutting can be performed; and ultra-short pulses of the picosecond level are conducive to high-precision, low-heat-affected precision cutting. Therefore, infrared lasers with a pulse width of picoseconds can be used to perform invisible cutting of SiC.
[0042] Figure 2 (a) shows the optical micrograph of the surface of uncut SiC after laser stealth cutting. Figure 2 (b) shows the optical micrograph of the surface of SiC cracks after laser invisible cutting. After laser invisible cutting of SiC surface, there is no material processing debris on the surface, the surface is relatively clean, and there is no edge collapse.
[0043] and Figure 3 (a) Optical micrograph of the surface of SiC without cracks after laser cutting through the surface. Figure 3 (b) shows the optical micrograph of the surface after the laser cuts through the SiC surface. After the laser cuts through the SiC surface layer by layer from the lower surface to the upper surface, thermal cracks appear on the surface due to the heat effect, causing the subsequent cracks to break along the cracks, with severe edge collapse, reaching 11.6 μm.
[0044] Table 2 summarizes the comprehensive evaluation results of invisible cutting of semiconductor materials under different laser parameters. It can be seen that under the selected laser parameters (1064nm, 5ps, 200kHz, 1W, M²<1.5), the depth-to-width ratio of the modified layer inside the semiconductor material is the largest, the heat-affected zone is the smallest, and the surface damage is the slightest, which is the optimal parameter combination for precision cutting of semiconductor materials.
[0045] Table 2 Wavelength (nm) Pulse width (ps) Frequency (kHz) Power(W) Aspect Ratio Heat affected zone(μm) Surface damage 1064 5 200 1 200:01:00 5 none 1064 10 100 0.8 150:01:00 8 slight 1030 5 200 1 200:01:00 5 none 1030 10 100 0.8 150:01:00 8 slight Forming a modified layer with a high aspect ratio (>100:1) inside the semiconductor material is the key to achieving high-quality invisible cutting. This is because: first, a high aspect ratio means that the modified layer induced by a single laser scribing has a large depth and a small line width, which is conducive to more continuous and uniform modification along the cutting track direction and the laser focus feed direction; second, a high aspect ratio helps to suppress the local thermal effect of the semiconductor material under the action of the laser, thereby minimizing the heat-affected zone and thermal damage, greatly improving material utilization, and reducing the subsequent polishing process time; finally, the larger the aspect ratio, the deeper the modified layer formed in a single scribing inside the semiconductor material, which can reduce the number of laser scribing times and greatly reduce time costs.
[0046] Table 3 compares the key quality indicators of semiconductor material grains prepared by different cutting methods. It can be seen that the method of laser invisible cutting combined with local cooling assisted fracture is far superior to traditional diamond cutting and laser thermal cracking cutting in terms of grain size consistency, fracture surface roughness, and edge collapse defects, and is currently the best solution for semiconductor material grain cutting.
[0047] Table 3 Cutting method Dimensional consistency (%) Fracture surface roughness (μm) Edge chipping defect (%) Pass rate (%) Diamond Cutting 85 10-50 5-10 70 Laser thermal cutting 90 5-20 3-7 80 Laser invisible cutting 98 0.2-2 <2 95 A coaxial air blowing auxiliary device can also be introduced during the laser cutting process. High-purity nitrogen (N2) scans the cutting area synchronously with the laser beam at a flow rate of 5-10L / min. Local air blowing can not only remove the heat and plasma generated during the cutting process, but also accelerate the heat diffusion in the cutting area, further reducing the heat affected zone. Air blowing can also effectively prevent the tiny debris and dust generated by cutting from adhering to the surface of the semiconductor material, ensuring the cutting quality. Therefore, the combination of laser invisible cutting and coaxial air blowing is an effective way to improve the efficiency and quality of semiconductor material cutting.
[0048] S3: Stop heating the semiconductor material and locally cool the corresponding area of the modified layer.
[0049] After the laser invisible cutting is completed, the overall heating of the semiconductor material is stopped immediately and it is allowed to cool naturally to room temperature. At the same time, helium (He) is used to quickly cool the adjacent areas on both sides of the modified layer. The temperature of the cooling airflow is -20°C, the flow rate is 20-30L / min, the distance between the nozzle and the surface of the semiconductor material is controlled at 2-5mm, the cooling range covers the 5-10μm area on both sides of the modified layer, and the cooling time is 10-20s.
[0050] The reason for using local cooling is to form the largest possible temperature difference and stress near the modified layer. Due to the anisotropy of the thermal expansion coefficient of semiconductor materials, local rapid cooling will produce significant stress at the interface between the modified layer and the substrate. When the stress is greater than the fracture strength of the semiconductor material, cracks will be generated along the modified layer, preparing for subsequent fracture separation.
[0051] The selection of He as local cooling gas is mainly based on the following considerations: First, the thermal conductivity of He gas (0.142W / m·K) is much greater than that of air (0.026W / m·K), and it has excellent cooling performance; second, He gas has stable chemical properties, does not react with semiconductor materials, and does not introduce impurity contamination; finally, compared with cryogenic fluids such as liquid nitrogen, He gas has less impact on the surface of semiconductor materials and does not cause mechanical damage. Therefore, He gas is an ideal choice for local cooling of the modified layer of semiconductor materials.
[0052] Before cooling, the temperature difference between the modified layer and the surrounding substrate did not exceed 40K, and the thermal stress was small; after 20s of He gas cooling, the temperature difference between the modified layer and the substrate rapidly increased to more than 300K, forming a sharp temperature gradient and stress concentration at the edge of the modified layer. The stress exceeded the fracture limit of the semiconductor material (500MPa), thereby inducing crack generation and expansion.
[0053] S4: Apply external force to the semiconductor material to cause it to break along the modified layer.
[0054] After the local cooling is completed, external force is immediately applied to the semiconductor material to make it break along the direction of the modified layer. The specific operation is: place the semiconductor material on a splitter or other splitting platform that can place semiconductor materials, and place the semiconductor material in the air directly under the modified layer facing the avoidance groove; the splitting stage adsorbs the back of the wafer, and at the same time, a splitting knife (made of cemented carbide, with a blade angle of 30-45°) is set 2-5mm above the modified layer; then, the splitting knife moves at a uniform speed of 1mm / s along the direction of the modified layer, and presses vertically downward after contacting the SiC surface. The semiconductor material is completely broken due to the compressive stress. At this time, the splitting knife does not need to directly contact the modified layer, but can achieve grain separation by simply applying pressure to the surface of the semiconductor material.
[0055] Reference Figure 4-Figure 6 , Figure 4 The three-dimensional surface morphology of the SiC cross section measured by the laser confocal scanner under a 50x objective lens is shown, where the surface roughness Sa of the cross section in test area 1 is 324.471nm, the surface roughness Sa of the cross section in test area 2 is 346.148nm, the surface roughness Sa of the cross section in test area 3 is 159.319nm, and the surface roughness Sa of the entire cross section is about 0.324µm; Figure 5 The transverse linear cross-section image under a 50x objective lens is shown, and the transverse line roughness Ra of the overall cross-section is about 0.097 µm; Figure 6 The longitudinal linear cross-section under a 50x objective lens is shown, and the longitudinal line roughness Ra of the cross-section is about 0.269 µm. This result shows that the subsequent polishing process does not require rough polishing, which can greatly reduce the process cost.
[0056] In addition, the choice of the material and blade angle of the splitter is also crucial. Cemented carbide has super high hardness and good wear resistance, and can withstand the huge compressive stress during the fracture of semiconductor materials without deformation, thus ensuring the stability of the force. The blade angle of 30-45° can form a sharp stress concentration without damaging the surface of the semiconductor material due to being too sharp. It is the best angle range for breaking semiconductor materials.
[0057] It can be seen that the semiconductor material grains obtained after the fracture of the embodiment of the present application have the following characteristics: regular grain shape, high size consistency, smooth fracture surface with low roughness, no defects such as edge collapse and corner chipping, and fully meet the high quality requirements of subsequent device processing. According to statistics, the qualified rate of semiconductor material grains prepared by this method reaches more than 95%, which is much higher than the 60-70% of traditional cutting methods, and the fracture efficiency is increased by more than 5 times, and the comprehensive production cost is reduced by more than 50%.
[0058] Reference Figure 7 , Figure 7 (c) is an optical microscopic image of the cross section of the SiC fragment at a magnification of 5 times. Figure 7 (d) is an optical microscopic image of the cross section of the SiC chip after cracking at a magnification of 10 times. Laser-modified points and induced longitudinal microcracks can be observed on the cross section, and the presence of these longitudinal microcracks reduces the difficulty of cracking.
[0059] Reference Figure 8 , Figure 8 (c) is an optical microscopic image of the cross section of a SiC slice cut by laser thermal cracking at 5 times magnification. Figure 8(d) is an optical microscopic image of the cross section of the SiC crack after laser thermal cracking at 10 times magnification. It can be seen that the expansion direction of the thermal crack is difficult to control and often deviates from the laser processing trajectory, resulting in serious edge collapse, and the cross section is severely damaged near the surface, which is very uneven and the roughness is greatly increased to 10 µm. Subsequent polishing process is required to smooth the cross section surface, which increases time, process cost and material loss rate. Example 2
[0060] It is basically the same as Example 1, except for the fracture mode.
[0061] Place the semiconductor material on the vacuum adsorption table, with the back of the wafer facing upwards and the modified layer facing the breaking device. The breaking device consists of two vacuum suction cups set opposite to each other, with the distance between the suction cups slightly larger than the size of the semiconductor material. After the semiconductor material is fixed by the vacuum adsorption table, the two suction cups move synchronously and adsorb the two ends of the wafer, and then move at a constant speed in opposite directions until the wafer is broken along the modified layer.
[0062] The breaking force of the breaking method acts on the entire cross-section of the semiconductor material, making the stress distribution more uniform and the fracture more stable and controllable; secondly, the breaking force is constant and the direction is always perpendicular to the modified layer, so the fracture accuracy is higher and the fracture surface quality is better; finally, non-contact vacuum adsorption replaces direct mechanical pressure, avoiding surface damage that may be caused by contact between the tool and the splitting knife.
[0063] The key parameters of the pull-off process include: suction cup diameter, adsorption pressure, and moving speed. Among them, the suction cup diameter must be greater than 1 / 3 of the thickness of the semiconductor material to generate a sufficiently large adsorption force; the adsorption pressure is controlled at 50-80kPa, which can not only firmly adsorb the wafer but also not generate excessive mechanical stress; the moving speed is controlled at 0.1-1mm / s. The lower the speed, the smoother the fracture and the higher the cross-section quality. Experiments show that under the optimized parameters (suction cup diameter 10mm, adsorption pressure 60kPa, moving speed 0.5mm / s), the semiconductor material prepared by the pull-off method is superior to the splitting knife fracture in terms of cross-section flatness, edge collapse rate, and integrity, and the fracture efficiency is increased by more than 20%.
[0064] Table 4 compares the accuracy of the cut surfaces of semiconductor materials prepared by different process schemes.
[0065] Table 4 Fracture method Cutting accuracy (μm) Cutting surface roughness Ra(μm) Cleaver breakage ±3 0.2-2 Pull-off cutting 20 5 Thermal cutting 15 10 It should be noted that the above embodiments are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application is described in detail with reference to the above embodiments, a person of ordinary skill in the art should understand that the technical solution of the present application can still be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application. This specific embodiment is merely an explanation of the present application and is not intended to limit the present application. After reading this specification, a person of ordinary skill in the art can make modifications to the present embodiment without creative contributions as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A method for laser cutting semiconductor material, characterized in that: The following steps are involved: Heating the semiconductor material as a whole; Use laser to cut the inside of semiconductor material invisible to produce modified layer; Stop heating the semiconductor material; Cooling the surface corresponding to the modified layer produced by the semiconductor material so as to generate stress at the modified layer; A force is applied to the surface corresponding to the modified layer of the semiconductor material, so that the semiconductor material breaks from the modified layer to form grains.
2. A method for laser cutting semiconductor material according to claim 1, characterized in that: The temperature at which the semiconductor is heated as a whole is 50-70°C.
3. A method for laser cutting semiconductor material according to claim 1, characterized in that: The laser wavelength when the laser performs invisible cutting inside the semiconductor material is 1064nm or 1030nm or other wavelengths that are transparent to the material; and / or, the laser pulse duration is 270fs-150ps; and / or, the laser frequency is 50 kHz-20MHz; and / or, the maximum power of the laser is 5W-30W; and / or, the maximum pulse energy of the laser is 50 μJ-190 μJ; And / or, the laser beam quality is M 2 <2.
4. A method for laser cutting semiconductor material according to claim 1, characterized in that: During the stealth cutting, the focus of the laser is located inside the semiconductor and is not less than 10 μm away from the surface of the semiconductor material.
5. A method for laser cutting semiconductor material according to claim 1, characterized in that: A cold air stream is scanned along the processing area where the laser is invisible cutting semiconductor materials.
6. A method for laser cutting semiconductor material according to claim 1, characterized in that: When cooling the surface corresponding to the modified layer produced by the semiconductor material, the cooling range is within 5 μm from the edge of the modified layer.
7. A method for laser cutting semiconductor material according to claim 1, characterized in that: In the step of applying force to the modified layer, the semiconductor material is suspended below the corresponding position of the modified layer.
8. A method for laser cutting semiconductor material according to claim 1, characterized in that: Use a cleaver to apply force to the surface of the modified layer where the semiconductor is located.
9. A method for laser cutting semiconductor material according to claim 1, characterized in that: Before the step of heating the semiconductor material as a whole, the semiconductor material is ultrasonically cleaned with alcohol and deionized water, and then the semiconductor material is air-dried.
10. An apparatus for laser cutting of semiconductor material, comprising: A three-dimensional displacement platform with a heating function for heating semiconductor materials; A laser is used to emit a laser beam and focus it into the semiconductor material to perform invisible cutting to produce a modified layer; A cooling device for blowing cold air to the modified layer area after laser cutting; The splitting knife is used to apply force to the surface corresponding to the modified layer of the semiconductor material, so that the semiconductor material breaks from the modified layer to form grains.
Citation Information
Cited By
Method for improving laser slicing effect of semiconductor single crystal substrate
CN119304388A