Coaxial powder feeding repair method and equipment of hydrogenation reactor, medium and product
By obtaining the chemical components and test temperature of the hydrogenation reactor, the fracture toughness and fracture energy when containing hydrogen were determined, the optimal welding process parameters were determined by using the extended finite element method and orthogonal test, and coaxial powder feeding repair was carried out, and welding was solved The joint hardening and hydrogen-induced brittleness problems have improved the welding quality and service life of the hydrogenation reactor.
Patent Information
- Application Number
- CN202411147704.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
AI Technical Summary
When existing hydrogenation reactors are in service overtime in high-temperature and high-pressure environments, the high temperature and thermal stress generated during the welding process lead to hardening or cracks in the welded joints, and the hydrogen-induced brittleness problem affects the welding quality, resulting in a shorter service life and an increase in cost.
By obtaining the chemical components and test temperature of the hydrogenation reactor, the fracture toughness and fracture energy when containing hydrogen are determined, the optimal welding process parameters are determined by using the expansion finite element method, and the optimal powder feed rate and overlap rate are determined in combination with orthogonal tests. , coaxial powder feed repair is carried out to reduce residual stress and hydrogen brittleness after welding.
The welding quality of the hydrogenation reactor is improved, the service life is extended and the replacement cost is reduced. By minimizing residual stress and hydrogen-induced brittleness problems after welding, the strength and toughness of the material are improved.
Smart Images

Figure CN119035969A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of coaxial powder feeding repair of low alloy steel, and in particular to a coaxial powder feeding repair method, equipment, medium and product of a hydrogenation reactor. Background Art
[0002] The typical characteristics of hydrogenation reactors are that they are difficult to manufacture and have a harsh service environment. Hydrogenation reactors made of 2.25Cr1Mo steel have good creep resistance and fatigue resistance and can operate stably for a long time under high temperature and high pressure. However, hydrogenation reactors have been in service for a long time under high temperature (>400℃) and high pressure (>10Mpa) hydrogen conditions. Hydrogen damage, leakage and explosion accidents occur from time to time, and hydrogen-induced degradation, regeneration cracks and other problems occur. The research on welding process, welding residual stress and the influence of post-weld heat treatment on performance, and hydrogen damage mechanism is relatively weak. Therefore, repairing the over-serviced 2.25Cr1Mo steel can extend the service life of the hydrogenation reactor and reduce costs.
[0003] Currently, there are very few methods for repairing hydrogenation reactors that have been in extended service. There are many ways to repair 2.25Cr1Mo steel, such as manual arc welding, laser welding, solder welding, etc. However, in the extended service state, that is, in the high-temperature hydrogen state, the high temperature generated during the welding process will affect the structure and performance of the material, and will cause hardening or cracking in the weld joint area; and the control of hydrogen in the weld area is a factor that causes hydrogen embrittlement in the weld area, affecting the strength and toughness of the weld joint; and the thermal stress generated during the welding process and the shrinkage during cooling will cause residual stress in the weld joint area, which is the main reason for crack propagation. These factors lead to limitations in welding quality. Summary of the invention
[0004] The purpose of the present application is to provide a coaxial powder feeding repair method, equipment, medium and product for a hydrogenation reactor to improve the welding quality of the hydrogenation reactor.
[0005] To achieve the above objectives, this application provides the following solutions:
[0006] In a first aspect, the present application provides a coaxial powder feeding repair method for a hydrogenation reactor, comprising:
[0007] Obtain the chemical composition and test temperature of the hydrogenation reactor to be repaired;
[0008] Determining the fracture toughness of the hydrogenation reactor to be repaired according to the chemical composition of the hydrogenation reactor to be repaired and the test temperature;
[0009] Performing dehydrogenation and preheating treatment on the hydrogenation reactor to be repaired;
[0010] Determining the fracture energy of the hydrogenation reactor to be repaired when hydrogen is present according to the fracture toughness of the hydrogenation reactor to be repaired;
[0011] According to the fracture toughness and fracture energy of the hydrogenation reactor to be repaired when containing hydrogen, the optimal welding process parameters are determined by using the extended finite element method; the optimal welding process parameters include laser power, welding speed and spot diameter;
[0012] According to the optimal welding process parameters, an optimal powder feeding rate and an optimal overlap rate are determined by using an orthogonal test, so as to perform coaxial powder feeding repair on the hydrogenation reactor to be repaired.
[0013] Optionally, determining the fracture toughness of the hydrogenation reactor to be repaired according to the chemical composition and test temperature of the hydrogenation reactor to be repaired specifically includes:
[0014] Determining the J coefficient according to the chemical composition of the hydrogenation reactor to be repaired;
[0015] According to the J coefficient, the ductile-brittle transition temperature value is determined;
[0016] The fracture toughness of the hydrogenation reactor to be repaired is determined according to the test temperature of the hydrogenation reactor to be repaired and the ductile-brittle transition temperature value.
[0017] Optionally, the heating temperature of the preheating treatment is 200° C., and the insulation time is 30 min-2 h.
[0018] Optionally, according to the fracture toughness of the hydrogenation reactor to be repaired, the fracture energy of the hydrogenation reactor to be repaired when containing hydrogen is determined, specifically comprising:
[0019] According to the fracture toughness of the hydrogenation reactor to be repaired, the hydrogen concentration of the hydrogenation reactor to be repaired after dehydrogenation and preheating is determined by using a relationship curve between hydrogen content and fracture toughness;
[0020] Determining the hydrogen adhesion rate of the hydrogenation reactor to be repaired after dehydrogenation and preheating according to the hydrogen concentration;
[0021] Determining the material fracture energy of the hydrogenation reactor to be repaired according to the fracture toughness of the hydrogenation reactor to be repaired;
[0022] The fracture energy of the hydrogenation reactor to be repaired when containing hydrogen is determined according to the hydrogen adhesion rate and the material fracture energy.
[0023] Optionally, determining the material fracture energy of the hydrogenation reactor to be repaired according to the fracture toughness of the hydrogenation reactor to be repaired specifically includes:
[0024] Using the formula Determine the material fracture energy of the hydrogenation reactor to be repaired; wherein, Gc (0) is the material fracture energy of the hydrogenation reactor to be repaired; K IC is the fracture toughness of the hydrogenation reactor to be repaired; E is the elastic modulus of the hydrogenation reactor to be repaired; v is the Poisson's ratio of the hydrogenation reactor to be repaired.
[0025] Optionally, determining the fracture energy of the hydrogenation reactor to be repaired when containing hydrogen according to the hydrogen adhesion rate and the material fracture energy specifically includes:
[0026] Using formula G c (θ) = (1 - 1.0467θ + 0.1687θ 2 )G c (0) determining the fracture energy of the hydrogenation reactor to be repaired when it contains hydrogen; wherein G c (θ) is the fracture energy of the hydrogenation reactor to be repaired when it contains hydrogen; G c (0) is the material fracture energy of the hydrogenation reactor to be repaired; θ is the hydrogen adhesion rate, θ=c / (c+5.5), c is the hydrogen concentration.
[0027] Optionally, the method further includes: conducting a quality assessment on the repaired hydrogenation reactor, specifically including:
[0028] Performing residual stress testing on the repaired area, heat-affected zone and substrate of the repaired hydrogenation reactor to determine the transverse stress distribution and the longitudinal stress distribution and perform stress assessment;
[0029] Conducting a tensile test on the repaired area, heat-affected zone and substrate of the repaired hydrogenation reactor to determine the tensile strength, yield strength, yield strength ratio and impact energy, and to conduct a strength assessment;
[0030] Perform toughness evaluation according to the impact energy of the repaired area and the impact energy at the substrate of the repaired hydrogenation reactor;
[0031] The repaired area of the repaired hydrogenation reactor is subjected to microstructure analysis to evaluate the structure of the hydrogenation reactor.
[0032] In a second aspect, the present application provides a computer device, comprising: a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor executes the computer program to implement the coaxial powder feeding repair method for the hydrogenation reactor described in any one of the above.
[0033] In a third aspect, the present application provides a computer-readable storage medium having a computer program stored thereon, which, when executed by a processor, implements the coaxial powder feeding repair method for a hydrogenation reactor as described in any one of the above.
[0034] In a fourth aspect, the present application provides a computer program product, including a computer program, which, when executed by a processor, implements the coaxial powder feeding repair method for a hydrogenation reactor as described in any one of the above.
[0035] According to the specific embodiments provided in this application, this application discloses the following technical effects:
[0036] The present application provides a coaxial powder feeding repair method, equipment, medium and product for a hydrogenation reactor, which obtains the chemical composition and test temperature of the hydrogenation reactor to be repaired; determines the fracture toughness of the hydrogenation reactor to be repaired according to the chemical composition and test temperature of the hydrogenation reactor to be repaired; dehydrogenates and preheats the hydrogenation reactor to be repaired; determines the fracture energy of the hydrogenation reactor to be repaired in the presence of hydrogen according to the fracture toughness of the hydrogenation reactor to be repaired; uses the extended finite element method to determine the optimal welding process parameters according to the fracture toughness and fracture energy of the hydrogenation reactor to be repaired in the presence of hydrogen; and uses orthogonal experiments to determine the optimal powder feeding rate and the optimal overlap rate according to the optimal welding process parameters, so as to perform coaxial powder feeding repair on the hydrogenation reactor to be repaired. The present application is aimed at repairing hydrogenation reactors that have been in temper embrittlement, hydrogen embrittlement and cracked conditions for over-service, and uses coaxial powder feeding for repair, providing the optimal welding process parameters, thereby achieving the effect of minimum residual stress after welding, thereby improving the welding quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 A schematic flow chart of a coaxial powder feeding repair method for a hydrogenation reactor provided in one embodiment of the present application;
[0039] Figure 2 It is a schematic diagram of the curve corresponding to hydrogen content and fracture toughness;
[0040] Figure 3 The figure is a schematic diagram of the curves of various parameters of 2.25Cr1Mo steel changing with temperature;
[0041] Figure 4 A schematic diagram of the structure of a computer device provided in one embodiment of the present application. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0043] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below with reference to the accompanying drawings and specific implementation methods.
[0044] In an exemplary embodiment, Figure 1 As shown, a coaxial powder feeding repair method for a hydrogenation reactor is provided, comprising the following steps:
[0045] S1: Obtain the chemical composition and test temperature of the hydrogenation reactor to be repaired.
[0046] S2: Determine the fracture toughness of the hydrogenation reactor to be repaired according to the chemical composition of the hydrogenation reactor to be repaired and the test temperature.
[0047] As an optional implementation, S2 specifically includes:
[0048] S21: Determine the J coefficient according to the chemical composition of the hydrogenation reactor to be repaired.
[0049] In practical applications, the degree of temper embrittlement is predicted based on the chemical composition and service time of the hydrogenation reactor to be repaired, and the fracture toughness of the reactor material is determined.
[0050] Among them, the first method to predict the ductile-brittle transition temperature FATT using the J coefficient is now the mainstream method. The J coefficient calculation method is:
[0051] J=(Mn+Si)(P+Sn)×10 4 .
[0052] Wherein, Mn is the content of manganese element; Si is the content of silicon element; P is the content of phosphorus element; Sn is the content of tin element.
[0053] S22: Determine the ductile-brittle transition temperature value according to the J coefficient.
[0054] In practical applications, the calculation formula for predicting the ductile-brittle transition temperature FATT from the J coefficient is as follows:
[0055] FATT max99% =-8.0043(10 -4 )J 2 +0.7267J-15.416.
[0056] FATT max95% =-8.5424(10 -4 )J 2 +0.7745J-48.782.
[0057] FATT max50% =-5.5147(10 -4 )J 2 +0.5757J-7732.1.
[0058] Among them, FATT max99% is the ductile-brittle transition temperature value predicted by the J factor at a 99% confidence level; FATT max95% is the ductile-brittle transition temperature value predicted by the J factor at a 95% confidence level; FATT max50% is the ductile-brittle transition temperature value predicted by the J coefficient at a 50% confidence level.
[0059] S23: Determine the fracture toughness of the hydrogenation reactor to be repaired according to the test temperature of the hydrogenation reactor to be repaired and the ductile-brittle transition temperature value.
[0060] In practical applications, the API579-2016 assessment specification provides a method for predicting the K value of the material after long-term service by using the ductile-brittle transition temperature value. IC The calculation formula is:
[0061] K IC =36.5+3.084exp[0.036(TT ref +56)].
[0062] Where, T is the test temperature; T ref FATT is the ductile-brittle transition temperature.
[0063] S3: performing dehydrogenation and preheating treatment on the hydrogenation reactor to be repaired.
[0064] In practical applications, the sample (hydrogenation reactor to be repaired) is dehydrogenated, the heating temperature is 200℃, and the holding time is 30min-2h, and then the preheating effect before welding can be achieved directly. The purpose of preheating is to reduce the thermal stress and deformation during welding; to prevent the generation of cold cracks; and to make the microstructure more uniform and reduce the formation of hardened structure and other unfavorable phases. Laser cladding welding experiments can be carried out after preheating, and preheating is the preparation work before welding.
[0065] S4: Determine the fracture energy of the hydrogenation reactor to be repaired when containing hydrogen according to the fracture toughness of the hydrogenation reactor to be repaired.
[0066] In practical applications, according to different degrees of hydrogen embrittlement, the residual hydrogen concentration is calculated based on the corresponding curve between hydrogen content and fracture toughness, and the fracture energy of the material when it contains hydrogen is calculated.
[0067] As an optional implementation, S4 specifically includes:
[0068] S41: According to the fracture toughness of the hydrogenation reactor to be repaired, the hydrogen concentration of the hydrogenation reactor to be repaired after dehydrogenation and preheating is determined by using a curve of the relationship between hydrogen content and fracture toughness.
[0069] like Figure 2 As shown in the figure, according to the corresponding curve of hydrogen content and fracture toughness (firstly, electrochemical hydrogenation is performed to obtain samples with different hydrogen contents, and then the fracture toughness of the samples with different hydrogen contents is tested to obtain Figure 2 The XFEM method (Extended Finite Element Method) follows the damage initiation criterion of the line traction separation response. When the traction force reaches the initial requirement, the crack propagation analysis and calculation begins. After the elastic-plastic change occurs, the crack tip begins to expand according to the damage law.
[0070] S42: Determine the hydrogen adhesion rate of the hydrogenation reactor to be repaired after dehydrogenation and preheating according to the hydrogen concentration.
[0071] S43: Determine the material fracture energy of the hydrogenation reactor to be repaired according to the fracture toughness of the hydrogenation reactor to be repaired.
[0072] Using the maximum principal stress damage initiation criterion in XFEM:
[0073]
[0074] f is the maximum principal stress, and damage begins to occur when f exceeds 1.
[0075] After defining the damage criterion, the damage evolution law should be defined. XFEM provides two damage evolution laws, one related to displacement and the other related to energy. The energy-based evolution law generally distinguishes the equivalent strain energy release rate Gequiv and the critical energy release rate GequivC. When Gequiv is greater than GequivC, the crack will expand. Because fracture energy is a material property that describes the material's anti-fracture performance, the energy-based evolution law is selected. The conditions for material fracture failure are defined by the BK criterion:
[0076]
[0077] With tensile strength σ b =σmax As the maximum principal stress starting criterion; the I-type crack is studied, so the material fracture energy G c =G IC =G IIC =G IIIC , is the material fracture energy of type I crack; G IIC is the material fracture energy of type II grain; G IIIC is the material fracture energy of type III grain. According to fracture mechanics theory, the material fracture energy is:
[0078]
[0079] Among them, G c (0) is the material fracture energy of the hydrogenation reactor to be repaired; K IC is the fracture toughness of the hydrogenation reactor to be repaired; E is the elastic modulus of the hydrogenation reactor to be repaired; v is the Poisson's ratio of the hydrogenation reactor to be repaired.
[0080] S44: Determine the fracture energy of the hydrogenation reactor to be repaired when containing hydrogen according to the hydrogen adhesion rate and the material fracture energy.
[0081] Due to the effect of hydrogen on the surface energy and fracture energy of the material G c The relationship between the two is the same, and the effect of hydrogen on the fracture energy of the material still conforms to the mathematical formula, which can be used to obtain the fracture energy related to hydrogen:
[0082] G c (θ) = (1 - 1.0467θ + 0.1687θ 2 )G c (0).
[0083] Among them, G c (θ) is the fracture energy of the hydrogenation reactor to be repaired when it contains hydrogen; θ is the hydrogen adhesion rate, θ=c / (c+5.5), c is the hydrogen concentration (ppm).
[0084] S5: According to the fracture toughness and fracture energy of the hydrogenation reactor to be repaired in the presence of hydrogen, an extended finite element method is used to determine optimal welding process parameters; the optimal welding process parameters include laser power, welding speed and spot diameter.
[0085] In practical applications, the extended finite element method is used to simulate the defect expansion of a reactor with micro-defects that has been in service for a long time under welding heat input conditions, detect the residual stress at the crack, and the hydrogen diffusion concentration field, so as to obtain the optimal welding process parameters.
[0086] In the process of using XFEM simulation calculation, the nodes and units with the same temperature field and stress field are used. The created cracks are imported into the cladding model, and the tangential and normal effects are added to the interaction. Then, the damage initial criterion and damage evolution law are set. According to the fracture toughness K IC With hydrogen fracture energy G c The elastic-plastic parameters obtained by (θ) are input through the material properties option.
[0087] The elastic-plastic parameters include the temperature field parameters used in the model, including thermal conductivity λ (10 W / m·K) and specific heat capacity C (10 3 J / Kg·K) and the mechanical properties parameters required in the stress field calculation. The mechanical properties parameters include the elastic modulus E(10 11 Pa), Poisson's ratioυ(10 -1 ) and thermal expansion coefficient α(10 -5 W / K). These parameters are material properties and can be found in the literature.
[0088] In the simulation of the temperature field of the cladding process, the ambient temperature is set to room temperature, the boundary conditions are convection heat transfer and thermal radiation, the radiation emissivity is 0.85, and the convection heat transfer coefficient is 10W / (m 2 .℃). In the stress field simulation calculation, the constraints of the four bottom corners are only to prevent rigid displacement, which is equivalent to cladding without external constraints. In the hydrogen diffusion analysis, the boundary condition is hydrogen activity φ, The main source of hydrogen in the cladding process is the hydrogen retained in the wall of the pressure vessel after the pressure vessel is shut down and cooled. Therefore, the introduction of hydrogen is achieved by setting the φ value at the junction of the model cladding layer and the substrate. The various parameters of 2.25Cr1Mo steel required for simulation change with temperature as follows Figure 3 shown.
[0089] The three-factor three-level orthogonal experimental method was used to conduct numerical simulation analysis under 9 groups of working conditions, and Mises stress, temperature gradient, and maximum hydrogen concentration were used as evaluation indicators for process optimization. Orthogonal analysis was performed on the design results of Mises equivalent stress, temperature gradient, and maximum hydrogen concentration to obtain the variance analysis mean diagram.
[0090] In order to determine the optimal combination of process parameters, the following formula is calculated:
[0091] S i =a i1 s i1 +a i2 s i2 +a i3 s i3 +…+a ij s ij .
[0092] Where: aij is the corresponding index coefficient; S i is the comprehensive evaluation value (total score); s ij is the corresponding indicator value.
[0093] The three indicators are selected with different importance. According to the optimization direction, the residual stress value indicator is set to 40 points, the temperature gradient value indicator is set to 30 points, and the hydrogen concentration value indicator is set to 30 points. ij = score / Δi, Δi is the difference between the maximum and minimum index values. According to the above formula, the comprehensive weighted score is calculated, and finally the welding process parameters with the highest comprehensive score are obtained, that is, the optimal welding process parameters (laser power, welding speed, spot diameter).
[0094] S6: According to the optimal welding process parameters, an optimal powder feeding rate and an optimal overlap rate are determined by using an orthogonal test to perform coaxial powder feeding repair on the hydrogenation reactor to be repaired.
[0095] Select the optimal laser power, welding speed, and spot diameter parameters, conduct welding tests, and obtain the optimal powder feeding rate and overlap rate according to the welding forming quality. That is, after the three parameters of laser power, welding speed, and spot diameter are determined, add the powder feeding rate or overlap rate, select the orthogonal experiment, combine the three factors and three levels, observe the cladding cross-sectional morphology, and whether the surface of the cladding layer is flat, so as to obtain the optimal powder feeding rate and the optimal overlap rate. Proportion the cladding powder according to the material elements. Set gas protection, use a gas mixture (M21) 82% Ar + 18% CO2, and the protective gas flow rate is 20L / min. Adjust the welding head position according to the required weld shape and cladding area, select the welding path, and use the swing welding method. After welding, heat treatment of the material is carried out to reduce residual stress. The starting temperature of the heat treatment is 400℃, the heating rate is 55℃ / h, the insulation temperature is 680℃, the insulation time is 2h, the cooling rate is 55℃ / h, and air cooling is performed after 400℃.
[0096] The powder particle size range is 50μm-150μm, and the proportion of each element is shown in Table 1.
[0097] Table 12.25Cr1Mo steel metal powder ratio table
[0098]
[0099] Residual stress tests are conducted on the repaired area, heat-affected zone and matrix to obtain transverse and longitudinal stresses. The weld samples are processed into sheet-like tensile materials and subjected to tensile tests to obtain tensile strength, yield strength and yield strength ratio. Impact tests are conducted on the sample samples to obtain impact energy. Microstructure analysis is also conducted on the sample samples to observe whether the grains are uniform and fine.
[0100] As an optional implementation method, the method further includes: performing a quality assessment on the repaired hydrogenation reactor, specifically including:
[0101] The repaired hydrogenation reactor is subjected to residual stress testing at the repaired area, heat-affected zone and substrate to determine the transverse stress distribution and the longitudinal stress distribution, and stress evaluation is performed to detect whether the residual stress distribution is uniform and within an acceptable range.
[0102] A tensile test is performed on the repaired area, heat-affected zone and substrate of the repaired hydrogenation reactor to determine the tensile strength, yield strength, yield strength ratio and impact energy, and a strength assessment is performed. The tensile strength and yield strength of different areas are compared with the tensile strength of the substrate to see whether they are close to or higher than the tensile strength and yield strength of the substrate.
[0103] The toughness is evaluated based on the impact energy of the repaired area of the repaired hydrogenation reactor and the impact energy at the substrate. The impact energy of the weld area is compared with the impact energy of the substrate through an impact test, and the impact energy of the weld area should be close to or higher than the impact energy of the substrate.
[0104] The repaired area of the repaired hydrogenation reactor is subjected to microstructural analysis to evaluate the structure of the hydrogenation reactor. The welded area should have a uniform and fine grain structure, which helps to improve the strength and toughness of the material. Check whether there are unfavorable microstructures, such as coarse grains, brittle phase precipitation in the weld heat affected zone, etc.
[0105] The present application aims at repairing the 2.25Cr1Mo steel hydrogenation reactor which has been in service for a long time and is suffering from temper embrittlement, hydrogen embrittlement and cracks. The application uses coaxial powder feeding for the repair and provides the optimal process parameters to achieve the effect of minimum residual stress after welding. The application also detects the crack propagation through mechanical property testing and microstructure observation, thereby evaluating the welding quality. The application ultimately achieves the effect of improving the coaxial powder feeding repair of the 2.25Cr1Mo steel which has been in service for a long time, prolonging the service life and reducing the replacement cost.
[0106] In an exemplary embodiment, a computer device is provided. The computer device may be a server or a terminal. The internal structure diagram thereof may be as follows: Figure 4As shown. The computer device includes a processor, a memory, an input / output interface (Input / Output, referred to as I / O) and a communication interface. Among them, the processor, the memory and the input / output interface are connected through a system bus, and the communication interface is connected to the system bus through the input / output interface. Among them, the processor of the computer device is used to provide computing and control capabilities. The memory of the computer device includes a non-volatile storage medium and an internal memory. The non-volatile storage medium stores an operating system, a computer program and a database. The internal memory provides an environment for the operation of the operating system and the computer program in the non-volatile storage medium. The input / output interface of the computer device is used to exchange information between the processor and an external device. The communication interface of the computer device is used to communicate with an external terminal through a network connection. When the computer program is executed by the processor, a coaxial powder feeding repair method for a hydrogenation reactor is implemented.
[0107] Those skilled in the art will understand that Figure 4 The structure shown in the figure is only a block diagram of a part of the structure related to the scheme of the present application, and does not constitute a limitation on the computer device to which the scheme of the present application is applied. The specific computer device may include more or fewer components than those shown in the figure, or combine certain components, or have a different arrangement of components. In an exemplary embodiment, a computer device is provided, including a memory and a processor, wherein a computer program is stored in the memory, and when the processor executes the computer program, the coaxial powder feeding repair method of the hydrogenation reactor described above is implemented.
[0108] In an exemplary embodiment, a computer-readable storage medium is provided, storing a computer program, and when the computer program is executed by a processor, the coaxial powder feeding repair method of the hydrogenation reactor is implemented.
[0109] In an exemplary embodiment, a computer program product is provided, including a computer program, which, when executed by a processor, implements the above-mentioned coaxial powder feeding repair method for the hydrogenation reactor.
[0110] It should be noted that the user information (including but not limited to user device information, user personal information, etc.) and data (including but not limited to data used for analysis, stored data, displayed data, etc.) involved in this application are all information and data authorized by the user or fully authorized by all parties, and the collection, use and processing of relevant data must comply with relevant regulations.
[0111] Those skilled in the art can understand that all or part of the processes in the above-mentioned embodiment methods can be completed by instructing the relevant hardware through a computer program, and the computer program can be stored in a non-volatile computer-readable storage medium. When the computer program is executed, it can include the processes of the embodiments of the above-mentioned methods. Among them, any reference to the memory, database or other medium used in the embodiments provided in the present application can include at least one of non-volatile and volatile memory. Non-volatile memory can include read-only memory (ROM), magnetic tape, floppy disk, flash memory, optical memory, high-density embedded non-volatile memory, resistive random access memory (ReRAM), magnetic random access memory (MRAM), ferroelectric random access memory (FRAM), phase change memory (PCM), graphene memory, etc. Volatile memory can include random access memory (RAM) or external cache memory, etc. By way of illustration and not limitation, RAM may be in various forms, such as static random access memory (SRAM) or dynamic random access memory (DRAM).
[0112] The database involved in each embodiment provided in this application may include at least one of a relational database and a non-relational database. The non-relational database may include a distributed database based on blockchain, etc., but is not limited thereto. The processor involved in each embodiment provided in this application may be a general-purpose processor, a central processing unit, a graphics processor, a digital signal processor, a programmable logic device, a data processing logic device based on quantum computing, etc., but is not limited thereto.
[0113] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0114] This article uses specific examples to illustrate the principles and implementation methods of this application. The description of the above embodiments is only used to help understand the method and core ideas of this application. At the same time, for those skilled in the art, according to the ideas of this application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting this application.
Claims
1. A coaxial powder feeding repair method for a hydrogenation reactor, characterized in that: include: Obtain the chemical composition and test temperature of the hydrogenation reactor to be repaired; Determining the fracture toughness of the hydrogenation reactor to be repaired according to the chemical composition of the hydrogenation reactor to be repaired and the test temperature; Performing dehydrogenation and preheating treatment on the hydrogenation reactor to be repaired; Determining the fracture energy of the hydrogenation reactor to be repaired when hydrogen is present according to the fracture toughness of the hydrogenation reactor to be repaired; According to the fracture toughness and fracture energy of the hydrogenation reactor to be repaired when containing hydrogen, the optimal welding process parameters are determined by using the extended finite element method; the optimal welding process parameters include laser power, welding speed and spot diameter; According to the optimal welding process parameters, an optimal powder feeding rate and an optimal overlap rate are determined by using an orthogonal test, so as to perform coaxial powder feeding repair on the hydrogenation reactor to be repaired.
2. The coaxial powder feeding repair method of the hydrogenation reactor according to claim 1, characterized in that: Determining the fracture toughness of the hydrogenation reactor to be repaired according to the chemical composition and test temperature of the hydrogenation reactor to be repaired includes: Determining the J coefficient according to the chemical composition of the hydrogenation reactor to be repaired; According to the J coefficient, the ductile-brittle transition temperature value is determined; The fracture toughness of the hydrogenation reactor to be repaired is determined according to the test temperature of the hydrogenation reactor to be repaired and the ductile-brittle transition temperature value.
3. The coaxial powder feeding repair method of the hydrogenation reactor according to claim 1, characterized in that: The heating temperature of the preheating treatment is 200° C., and the insulation time is 30 min-2 h.
4. The coaxial powder feeding repair method of the hydrogenation reactor according to claim 1, characterized in that: Determining the fracture energy of the hydrogenation reactor to be repaired when containing hydrogen according to the fracture toughness of the hydrogenation reactor to be repaired, specifically includes: According to the fracture toughness of the hydrogenation reactor to be repaired, the hydrogen concentration of the hydrogenation reactor to be repaired after dehydrogenation and preheating is determined by using a relationship curve between hydrogen content and fracture toughness; Determining the hydrogen adhesion rate of the hydrogenation reactor to be repaired after dehydrogenation and preheating according to the hydrogen concentration; Determining the material fracture energy of the hydrogenation reactor to be repaired according to the fracture toughness of the hydrogenation reactor to be repaired; The fracture energy of the hydrogenation reactor to be repaired when containing hydrogen is determined according to the hydrogen adhesion rate and the material fracture energy.
5. The coaxial powder feeding repair method of the hydrogenation reactor according to claim 4, characterized in that: Determining the material fracture energy of the hydrogenation reactor to be repaired according to the fracture toughness of the hydrogenation reactor to be repaired includes: Using the formula Determine the material fracture energy of the hydrogenation reactor to be repaired; wherein, G c (0) is the material fracture energy of the hydrogenation reactor to be repaired; K IC is the fracture toughness of the hydrogenation reactor to be repaired; E is the elastic modulus of the hydrogenation reactor to be repaired; v is the Poisson's ratio of the hydrogenation reactor to be repaired.
6. The coaxial powder feeding repair method of the hydrogenation reactor according to claim 4, characterized in that: Determining the fracture energy of the hydrogenation reactor to be repaired when containing hydrogen according to the hydrogen adhesion rate and the material fracture energy, specifically includes: Using formula G c (θ) = (1 - 1.0467θ + 0.1687θ 2 )G c (0) determining the fracture energy of the hydrogenation reactor to be repaired when it contains hydrogen; wherein G c (θ) is the fracture energy of the hydrogenation reactor to be repaired when it contains hydrogen; G c (0) is the material fracture energy of the hydrogenation reactor to be repaired; θ is the hydrogen adhesion rate, θ=c / (c+5.5), c is the hydrogen concentration.
7. The coaxial powder feeding repair method of the hydrogenation reactor according to claim 1, characterized in that: Also includes: Conduct quality assessment on the repaired hydrogenation reactor, including: Performing residual stress testing on the repaired area, heat-affected zone and substrate of the repaired hydrogenation reactor to determine the transverse stress distribution and the longitudinal stress distribution and perform stress assessment; Conducting a tensile test on the repaired area, heat-affected zone and substrate of the repaired hydrogenation reactor to determine the tensile strength, yield strength, yield strength ratio and impact energy, and to conduct a strength assessment; Perform toughness evaluation according to the impact energy of the repaired area and the impact energy at the substrate of the repaired hydrogenation reactor; The repaired area of the repaired hydrogenation reactor is subjected to microstructure analysis to evaluate the structure of the hydrogenation reactor.
8. A computer device comprising: A memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor executes the computer program to implement the coaxial powder feeding repair method for the hydrogenation reactor according to any one of claims 1 to 7.
9. A computer-readable storage medium having a computer program stored thereon, characterized in that: When the computer program is executed by a processor, the coaxial powder feeding repair method for the hydrogenation reactor according to any one of claims 1 to 7 is implemented.
10. A computer program product, comprising a computer program, characterized in that When the computer program is executed by a processor, the coaxial powder feeding repair method for the hydrogenation reactor according to any one of claims 1 to 7 is implemented.
Citation Information
Patent Citations
Test method for detecting hydrogen embrittlement sensitivity of steel
CN112945660A
Method and equipment for determining lowest boosting temperature of hydrogenation reactor and medium
CN118350195A
Method for repairing welded joint of pressure swing adsorber under hydrogen-rich alternating load
CN118438071A