Double-door ring one-time punch forming production process

The manufacturing process of side door rings is simplified through the one-stamping forming process, solving the complex and inefficient problems in traditional processes, achieving efficient production and strength improvement, and reducing costs and weight.

CN119035981APending Publication Date: 2024-11-29CHONGQING ZHIXIN IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411176792.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The manufacturing process of traditional side door ring reinforcements is complex and inefficient, requiring multiple stamping and welding, resulting in an increase in the number of molds, an extended production cycle, high cost and structural strength and durability.

Method used

Using a one-time stamping forming process, multiple sheets are prepared for laser welding and heat treatment, and then one-time stamping is performed with a large tonnage press to reduce the number of molds and stamping times, optimize the weld position and heating method to improve the finished product rate and strength.

Benefits of technology

Simplify production processes, reduce production costs, improve the strength and lightweight performance of double door rings, reduce welding difficulty and scrapping rate, and improve overall production efficiency and finished product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035981A_ABST
    Figure CN119035981A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of door ring production, and discloses a double-door ring one-time punch forming production process which comprises the following steps: step 1, preparing a plurality of material sheets according to set material sheet specifications; 2, the multiple manufactured material sheets are subjected to tailor welding according to the door ring structure, and a continuous door ring reinforcing plate is formed; 3, the whole door ring reinforcing plate is put into a heating furnace, and heating treatment is conducted according to a set heating mode; and 4, the heated door ring reinforcing plate is subjected to one-time punch forming according to a set punching mode. Through tailored blank laser welding and reheating, one-time punch forming is achieved through a large-tonnage press, the number of dies and the number of punching times are reduced, parts are lighter in weight and better in strength, and the effects of cost reduction and efficiency improvement are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of door ring production, and in particular to a one-time stamping production process for double door rings. Background Art

[0002] In the field of automobile manufacturing, the side door ring reinforcement is a key component to improve the safety of vehicle side collisions. Its design and manufacturing process have a crucial impact on the safety performance, lightweight and production efficiency of the entire vehicle. In traditional processes, the side door ring reinforcement is usually composed of multiple independent parts through welding or riveting. This multi-component structure is designed to optimize the local strength and stiffness distribution to cope with collision forces in different directions. However, even with advanced laser welding technology, the process is still complicated and inefficient.

[0003] Although laser welding can achieve high-precision and high-strength connections, due to the particularity of the side door ring reinforcement structure, at least two or more stamping processes are required to complete the initial forming of all parts, which also requires at least two sets of molds corresponding to different parts or forming stages. The increase in the number of molds not only increases the investment cost in the production preparation stage, but also extends the production cycle and increases the difficulty of maintenance. In addition, multiple stamping and welding processes may introduce additional stress concentration points, affecting the strength and durability of the overall structure, especially in complex working conditions and collision tests. At the same time, multiple processing also means higher energy consumption and material loss, further pushing up production costs. Summary of the invention

[0004] The present invention aims to provide a one-time stamping production process for double door rings, which simplifies the production process, reduces the number of molds, improves production efficiency, enhances the strength of the double door rings, and effectively reduces the weight of the door rings.

[0005] To achieve the above object, the present invention adopts the following technical scheme, a double door ring one-time stamping production process, comprising the following steps:

[0006] Step 1, preparing a plurality of sheets according to set sheet specifications;

[0007] Step 2, welding the prepared multiple sheets according to the door ring structure to form a continuous door ring reinforcement sheet;

[0008] Step 3, putting the whole door ring reinforcement sheet into the heating furnace and heating it according to the set heating mode;

[0009] Step 4, stamping the heated door ring reinforcement sheet material in one step according to a set stamping method.

[0010] The principles and advantages of this solution are:

[0011] The side door ring reinforcement is usually composed of multiple parts, usually 7. In the prior art, due to the large number of parts and the large structure and special shape after assembly, in actual processing, a side door ring reinforcement needs to be stamped at least twice, and the corresponding number of molds also needs at least 2 sets. After stamping separately, they are welded together to form the side door ring reinforcement. Although this processing process can ensure the accuracy and stability of each part, it still requires multiple stampings and multiple sets of different molds, and finally welding, resulting in a long processing cycle, poor production synchronization, and a corresponding increase in the cost of its production equipment. Finally, after forming, it undergoes multiple welding. Due to the limitations of the formed product, its welding assembly is difficult, which affects the stability of the weld and causes a high scrap rate of the product.

[0012] However, this solution first formulates multiple pieces of corresponding shapes and structures according to the structure of the side door ring, and welds the pieces first. However, when multiple pieces are welded, the position of the weld is unstable and prone to cracking. Therefore, while reducing the number of pieces, this solution selects the parts with small material feeding positions for welding, reduces the number and length of welds, prevents cracking, improves the stability of the welds, and reduces the amount of welding consumables. At the same time, the pieces are welded first to reduce the difficulty of welding and effectively reduce the scrap rate. When heating, the heating method is controlled according to the thickness of the material to prevent the parts from being overburned or underburned, ensure the stability of the heating process, and improve the yield rate. After heating, the parts are stamped and formed in one go by a large-tonnage press, which effectively reduces the number of molds and the number of stamping times, making the parts lighter and stronger.

[0013] Furthermore, in step 1, 6 sheets are used to make 6 sheets according to the set sheet specifications; and the thickness and material of each sheet are set differently according to the strength requirements.

[0014] Furthermore, in step 2, the sheets are joined by laser welding, and the weld is located in an area with a smaller material flow position.

[0015] Furthermore, the heating mode is to put the whole door ring reinforcement sheet into a heating furnace at a temperature of 840-950°C and continue heating for 4.2-5.0 minutes. According to the thickness of the sheet, different heating modes are selected and set. Specifically, the heating time and temperature are calculated according to the formula heating time T = material thickness * 90 + (100-135) s to ensure that the parts are fully heated and prevent overburning, thereby improving the part yield rate.

[0016] Furthermore, the stamping method is to use a stamping device with a size of not less than 3500*25000mm and perform one-time stamping with a pressure value of not less than 1500T, so as to ensure that the welded parts can be stamped and formed in one time, ensure the stamping and forming efficiency, and meet the stamping requirements of large parts.

[0017] Furthermore, the six sheets include a first sheet corresponding to the upper position of the A-pillar, a second sheet corresponding to the top beam position, a third sheet corresponding to the upper position of the C-pillar, a fourth sheet corresponding to the rear section of the side panel, a fifth sheet corresponding to the lower position of the B-pillar, and a sixth sheet corresponding to the door sill position.

[0018] Furthermore, the corresponding thickness of the 6 sheets is 1.2-1.8mm; among them, the corresponding material and thickness of the first sheet are CR780 / 980HS AS75 / 75, T=1.6mm; the corresponding material and thickness of the second and fourth sheets are CR950 / 1300HSAS75 / 75, T=1.4mm; the corresponding material and thickness of the third sheet are CR950 / 1300HS AS75 / 75, T=1.2mm; the corresponding material and thickness of the fifth sheet are CR950 / 1300HS AS75 / 75, T=1.8mm; the corresponding material and thickness of the sixth sheet are CR1200 / 1800HS AS75 / 75, T=1.8mm; wherein T represents thickness.

[0019] Furthermore, during the welding, the material pieces are joined together by means of wire-filling laser welding, and the joint gap between the material pieces is adjusted according to the multiple of the diameter of the filling metal wire.

[0020] Furthermore, the heating time T = material thickness * 90 + (100-135) s.

[0021] Furthermore, the method also includes step 5, laser cutting the stamped door knocker and trimming it to obtain a finished product. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a schematic diagram of the process flow of a one-time stamping production process for a double door ring.

[0023] Figure 2 The present invention is a schematic diagram of a door ring structure of a double door ring one-time stamping production process. DETAILED DESCRIPTION

[0024] The following is further described in detail through specific implementation methods:

[0025] The reference numerals in the drawings of the specification include: a first material sheet 1 , a second material sheet 2 , a third material sheet 3 , a fourth material sheet 4 , a fifth material sheet 5 , and a sixth material sheet 6 .

[0026] Example

[0027] A double door ring one-time stamping production process in the present embodiment is achieved by laser welding multiple pieces of material, heating them as a whole, and then stamping them out in one go using a large-tonnage press, thereby reducing the number of molds and the number of stamping times, while making the parts lighter and stronger, thereby achieving the effect of reducing costs and increasing efficiency.

[0028] Details are as attached Figure 1 As shown, the production process includes the following steps:

[0029] S1, according to the set sheet specifications, a plurality of sheets are prepared. Figure 2 As shown, 6 sheets of plate materials are used to make 6 sheets of material according to the set sheet specifications, and they are respectively formed into corresponding shapes. In this embodiment, the R corner of the door knocker is set to be a whole with the sheet, and no splicing is performed at the R corner to improve the splicing strength; and the thickness and material of each sheet of material are set differently according to the strength requirements.

[0030] In this embodiment, 6 sheets of 3 materials are used, namely CR950 / 1300HS AS75 / 75, CR780 / 980HS AS75 / 75, and CR1200 / 1800HS AS75 / 75; each sheet corresponds to the door sill, C-pillar, rear section of the side panel, A-pillar, and side panel position of the door knocker, and the corresponding thickness of the 6 sheets is 1.2 to 1.8 mm; and the thickness of each sheet is set differently according to the strength requirements.

[0031] Specifically, as attached Figure 2 As shown, the six pieces include a first piece 1 corresponding to the upper position of the A-pillar, wherein the first piece 1 includes the R corner corresponding to the upper part of the A-pillar; a second piece 2 corresponding to the top beam position; a third piece 3 corresponding to the upper position of the C-pillar, wherein the third piece 3 includes the R corner of the upper part of the C-pillar; a fourth piece 4 corresponding to the rear section of the side panel, wherein the fourth piece 4 includes the R corner of the side panel and the rear part of the rear window frame; a fifth piece 5 corresponding to the lower position of the B-pillar, wherein the middle part of the fifth piece 5 is the R corner of the rear part of the front window frame and the front part of the rear window frame; a sixth piece 6 corresponding to the door sill position, wherein the sixth piece 6 includes the R corner of the lower part of the A-pillar and the front part of the front window frame. The corners of the door ring are directly formed integrally with the piece, and no splicing is performed at the R corner. The area with a small material flow position is selected as the welding seam, thereby improving the connection strength of the door ring, effectively reducing the amount of solder, improving the strength performance and reducing the cost.

[0032] According to the strength requirements of the corresponding positions of each sheet, the material and thickness of each sheet are set as follows:

[0033] The corresponding material and thickness of the first sheet 1 are CR780 / 980HS AS75 / 75, T=1.6mm; the corresponding material and thickness of the second sheet 2 and the fourth sheet 4 are CR950 / 1300HS AS75 / 75, T=1.4mm; the corresponding material and thickness of the third sheet 3 are CR950 / 1300HS AS75 / 75, T=1.2mm; the corresponding material and thickness of the fifth sheet 5 are CR950 / 1300HS AS75 / 75, T=1.8mm; the corresponding material and thickness of the sixth sheet 6 are CR1200 / 1800HS AS75 / 75, T=1.8mm. T represents thickness. To ensure the strength of the corresponding position of each sheet, while reducing the overall weight as much as possible to meet the lightweight requirements of the door knocker.

[0034] S2, welding a plurality of sheet materials according to the door ring structure to form a continuous door ring reinforcement sheet material.

[0035] In this embodiment, after each sheet is cut according to the structural size, the sheets are spliced ​​by laser welding. When splicing, the weld position needs to be set in an area with a smaller material flow position. Figure 2 The R corner shown cannot be set with a laser welding position. The size of the material position is determined by the CAE analysis results. When the thinning rate exceeds 15%, the material position is determined to be large; when the thinning rate is less than 15%, the material position is determined to be small. Generally, when multiple pieces are welded, the weld position is prone to cracking. The more weld lines there are, the higher the probability of scrapping the piece. Therefore, the weld is set in a smaller area, and the number and length of weld lines are reduced to improve the strength of the piece at the weld. At the same time, the weld is used for splicing, and the strength of the connection is higher than that of the welding point.

[0036] In this embodiment, the materials are joined by wire-filled laser welding, and the gap between the materials is adjusted according to the multiple of the filler wire diameter. Specifically, the size of the gap is usually related to the diameter of the filler wire, and the gap size is adjusted and set according to 0.5 to 2 times the diameter of the wire, and is adjusted according to the actual situation to ensure the accuracy of the weld butt joint and the stability of the weld.

[0037] S3, putting the whole door ring reinforcement sheet into the heating furnace and performing heating treatment according to the set heating mode.

[0038] The whole door ring reinforcement plate after welding is placed in a heating furnace at a temperature of 840-950°C and heated for 4.2-5 minutes to convert the internal crystal structure of the steel plate into austenite, thereby improving its plasticity and formability. In this embodiment, the heating time is calculated according to the formula T=material thickness*90+(100-135)s according to the actual material thickness to ensure sufficient heating without overburning, and to ensure the stability and effectiveness of heating.

[0039] S4, performing one-time stamping forming on the heated door ring reinforcement sheet according to a set stamping method.

[0040] After heating is completed, the entire door ring reinforcement sheet is quickly transferred to the mold for high-speed stamping. During the stamping process, the door ring reinforcement sheet is subjected to high pressure and rapid cooling in the mold, and gradually formed into the required double door ring shape.

[0041] In this embodiment, the stamping method is to use a stamping equipment with a size of not less than 3500*25000mm and perform a one-time stamping with a pressure value of not less than 1500T to complete the hot pressing process and obtain a semi-finished product.

[0042] At the same time, the present embodiment also includes step 5, laser cutting the stamped door ring to cut off excess waste and holes, and trimming to obtain a finished product, thereby completing a one-time stamping production process of the double door ring.

[0043] In this embodiment, laser welding, reheating, and one-time stamping by a large-tonnage press are used to reduce the number of molds and the number of stamping times. At the same time, welding is performed first and then heating and stamping is performed, which can reduce the overlapping parts of the parts, make the parts lighter, and increase the strength of the welds, thereby improving the overall strength and achieving the effect of reducing costs and increasing efficiency.

[0044] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A one-step stamping production process for double door rings, characterized in that: The following steps are involved: Step 1, preparing a plurality of sheets according to set sheet specifications; Step 2, welding the prepared multiple sheets according to the door ring structure to form a continuous door ring reinforcement sheet; Step 3, putting the whole door ring reinforcement sheet into the heating furnace and heating it according to the set heating mode; Step 4, stamping the heated door ring reinforcement sheet material in one step according to a set stamping method.

2. The one-step stamping production process for double door rings according to claim 1, characterized in that: In step 1, 6 sheets are used to manufacture 6 sheets according to set sheet specifications; and the thickness and material of each sheet are set differently according to strength requirements.

3. The one-step stamping production process for double door rings according to claim 1 is characterized in that: In step 2, the sheets are joined by laser welding, and the weld position is set in an area with a smaller material flow position; when the thinning rate exceeds 15%, the material flow position is determined to be large; when the thinning rate is less than 15%, the material flow position is determined to be small.

4. The one-step stamping production process for double door rings according to claim 1 is characterized in that: The heating mode is to place the entire door ring reinforcement plate into a heating furnace at a temperature of 840 to 950° C. and continue heating for 4.2 to 5.0 minutes.

5. The one-step stamping production process for double door rings according to claim 1 is characterized in that: The stamping method is to use a stamping equipment with a size of not less than 3500*25000mm and perform a one-time stamping with a pressure value of not less than 1500T.

6. The one-step stamping production process for double door rings according to claim 2 is characterized in that: The 6 sheets include a first sheet corresponding to the upper position of the A-pillar, a second sheet corresponding to the top beam position, a third sheet corresponding to the upper position of the C-pillar, a fourth sheet corresponding to the rear section of the side panel, a fifth sheet corresponding to the lower position of the B-pillar, and a sixth sheet corresponding to the door sill position.

7. The one-step stamping production process for double door rings according to claim 6 is characterized in that: The corresponding thickness of the 6 sheets is 1.2-1.8 mm; among them, the corresponding material and thickness of the first sheet are CR780 / 980HS AS75 / 75, T=1.6 mm; the corresponding material and thickness of the second and fourth sheets are CR950 / 1300HS AS75 / 75, T=1.4 mm; the corresponding material and thickness of the third sheet are CR950 / 1300HS AS75 / 75, T=1.2 mm; the corresponding material and thickness of the fifth sheet are CR950 / 1300HS AS75 / 75, T=1.8 mm; the corresponding material and thickness of the sixth sheet are CR1200 / 1800HS AS75 / 75, T=1.8 mm; wherein T represents thickness.

8. The one-step stamping production process for double door rings according to claim 3 is characterized in that: During butt welding, each piece is joined together by means of filler wire laser welding, and the gap between each piece is adjusted according to the multiple of the filler wire diameter.

9. The one-step stamping production process for double door rings according to claim 4, characterized in that: Heating time T = material thickness * 90 + (100 ~ 135) s.

10. The one-step stamping production process for double door rings according to claim 1, characterized in that: The method further comprises step 5 of laser cutting the stamped door knocker and trimming the door knocker to obtain a finished product.

Citation Information

Patent Citations

  • Integrated forming method and die for automobile door ring

    CN115401429A

  • Integrated side wall inner plate double-door-ring structure, forming process and vehicle

    CN116605299A

  • Integrated tailor-welded double-door-ring structure

    CN117818761A

  • Thermal forming tailored blank laser welding integrated door ring structure and machining method

    CN118004284A

  • Side wall reinforcing plate structure

    CN221068230U