Preparation method of high-temperature-resistant graphite bipolar plate
By using an epoxy resin sealing layer to fill the pores of the graphite bipolar plate, the problem of reducing performance of the graphite bipolar plate in high temperature environment is solved, and its high temperature resistance and service life are improved, while reducing production costs.
Patent Information
- Application Number
- CN202411527487.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing graphite bipolar plates have pore problems in high temperature environments, resulting in a decrease in fuel cell performance, and poor reusability and acid-base resistance of phenolic resins, which limits the service life of the bipolar plates.
Resin A glue and resin B glue are prepared by using bisphenol A epoxy resin, phenolic epoxy resin and polyfunctional epoxy resin. Through vacuum impregnation and thermal curing treatment, high-strength and high-temperature epoxy resin sealing is formed. The layer is filled with pores of the graphite bipolar plate and improves its heat resistance.
It significantly reduces the porosity of graphite bipolar plates, improves its hardness and high temperature resistance, extends service life, and reduces production costs without affecting conductivity and mechanical properties.
Smart Images

Figure CN119036899A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to hydrogen fuel cell technology, and in particular to a method for preparing a high-temperature resistant graphite bipolar plate. Background Art
[0002] Bipolar plate (BP) is a key component in fuel cells, accounting for a large proportion of the weight, volume and cost of the fuel cell stack. Bipolar plates play many functions in fuel cells, such as distributing fuel gas and air, realizing electrical connection between monolithic cells, removing waste heat from the active area, preventing gas and coolant leakage, and promoting water management in the battery. At present, fuel cell bipolar plates are divided into the following four types: graphite bipolar plates, metal surface modified bipolar plates, and composite bipolar plates. Since the corrosion resistance of metal bipolar plates is not ideal, it is difficult to resist the corrosion caused by the acidic environment in fuel cells, and the contact resistance between metal bipolar plates and diffusion layers is higher than that between pure graphite bipolar plates and resin composite bipolar plates and diffusion layers. Therefore, graphite bipolar plates are widely used in fuel cells at present. Graphite is the earliest and most widely used material for manufacturing PEMFC bipolar plates because of its excellent electrical conductivity, thermal conductivity, chemical stability, low expansion coefficient, corrosion resistance and other properties.
[0003] During the graphitization production process, high temperature causes the organic matter in the graphite to decompose and volatilize, resulting in pores in the graphite. The pores will cause mutual penetration of the fuel cell, thereby reducing the concentration of the reaction gas and further reducing the risk of the stack performance, so the graphite bipolar plate needs to be impregnated to reduce its porosity and improve its surface quality. The most commonly used impregnation resin for graphite material is phenolic resin, and the 2124 type phenolic resin with strong fluidity and good impregnation is usually used. However, after the phenolic resin is first impregnated with graphite, its viscosity increases significantly, its fluidity deteriorates, and it cannot achieve the initial impregnation effect, so the reusability of the phenolic resin is poor. In addition, the acid and alkali resistance and high temperature resistance of phenolic resin are poor, which greatly limits the service life of the graphite bipolar plate.
[0004] Therefore, it is necessary to propose a new graphite bipolar plate preparation technology to solve the above problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a high temperature resistant graphite bipolar plate.
[0006] To solve the technical problem, the solution of the present invention is: Provided is a method for preparing a high temperature resistant graphite bipolar plate, comprising the following steps: (1) Mixing bisphenol A epoxy resin, phenolic epoxy resin, multifunctional epoxy resin, leveling agent and defoaming agent as auxiliary agents under stirring conditions to prepare resin A glue; (2) Mixing the anhydride curing agent and the accelerator under stirring conditions to obtain resin B glue; (3) Fully mixing resin A and resin B under stirring conditions to obtain a mixed resin for impregnation; (4) Adding the mixed resin into an impregnation kettle, immersing the dried graphite bipolar plate into the mixed resin, and evacuating the impregnation kettle to remove air; first impregnating under vacuum conditions, and then pressurizing the impregnation kettle and maintaining it for a period of time; (5) The graphite bipolar plate is taken out and subjected to a heat curing treatment. After natural cooling, the excess resin residue on the surface is removed by a grinder to obtain a final product, which is a high temperature resistant graphite bipolar plate.
[0007] As a preferred embodiment of the present invention, in the step (1), the model of the bisphenol A epoxy resin is one or more of E51, E54, and ZLA-185B; the model of the phenolic epoxy resin is one of F51 or F44; the model of the multifunctional epoxy resin is one of AG-80, AFG-90, and TDE-85; the model of the leveling agent is one of SY-9484, KMT-5519, and BYK-385N; and the model of the defoaming agent is one of DU-305, CK-301, and D-4200.
[0008] As a preferred embodiment of the present invention, in step (1), the mass ratio of bisphenol A epoxy resin, phenolic epoxy resin and multifunctional epoxy resin is 30-50:20-50:20-30; the leveling agent accounts for 0.1-3% of the total mass of resin A glue, and the defoaming agent accounts for 0.1-3% of the total mass of resin A glue.
[0009] As a preferred embodiment of the present invention, in the step (1), the stirring time during mixing is 10 to 40 minutes.
[0010] As a preferred embodiment of the present invention, in step (2), the anhydride curing agent is one of methyl nadic anhydride, methyl tetrahydrophthalic anhydride or methyl hexahydrophthalic anhydride; the accelerator is 2-ethyl-4-methylimidazole; and the mass ratio of the anhydride curing agent to the accelerator is 95-99.5:0.5-5.
[0011] As a preferred embodiment of the present invention, in the step (2), the stirring time during mixing is 10 to 30 minutes.
[0012] As a preferred embodiment of the present invention, in step (3), the mass ratio of resin A glue to resin B glue is 1:0.7-1.2.
[0013] As a preferred embodiment of the present invention, in the step (3), the stirring time during mixing is 10 to 30 minutes.
[0014] As a preferred embodiment of the present invention, in the step (4), the pressure in the kettle is first evacuated to less than 0.1 MPa, and the immersion time under vacuum conditions is 12 to 24 hours; then air is filled to 0.5 to 2.0 MPa, and the pressure is maintained for 2 to 6 hours.
[0015] As a preferred embodiment of the present invention, the heat curing treatment in step (5) is divided into two stages: first, the temperature is raised to 80°C for a curing time of 60 to 180 min; then, the temperature is raised to 150°C for a curing time of 240 to 600 min.
[0016] Description of the invention principle:
[0017] Epoxy resin is a special composite material of thermosetting polymer, which has excellent mechanical properties, thermal stability, excellent corrosion resistance (especially alkali resistance) and other excellent properties. The present invention proposes to use epoxy resin as an impregnating agent to replace the phenolic resin in the prior art as a plugging material for graphite bipolar plates for impregnating graphite bipolar plates.
[0018] The structure of epoxy resin contains many active groups, such as epoxy groups, ether bonds, hydroxyl groups, etc., which ensure that epoxy cured products have extremely high bonding properties. At the same time, their own high-strength cohesive force further improves the bonding strength. Moreover, epoxy resin can not only form a body cross-linked cured product with chemical bonds with the curing agent, but also undergo a ring-opening reaction under the action of a catalyst to form a cross-linked network polymer, thereby forming a cured product with different compositions and network structures. The main mechanism is that the accelerator forms a zwitterionic pair with the anhydride, in which the oxygen anion of the carboxyl group attacks the epoxy group to generate an ester bond and a new alkoxy anion, which can combine with the anhydride molecule to form a new ion pair to continue to open the epoxy group. Alternating and continuously following the above process of reaction, chain extension, branching and cross-linking, a relatively complete epoxy-anhydride cross-linked network can be formed, thereby giving the epoxy resin a variety of properties.
[0019] A certain amount of multifunctional epoxy resin is introduced into the epoxy resin plugging material used in the present invention to improve the temperature resistance. The resin is cured at high temperature to form an insoluble and infusible three-dimensional network structure with a glass transition temperature (Tg) of nearly 130°C. The present invention uses negative pressure impregnation to uniformly fill the resin in the internal pores of the graphite bipolar plate. The sealing of the bipolar plate can be reduced from 2.560sccm to 0.002sccm after one impregnation, so that the graphite bipolar plate achieves a plugging effect, while also ensuring its thermal stability in a high temperature environment.
[0020] Compared with the prior art, the technical effects of the present invention are:
[0021] 1. The main plugging material used in the present invention is epoxy resin. The presence of benzene rings in the molecular chain of bisphenol A epoxy resin improves its heat resistance, the presence of ether bonds and hydroxyl groups in the molecular chain improves its adhesion, and the presence of ether bonds in the molecular chain makes it have good alkali resistance. At the same time, the present invention introduces multifunctional epoxy resin monomers with a functionality of about 3 to 3.5, and the addition of rigid groups in the molecular chain reduces the flexibility of the molecular chain. After curing, the resin has a high cross-linking density, which improves the thermal stability of the resin at high temperatures.
[0022] 2. The epoxy resin monomer used in the present invention has a high solid content. The graphite plate is completely filled with the resin through vacuum and pressure impregnation, and the surface micropores can be effectively blocked after high-temperature treatment.
[0023] 3. The method of the present invention is simple to operate, has low equipment requirements, and has low overall cost. The prepared graphite bipolar plate will not increase the machining cost and will not cause any negative impact on the performance of the bipolar plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The figure is a flow chart for preparing the high temperature resistant graphite bipolar plate of the present invention.
[0025] Figure 2 This is a temperature test spectrum of the mixed resin used for impregnating graphite bipolar plates in Example 1.
[0026] Figure 3 This is a graph showing the change in Shore hardness of the graphite bipolar plate product in Example 1 after long-term heating (95° C.) in different media. DETAILED DESCRIPTION
[0027] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings.
[0028] The method for preparing a high temperature resistant graphite bipolar plate of the present invention has a preparation process as follows: Figure 1 As shown, the specific steps include: (1) Bisphenol A epoxy resin, novolac epoxy resin, and multifunctional epoxy resin (corresponding to Figure 1 The monomers 1, 2, 3) in the mixture are mixed with the additives (leveling agent and defoaming agent) under stirring conditions to obtain resin A glue; wherein the mass ratio of bisphenol A epoxy resin, phenolic epoxy resin and multifunctional epoxy resin is 30-50:20-50:20-30; the leveling agent accounts for 0.1-3% of the total mass of resin A glue, and the defoaming agent accounts for 0.1-3% of the total mass of resin A glue; the stirring time during mixing is 10-40 minutes.
[0029] (2) Mixing the anhydride curing agent and the accelerator under stirring conditions to obtain resin B glue; wherein the mass ratio of the anhydride curing agent to the accelerator is 95-99.5:0.5-5; and the stirring time during mixing is 10-30 min.
[0030] (3) Resin A and resin B are fully mixed under stirring conditions to obtain a mixed resin for impregnation; wherein the mass ratio of resin A to resin B is 1:0.7-1.2; and the stirring time during mixing is 10-30 min.
[0031] (4) Add the mixed resin into the impregnation kettle, immerse the dried graphite bipolar plate into the mixed resin, and evacuate the impregnation kettle to remove air; first immerse under vacuum conditions, and then pressurize the impregnation kettle and maintain it for a period of time; specifically, first evacuate the kettle until the pressure inside the kettle is less than 0.1 MPa, and the impregnation time under vacuum conditions is 12 to 24 hours; then fill it with air to 0.5 to 2.0 MPa, and maintain the pressure for 2 to 6 hours.
[0032] (5) Take out the graphite bipolar plate and perform heat curing on it; the heat curing treatment is divided into two stages: first, the temperature is raised to 80°C and the curing time is 60 to 180 minutes; then the temperature is raised to 150°C and the curing time is 240 to 600 minutes. After natural cooling, the excess resin residue on the surface is removed by a grinder, and the final product is a high temperature resistant graphite bipolar plate.
[0033] The bisphenol A epoxy resin, phenolic epoxy resin, multifunctional epoxy resin, curing agent, accelerator, defoaming agent and other raw materials described in the present invention can all be selected from commercially available products. As an optional example, the model of bisphenol A epoxy resin is one or more of E51, E54, and ZLA-185B (Kunlun ultra-pure epoxy resin); the model of phenolic epoxy resin is one of F51 or F44; the model of multifunctional epoxy resin is one of AG-80, AFG-90, and TDE-855 (4.5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester); the model of leveling agent is one of SY-9484 (Sanyue High Molecular), KMT-5519 (Foshan Koning New Materials), BYK-385N (Bick), and the model of defoaming agent is one of DU-305 (Institute), CK-301 (Tianjin Gaotian), and D-4200 (Yoshida). The anhydride curing agent is one of methyl nadic anhydride, methyl tetrahydrophthalic anhydride or methyl hexahydrophthalic anhydride; the accelerator is 2-ethyl-4-methylimidazole.
[0034] In the following embodiments and comparative examples, the graphite bipolar plates used are all products from the same batch, and the preparation process thereof refers to the preparation method disclosed in the document “A Process for Producing Isostatic Graphite” (CN101823707).
[0035] Example 1: (1) Preparation of resin A: monomers E54, F51, and AG-80 were mixed at a mass ratio of 30:50:20, and defoamer CK-301 and leveling agent SY-9484 were mixed at 3% and 3% of the total mass of A, respectively, and stirred for 20 minutes; (2) Preparation of resin B: Mix methyl nadic anhydride and 2-ethyl-4-methylimidazole in a mass ratio of 95:5 and stir for 20 minutes; (3) Mix the glue A from step (1) and the glue B from step (2) in a ratio of 1:0.7 and stir thoroughly for 30 minutes; (4) Bake the graphite bipolar plate at 170°C for 2 hours to remove trace moisture and organic matter in the graphite plate, then evacuate the resin and graphite plate to remove the air, maintain the vacuum pressure at -0.1Mpa, and hold the pressure for 12 hours. Then use an impregnation kettle to pressurize and add air to the pressure of 0.5MPa, and hold the pressure for 6 hours; (5) After impregnation, the graphite plate is taken out and then subjected to two stages of thermal curing treatment, with the thermal curing temperatures being 80°C and 150°C, and the curing times being 60 min and 600 min, respectively. After curing, the resin on the surface of the graphite plate is removed by a grinder, and finally a high-temperature resistant graphite bipolar plate sealed with resin is obtained.
[0036] Example 2: (1) Preparation of resin A: monomers E51, F44, and AFG-90 were mixed at a mass ratio of 40:35:25, and defoamer and leveling agent D-4200 and KMT-5519 were mixed at 1.5% and 1.5% of the total mass of A, respectively, and stirred for 10 minutes; (2) Preparation of resin B: methyltetrahydrophthalic anhydride and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 98:2 and stirred for 10 min; (3) Mix the glue A from step (1) and the glue B from step (2) in a ratio of 1:1.2 and stir thoroughly for 10 minutes; (4) Bake the graphite bipolar plate at 170°C for 2 hours to remove trace moisture and organic matter in the graphite plate, then evacuate the resin and graphite plate to remove the air, maintain the vacuum pressure at -0.1Mpa, and hold the pressure for 24 hours. Then use an impregnation kettle to pressurize and add air to the pressure of 1.0MPa, and hold the pressure for 3 hours; (5) After impregnation, the graphite plate is taken out and then subjected to two stages of thermal curing treatment, with the thermal curing temperatures being 80°C and 150°C, and the curing times being 120 min and 300 min, respectively. After curing, the resin on the surface of the graphite plate is removed by a grinder, and finally a high-temperature resistant graphite bipolar plate sealed with resin is obtained.
[0037] Example 3: (1) Preparation of resin A: monomers ZLA-185, F44, and TDE-85 were mixed at a mass ratio of 50:20:30, and defoamers DU-305 and leveling agents BYK-385N were mixed at 0.1% and 0.1% of the total mass of A, respectively, and stirred for 40 minutes; (2) Preparation of resin B: methyltetrahydrophthalic anhydride and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 99.5:0.5 and stirred for 30 min; (3) Mix the glue A from step (1) and the glue B from step (2) in a ratio of 1:1 and stir thoroughly for 20 minutes; (4) Bake the graphite bipolar plate at 170°C for 2 hours to remove trace moisture and organic matter in the graphite plate, then evacuate the resin and graphite plate to remove the air, maintain the vacuum pressure at -0.1Mpa, and hold the pressure for 16 hours. Then use an impregnation kettle to pressurize and add air to the pressure of 2.0MPa, and hold the pressure for 2 hours; (5) After impregnation, the graphite plate is taken out and then subjected to two stages of thermal curing treatment, with the thermal curing temperatures being 80°C and 150°C, and the curing times being 180 min and 240 min, respectively. After curing, the resin on the surface of the graphite plate is removed by a grinder, and finally a high-temperature resistant graphite bipolar plate sealed with resin is obtained.
[0038] The process parameters of each embodiment are summarized in Table 1: Table 1 Process parameters of each embodiment
[0039] Comparative Example 1 Referring to the technical solution disclosed in the patent document "A manufacturing process for impregnated graphite bipolar plates" (CN105680074A), the graphite bipolar plates are impregnated with a resin mixture.
[0040] Product testing and result analysis: The conductivity of the graphite bipolar plates in each embodiment and comparative example was tested using a four-probe resistance tester. The hardness of the graphite bipolar plates in each embodiment and comparative example was tested using a Shore hardness tester.
[0041] 1. The graphite bipolar plates were tested before resin plugging, after plugging in three embodiments of the present invention, and two graphite bipolar plates plugged by the prior art. The test results are shown in Table 2.
[0042] Table 2 Comparison of air tightness before and after plugging
[0043] From the data in Table 2, it can be seen that the hardness of the modified product of the present invention is increased from 45HS to 63HS, and the air tightness is reduced from 2.560 sccm to below 0.05 sccm, and the relevant data are significantly better than the prior art. Figure 3 It can be seen that the modified graphite bipolar plate product in Example 1 was placed in different media (HF, ethylene glycol, non-alcohol, water). After the durability verification test at 95°C and 3400 hours, the resin hardness on the product surface did not decrease significantly.
[0044] In addition, the present invention can also form a denser three-dimensional structure on the surface of the graphite bipolar plate together with other monomers by introducing a multifunctional resin containing a rigid group, so that the product has better high temperature resistance. Figure 2 This is the temperature test spectrum of the mixed resin used to impregnate the graphite bipolar plate in Example 1. It can be seen from the figure that the Tg temperature of the compounded resin is nearly 130°C, while the operating temperature of the fuel cell is between 60 and 100°C. Therefore, the present invention uses the mixed resin to impregnate the graphite bipolar plate, which can ensure the long-term stable operation of the graphite bipolar plate at high temperature. In existing public literature or commercially available products, ordinary epoxy resins, phenolic resins, dodecyl and tetradecyl glycidyl ethers are usually used for modification, and the technical starting point is only to "improve compressive strength and hardness, and reduce the generation rate of pores." The developers of these solutions did not take improving the high temperature resistance of the product as an important consideration when designing the product, and the relevant technical solutions did not bring the actual effect of improving the high temperature resistance of the product.
[0045] In summary, compared with products that have not been blocked or have been blocked by the prior art, the graphite bipolar plate that has been blocked by the preparation method of the present invention has high mechanical strength and excellent heat resistance due to the high crosslinking density and aromatic density formed by the resin on the surface. After the graphite bipolar plate is impregnated with resin, the porosity of the bipolar plate can be significantly reduced, and the hardness and density of the product can be effectively improved; and, since the main blocking material used in the present invention is epoxy resin, the high temperature resistance can be greatly improved after the impregnation treatment. Therefore, the product of the present invention can meet the requirements of air tightness, electrical conductivity and high temperature resistance of fuel cell bipolar plates.
Claims
1. A method for preparing a high temperature resistant graphite bipolar plate, characterized in that: The following steps are involved: (1) Mixing bisphenol A epoxy resin, phenolic epoxy resin, multifunctional epoxy resin, leveling agent and defoaming agent as auxiliary agents under stirring conditions to prepare resin A glue; (2) Mixing the anhydride curing agent and the accelerator under stirring conditions to obtain resin B glue; (3) Fully mixing resin A and resin B under stirring conditions to obtain a mixed resin for impregnation; (4) Adding the mixed resin into an impregnation kettle, immersing the dried graphite bipolar plate into the mixed resin, and evacuating the impregnation kettle to remove air; first impregnating under vacuum conditions, and then pressurizing the impregnation kettle and maintaining it for a period of time; (5) The graphite bipolar plate is taken out and subjected to a heat curing treatment. After natural cooling, the excess resin residue on the surface is removed by a grinder to obtain a final product, which is a high temperature resistant graphite bipolar plate.
2. The method according to claim 1, characterized in that In the step (1), the model of the bisphenol A epoxy resin is one or more of E51, E54, and ZLA-185B; the model of the phenolic epoxy resin is one of F51 or F44; the model of the multifunctional epoxy resin is one of AG-80, AFG-90, and TDE-85; the model of the leveling agent is one of SY-9484, KMT-5519, and BYK-385N; and the model of the defoaming agent is one of DU-305, CK-301, and D-4200.
3. The method according to claim 1, characterized in that In the step (1), the mass ratio of bisphenol A epoxy resin, phenolic epoxy resin and multifunctional epoxy resin is 30-50:20-50:20-30; the leveling agent accounts for 0.1-3% of the total mass of resin A glue, and the defoaming agent accounts for 0.1-3% of the total mass of resin A glue.
4. The method according to claim 1, characterized in that: In the step (1), the stirring time during mixing is 10 to 40 minutes.
5. The method according to claim 1, characterized in that In the step (2), the anhydride curing agent is one of methyl nadic anhydride, methyl tetrahydrophthalic anhydride or methyl hexahydrophthalic anhydride; the accelerator is 2-ethyl-4-methylimidazole; and the mass ratio of the anhydride curing agent to the accelerator is 95-99.5:0.5-5.
6. The method according to claim 1, characterized in that In the step (2), the stirring time during mixing is 10 to 30 minutes.
7. The method according to claim 1, characterized in that In the step (3), the mass ratio of resin A glue to resin B glue is 1:0.7-1.
2.
8. The method according to claim 1, characterized in that In the step (3), the stirring time during mixing is 10 to 30 minutes.
9. The method according to claim 1, characterized in that: In the step (4), the pressure in the kettle is first evacuated to less than 0.1 MPa, and the immersion time under vacuum conditions is 12 to 24 hours; then air is filled to 0.5 to 2.0 MPa, and the pressure is maintained for 2 to 6 hours.
10. The method according to claim 1, characterized in that The heat curing treatment in step (5) is divided into two stages: first, the temperature is raised to 80°C for a curing time of 60 to 180 minutes; then the temperature is raised to 150°C for a curing time of 240 to 600 minutes.
Citation Information
Patent Citations
Resin composition for fuel cell separator, process for producing same, and fuel cell separator
CN101933182A
Epoxy resin encapsulating material as well as preparation method and application thereof
CN104531027A
High-thermal-conductivity high-temperature-resistant toughening sealing epoxy resin and preparation method and application thereof
CN107057289A
Impregnated resin for reinforcing aramid honeycomb composite material and application of impregnated resin
CN107541018A
Graphite bipolar plate preparation method and graphite bipolar plate prepared by same
CN112310426A
Cited By
Flexible graphite composite bipolar plate for flow battery and preparation method of flexible graphite composite bipolar plate
CN120341303A
Preparation method of fuel cell graphite bipolar plate and bipolar plate prepared by preparation method
CN120784384A