Fireproof material for lithium battery module and manufacturing method thereof
Through the interlaced braiding process of oxidized fibers and silicon salt fibers with multi-layer mesh structure, the problems of failure and excessive weight of existing fire-resistant materials at high temperatures are solved, and the high fire resistance and lightweight characteristics of lithium battery modules are achieved, which is suitable for multiple Shape assembly and low cost production.
Patent Information
- Application Number
- CN202310658475.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2023-06-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-06-05
AI Technical Summary
The existing fire-resistant materials fail at high temperatures, are too heavy to bend, which limits the fire resistance, lightweight and multi-shaped assembly requirements of lithium battery modules.
The fire-resistant material with a multi-layer mesh structure is woven from staggered oxidized fibers and silicon salt fibers, and is formed by opening, blending, carding, woven cotton, needle rolling and hot pressing processes, with high refractory resistance and low thermal conductivity.
It achieves high refractory characteristics, lightness, bendability, buffering and vibration-absorbing, non-toxic, odor-free and low thermal conductivity, and is suitable for lithium battery module applications and supports fast and low-cost production.
Smart Images

Figure CN119036945A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a fireproof material, in particular to a fireproof material for a lithium battery module and a manufacturing method thereof. Background Art
[0002] like Figure 1 As shown, most of the existing fireproof materials 100a are formed by adding inorganic powder 1a to polymer resin 2a for application in lithium battery modules. Since the existing fireproof materials 100a contain polymer resin 2a, they cannot withstand temperatures higher than 400°C.
[0003] In addition, in order to improve fire resistance, existing fireproof materials need to be filled with a large amount of inorganic powder and increase thickness, resulting in excessively high material specific gravity and weight per unit area, which is not conducive to the market demand for lightweight. At the same time, existing fireproof materials are hard plates that cannot be bent, limiting terminal application products.
[0004] All of the above factors are not conducive to the fire resistance, light weight, space saving, rapid production and manufacturing requirements of existing fireproof materials, as well as the end-customers' requirements for the assembly of lithium battery modules of different shapes.
[0005] Therefore, the inventors felt that the above defects could be improved, so they devoted themselves to research and applied scientific principles, and finally proposed the present invention which has a reasonable design and effectively improves the above defects. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a fireproof material for a lithium battery module and a manufacturing method thereof in view of the deficiencies in the prior art.
[0007] In order to solve the above technical problems, one of the technical solutions adopted by the present invention is to provide a fireproof material for a lithium battery module, characterized in that the fireproof material has a stacked structure formed by stacking multiple layers of mesh structures, and each layer of the mesh structure includes: a first fiber material, which includes a plurality of first fibers, and each of the first fibers is an oxidized fiber; and a second fiber material, which includes a plurality of second fibers, and each of the second fibers is a silicate fiber (e.g., aluminum silicate fiber).
[0008] Each layer of the mesh structure is formed by interlacing a plurality of the first fibers and a plurality of the second fibers with each other; and the multi-layer mesh structure of the fireproof material has a stacking number of layers between 5 and 20 layers and a stacking thickness between 0.3 and 5 mm; wherein the fireproof material has a strength of between 0.05 and 2 g / cm 3and an overall density between 0.01 and 0.8 W / m·K.
[0009] Preferably, each of the first fibers has a first refractoriness of 700 to 1,000° C. and a first thermal conductivity of 0.02 to 0.45 W / m·K; wherein each of the second fibers has a second refractoriness of 900 to 1,100° C. and a second thermal conductivity of 0.02 to 0.5 W / m·K.
[0010] Preferably, each of the first fibers (oxidized fibers) has a first fiber length of 45 to 120 microns and a first fiber diameter of 1 to 15 microns; wherein each of the second fibers (silicon salt fibers) has a second fiber length of 50 to 75 microns and a second fiber diameter of 8 to 14 microns.
[0011] Preferably, based on 100 parts by weight of the total weight of the fireproof material, the amount of the first fiber material (oxidized fiber) is 30 to 70 parts by weight, and the amount of the second fiber material (silicon salt fiber) is 30 to 70 parts by weight.
[0012] Preferably, the multi-layer mesh structure of the fireproof material has a stacking layer number between 8 and 16 layers and a stacking thickness between 0.5 and 4 mm.
[0013] Preferably, the fireproof material has a mass of between 0.1 and 1.2 g / cm 3 and an overall density between 0.03 and 0.5 W / m·K.
[0014] In order to solve the above-mentioned technical problems, another technical solution adopted by the present invention is to provide a method for manufacturing a fireproof material for a lithium battery module, which includes: a cotton opening step, comprising: opening a plurality of first fibers and a plurality of second fibers by a cotton opener; wherein each of the first fibers is an oxidized fiber, and each of the second fibers is a silicate fiber; a cotton mixing step, comprising: mixing the opened plurality of first fibers and the plurality of second fibers with each other by a cotton mixing machine; a cotton combing step, comprising: combing the mixed plurality of first fibers and the plurality of second fibers by a cotton combing machine, so that the length direction of the plurality of first fibers and the length direction of the plurality of second fibers are straight. a cotton weaving step, comprising: weaving a plurality of the first fibers and a plurality of the second fibers through a cotton weaving machine to form a mesh structure; a needle pressing step, comprising: stacking the mesh structure into a stacked structure having a multi-layer mesh structure, and performing a needle pressing operation on the stacked structure; and a hot pressing step, comprising: performing a hot pressing operation on the needle-pressed stacked structure through a hot press to form a fireproof material for a lithium battery module; wherein the multi-layer mesh structure of the fireproof material has a stacking number of layers between 5 and 20 layers, and a stacking thickness between 0.3 and 5 mm; wherein the fireproof material has a thickness between 0.05 and 2 g / cm 3 and an overall density between 0.01 and 0.8 W / m·K.
[0015] Preferably, in the combing step, the carding machine combs the plurality of first fibers and the plurality of second fibers through a needle cloth roller.
[0016] Preferably, in the combing step, a combing needle spacing between any two adjacent combing needles among a plurality of combing needles disposed on the needle cloth roller is between 0.1 μm and 300 μm.
[0017] Preferably, in the needling step, the needling operation has a needling density of 400 to 1,800 times per inch.
[0018] Preferably, in the hot pressing step, a hot pressing temperature of the hot pressing operation is between 180°C and 240°C.
[0019] The beneficial effect of the present invention is that the fireproof material for lithium battery modules provided by the present invention can have high fire resistance through the technical scheme of "combination of the first fiber (oxidized fiber) and the second fiber (silicon salt fiber) of the mesh structure" and "specific stacking structure", and at the same time has the characteristics of light weight, bendability, thin thickness, buffering and vibration reduction, compressibility, non-toxicity, no odor, low thermal conductivity, etc. Accordingly, the fireproof material is suitable for application in lithium battery modules, especially in terminal fields for energy storage and power use. In addition, the fireproof material can be rapidly mass-produced by roll-to-roll method, so it has the advantage of low production cost.
[0020] To further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, the drawings provided are only for reference and description and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the fireproof material of the prior art.
[0022] Figure 2 It is a schematic side view of the mesh structure of the fireproof material according to an embodiment of the present invention.
[0023] Figure 3 It is a schematic top view of the mesh structure of the fireproof material according to an embodiment of the present invention.
[0024] Figure 4 Schematic diagram of the multi-layer stacking structure of the fireproof material according to an embodiment of the present invention.
[0025] Figure 5 The present invention is a flowchart of a method for manufacturing a fireproof material according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The following is an explanation of the disclosed embodiments of the present invention through specific embodiments. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the concept of the present invention. In addition, the drawings of the present invention are only simple schematic illustrations and are not depicted according to actual dimensions. It is stated in advance. The following embodiments will further explain the relevant technical contents of the present invention in detail, but the disclosed contents are not intended to limit the scope of protection of the present invention.
[0027] It should be understood that, although the terms "first", "second", "third" and the like may be used herein to describe various materials or parameters, these materials or parameters should not be limited by these terms. These terms are mainly used to distinguish one material from another material, or one parameter from another parameter. In addition, the term "or" used herein may include any one or more combinations of the associated listed items depending on the actual situation.
[0028] [Fireproof materials for lithium battery modules]
[0029] See also Figure 2 and Figure 3 As shown, an embodiment of the present invention provides a fireproof material 100 for a lithium battery module. The fireproof material 100 comprises a first fiber material 1 and a second fiber material 2.
[0030] The first fiber material 1 comprises a plurality of first fibers, and the second fiber material 2 comprises a plurality of second fibers. The plurality of first fibers and the plurality of second fibers are interlaced and woven with each other to form a mesh structure (such as Figure 3 shown).
[0031] Each of the first fibers is an oxidized fiber, which may be an oxidized polyacrylonitrile fiber (oxidized PAN fiber), but the present invention is not limited thereto.
[0032] The first fiber (oxidized fiber) has a first refractoriness between 700°C and 1,000°C (preferably 800°C to 900°C) and a first thermal conductivity between 0.02W / m·K and 0.45W / m·K (preferably 0.14W / m·K to 0.2W / m·K).
[0033] Specifically, each of the first fibers (oxidized fibers) has a first fiber length ranging from 45 μm to 120 μm (preferably 45 μm to 60 μm, particularly preferably 45 μm to 55 μm).
[0034] In addition, each of the first fibers (oxidized fibers) has a first fiber diameter ranging from 1 μm to 15 μm (preferably 1 μm to 5 μm, particularly preferably 1 μm to 3 μm).
[0035] Each of the second fibers is an aluminum silicate fiber.
[0036] The second fiber (silicon salt fiber) has a second refractoriness between 900°C and 1,100°C (preferably 950°C to 1,050°C) and a second thermal conductivity between 0.02W / m·K and 0.5W / m·K (preferably 0.03W / m·K to 0.4W / m·K).
[0037] Furthermore, each of the second fibers has a second fiber length between 50 μm and 75 μm (preferably 52 μm to 67 μm). In addition, each of the second fibers has a second fiber diameter between 8 μm and 14 μm (preferably 8 μm to 12 μm).
[0038] In terms of dosage, based on the total weight of the fire-proof material 100 being 100 parts by weight, the dosage of the first fiber material 1 (oxidized fiber) is between 30 parts by weight and 70 parts by weight, and preferably between 45 parts by weight and 60 parts by weight, and the dosage of the second fiber material 2 (silicon salt fiber) is between 30 parts by weight and 70 parts by weight, and preferably between 35 parts by weight and 45 parts by weight.
[0039] According to the above configuration, the first fiber (oxidized fiber) is used to provide the fabric support strength and basic fire-resistant properties required by the fire-resistant material 100 , and the second fiber (silicon salt fiber) is used to further enhance the fire-resistant properties of the fire-resistant material 100 .
[0040] In a specific embodiment of the present invention, Figure 4 As shown, the mesh structure formed by the plurality of first fibers and the plurality of second fibers can be further stacked to form a stacked structure having multiple layers of the mesh structure. In other words, the fireproof material 100 has multiple layers of the mesh structure stacked on each other, and each layer of the mesh structure is formed by multiple first fibers and multiple second fibers that are interlaced and woven with each other. The stacked structure can be formed by stacking the same mesh structure in a continuous shape, but the present invention is not limited thereto.
[0041] Furthermore, the fireproof material 100 having a multi-layer mesh structure stacked one above the other may have a stacking number of layers ranging from 5 to 20 layers, and preferably ranging from 8 to 16 layers. Furthermore, the fireproof material 100 has a stacking thickness T ranging from 0.3 mm to 5 mm, and preferably ranging from 0.5 mm to 4 mm.
[0042] In general, the fireproof material 100 formed by the first fiber material 1 and the second fiber material 2 has a hardness between 0.05 g / cm 3 Up to 2g / cm 3 An overall density of , and preferably between 0.1 g / cm 3 Up to 1.2g / cm 3The fireproof material 100 has an overall thermal conductivity between 0.01 W / m·K and 0.8 W / m·K, and preferably between 0.03 W / m·K and 0.5 W / m·K.
[0043] According to the above configuration, the fireproof material 100 provided in the embodiment of the present invention can have high fire resistance, and at the same time has the characteristics of light weight, thin thickness, flexibility, cushioning and vibration reduction, compressibility, non-toxicity, no odor, low thermal conductivity, etc., so that the fireproof material 100 is suitable for application in lithium battery modules, especially in terminal fields for energy storage and power purposes.
[0044] In addition, the fireproof material 100 provided in the embodiment of the present invention can be rapidly mass-produced in a roll-to-roll manner, and thus has the advantage of low production cost.
[0045] It is worth mentioning that the "thermal conductivity" or "K value" mentioned in this article refers to the ability of any uniform material to directly conduct heat, or thermal conductivity. If the K value of a material is 1, it means that when the temperature difference between the two surfaces of the material is 1 degree, 1 cubic meter of the material will transfer heat at a rate of 1 watt, that is, the K value is 1W / m·K. The lower the K value, the less the material's ability to transfer heat.
[0046] In addition, the "refractory" mentioned in this article refers to the temperature at which a material reaches a certain softening degree or whether it catches fire under high temperature, which characterizes the material's ability to resist high temperature. The refractoriness determination method can be, for example, the international standard test method GB / T7322-1997 (ISO 528:1983) "Refractoriness Test Method for Refractory Materials", but the present invention is not limited thereto.
[0047] It is worth mentioning that in a preferred embodiment of the present invention, the fireproof material 100 further includes a third fiber material (not shown) interlaced with the first fiber material 1 and the second fiber material 2 to form the mesh structure. The third fiber material includes a plurality of third fibers, and each of the third fibers is a ceramic fiber.
[0048] Each of the third fibers (ceramic fibers) has a third refractoriness between 1,000 and 1,200°C (preferably 1,050 to 1,150°C), and a third thermal conductivity between 0.02 and 0.5 W / m·K (preferably 0.05 to 0.5 W / m·K). Further, each of the third fibers (ceramic fibers) has a third fiber length between 30 microns and 60 microns (preferably 45 microns to 55 microns, particularly preferably 45 microns to 52 microns). In addition, each of the third fibers (ceramic fibers) has a third fiber diameter between 10 microns and 16 microns (preferably 10 microns to 14 microns, particularly preferably 11 microns to 13 microns). In terms of dosage, based on the total weight of the fireproof material being 100 parts by weight, the dosage of the third fiber (ceramic fiber) is between 1 part by weight and 20 parts by weight, preferably between 3 parts by weight and 18 parts by weight, and particularly preferably between 5 parts by weight and 10 parts by weight. The third fiber (ceramic fiber) can further provide a reinforcement and fire-resistant effect.
[0049] [Manufacturing method of fireproof material for lithium battery module]
[0050] The above is a description of the material characteristics of the fireproof material for lithium battery module according to the embodiment of the present invention. Figure 5 As shown, an embodiment of the present invention further provides a method for manufacturing a fireproof material for a lithium battery module, which includes step S110 (cotton opening step), step S120 (cotton mixing step), step S130 (cotton combing step), step S140 (cotton weaving step), step S150 (needle rolling step), and step S160 (hot pressing step).
[0051] It should be noted that the order of the steps and the actual operation methods in the embodiments of the present invention can be adjusted as needed and are not limited to those in the present embodiment. The manufacturing method of the embodiments of the present invention can provide additional operations before, during, or after each step, and some of the operations described can be replaced, eliminated, or relocated to achieve additional implementations.
[0052] The step S110 is to implement a cotton opening step, which includes opening a plurality of first fibers (oxidized fibers) of the first fiber material 1 and a plurality of second fibers (silicon salt fibers) of the second fiber material 2 through a cotton opening machine, so that the plurality of first fibers and the second fibers are in a uniformly opened and fluffy state.
[0053] The step S120 is to implement a cotton blending step, which includes mixing a plurality of first fibers (oxidized fibers) and a plurality of second fibers (silicon salt fibers) that have been opened with a cotton blending machine.
[0054] The step S130 is to implement a cotton carding step, which includes using a cotton carding machine to card the mixed first fibers (oxidized fibers) and the second fibers (silicon salt fibers) so that the length directions of the first fibers and the second fibers are consistent (e.g., Figure 3 shown).
[0055] It is worth mentioning that in a preferred embodiment of the present invention, the carding machine in step S130 combs the plurality of first fibers (oxidized fibers) and the plurality of second fibers (silicon salt fibers) through a card clothing roll of the carding machine.
[0056] The needle punch spacing between any two adjacent needle punches among the plurality of needle punches disposed on the needle cloth roller needs to be between 0.1 μm and 300 μm, preferably between 10 μm and 30 μm, and particularly preferably between 15 μm and 22 μm.
[0057] The step S140 is to implement a cotton weaving step, which includes weaving a plurality of first fibers (oxidized fibers) and a plurality of second fibers (silicon salt fibers) that have been combed by a cotton weaving machine to form a continuous mesh structure. In one embodiment of the present invention, the cotton weaving machine can be, for example, an air jet loom, but the present invention is not limited thereto.
[0058] It is worth mentioning that, since in the step S130, a needle spacing between any two adjacent needles among the plurality of needles arranged on the needle cloth roller is specially adjusted, the plurality of first fibers (oxidized fibers) and second fibers (silicon salt fibers) combed by the carding machine can be easily formed into the continuous mesh structure by a loom (such as a jet loom), and the fibers will not fall between the rollers in the loom, but the present invention is not limited to this.
[0059] If the combing needle spacing exceeds the above range, the plurality of fibers may not easily form a continuous mesh structure, or the plurality of fibers may easily fall between the rollers in the cotton loom.
[0060] The step S150 is to implement a needle rolling step, which includes: stacking the continuous mesh structure formed by the step S140 into a stacked structure with 5 to 20 layers (preferably 8 to 16 layers).
[0061] The needling step further includes: performing a needling operation on the stacked structure. The needling density of the needling operation is preferably 400 to 1,800 times per inch, and preferably 400 to 600 times, so that the stacked structure can have an ideal overall density (e.g., 0.05 to 2 g / cm 3 ), stack thickness (e.g., 0.3 to 5 mm), and thermal conductivity (e.g., 0.01 to 0.8 W / m·K).
[0062] The step S160 is to implement a heat pressing step, which includes performing a heat pressing operation on the needle-pressed stacked structure through a heat pressing machine to form the fireproof material 100 for the lithium battery module.
[0063] Wherein, a hot pressing temperature of the hot pressing operation is between 180°C and 240°C.
[0064] According to the above configuration, the fireproof material 100 provided in the embodiment of the present invention can have high fire resistance, and at the same time has the characteristics of light weight, thin thickness, flexibility, cushioning and vibration reduction, compressibility, non-toxicity, no odor, low thermal conductivity, etc., so that the fireproof material 100 is suitable for application in lithium battery modules, especially in terminal fields for energy storage and power purposes.
[0065] Preferably, the above manufacturing method can also be performed on the third fiber (ceramic fiber) at the same time.
[0066] [Experimental data and test results]
[0067] In order to verify the technical effect of the fireproof material for lithium battery module and the manufacturing method thereof of the present invention, the following will be described with experimental data and experimental results. However, the following embodiments and comparative examples are only for the purpose of facilitating the understanding of the present invention, and the protection scope of the present invention is not limited thereto.
[0068] Embodiment 1: According to the process parameters listed in Table 1, a plurality of oxidized fibers, a plurality of silicate fibers, and a plurality of ceramic fibers are opened by a cotton opener; the opened plurality of fibers are mixed with each other by a cotton blender; the mixed plurality of fibers are combed by a cotton combing machine to make the length directions of the fibers tend to be consistent; wherein a combing needle spacing between any two adjacent combing needles arranged on the needle cloth roller is as shown in Table 1; the combed plurality of fibers are woven by a cotton loom to form a continuous mesh structure; the continuous mesh structure is stacked into a stacking structure and a needle pressing operation is performed on the stacking structure, wherein a needle pressing density of the needle pressing operation is as shown in Table 1; and finally a hot pressing operation is performed on the needle pressed stacking structure by a hot press to form a fireproof material for a lithium battery module.
[0069] The preparation methods of Examples 2 to 4 and Comparative Examples 1 to 3 are the same as that of Example 1, except that the process conditions are summarized in Table 1. Comparative Example 4 uses commercially available PU foam insulation material. Comparative Example 5 uses commercially available aerogel fireproof material.
[0070] Next, the fireproof materials prepared in the above-mentioned embodiments and comparative examples were tested for properties such as thickness, density, thermal conductivity (k value), fiber state, fireproof material refractoriness, and lithium battery module introduction evaluation. The relevant test results are shown in Table 1.
[0071] In terms of test methods, the thickness is tested in a general conventional way, which will not be described in detail here. Density test method: Take a 100 square centimeters (tolerance ± 2mm) sample and weigh it. The weight is X g. Calculate the square meter weight (g / m 2 )=100×Xg, density (g / cm 3 ) = square meter weight g / m 2 / Thickness mm / 1000. The definition or test method of thermal conductivity and fire resistance of fireproof materials has been explained above and will not be repeated here.
[0072] The fiber state test method is to use a stereo microscope (dissecting microscope) to observe the fireproof material sample at a magnification of 50 times to confirm whether there is any breakage. The lithium battery module introduction evaluation is to introduce the fireproof material into the lithium battery module to evaluate whether the lithium battery module can operate normally. If it can operate normally, it will be evaluated as Pass, and if it cannot operate normally, it will be evaluated as NG.
[0073] [Table 1]
[0074]
[0075]
[0076] [Results and Discussion]
[0077] According to the above experimental results, the fiber state of the fireproof materials of Examples 1 to 4 did not break. The fireproof materials were fireproof and would not burn. The evaluation of the introduction into the lithium battery module was passed.
[0078] The needle rolling density per inch of Comparative Example 1 is 200 times, which is lower than the ideal 400 times. Therefore, the thermal conductivity of the fireproof material finally formed is lower than that of Examples 1 to 4, and it is evaluated as NG when introduced into the lithium battery module. The amount of oxidized fiber used in Comparative Example 2 is too high (85 grams) and the amount of silicate fiber used is too low (5 grams), so that the fireproof material will burn in the fire resistance test, and it is evaluated as NG when introduced into the lithium battery module. The amount of oxidized fiber used in Comparative Example 3 is too low (5 grams) and the amount of silicate fiber used is too high (85 grams), so that the fiber state will break, and it is evaluated as NG when introduced into the lithium battery module. Comparative Examples 4 to 5 use commercially available materials, which all severely caught fire and burned in the fire resistance test.
[0079] [Beneficial Effects of Embodiments]
[0080] The beneficial effect of the present invention is that the fireproof material for lithium battery modules provided by the present invention can have high fire resistance through the technical scheme of "combination of the first fiber (oxidized fiber) and the second fiber (silicon salt fiber) of the mesh structure" and "specific stacking structure", and at the same time has the characteristics of light weight, thin thickness, bendability, buffering and vibration reduction, compressibility, non-toxicity, no odor, low thermal conductivity, etc. Accordingly, the fireproof material is suitable for application in lithium battery modules, especially in terminal fields for energy storage and power use. In addition, the fireproof material can be rapidly mass-produced by roll-to-roll method, so it has the advantage of low production cost.
[0081] The contents disclosed above are only preferred feasible embodiments of the present invention, and are not intended to limit the scope of the present invention. Therefore, all equivalent technical changes made using the contents of the present invention description and drawings are included in the scope of the present invention.
Claims
1. A fireproof material for lithium battery modules, It is characterized in that The fireproof material has a stacked structure formed by stacking multiple layers of mesh structures, and each layer of the mesh structure includes: a first fiber material, which includes a plurality of first fibers, and each of the first fibers is an oxidized fiber; and a second fiber material comprising a plurality of second fibers, wherein each of the second fibers is a silicate fiber; Each layer of the mesh structure is formed by interlacing a plurality of the first fibers and a plurality of the second fibers with each other; and the multi-layer mesh structure of the fireproof material has a stacking number of layers between 5 and 20 layers and a stacking thickness between 0.3 and 5 mm; wherein the fireproof material has a strength of between 0.05 and 2 g / cm 3 and an overall density between 0.01 and 0.8 W / m·K.
2. The fireproof material for lithium battery module according to claim 1, It is characterized in that Each of the first fibers has a first refractoriness of 700 to 1,000 degrees Celsius and a first thermal conductivity of 0.02 to 0.45 W / m·K; wherein each of the second fibers has a second refractoriness of 900 to 1,100 degrees Celsius and a second thermal conductivity of 0.02 to 0.5 W / m·K.
3. The fireproof material for lithium battery module according to claim 2, It is characterized in that Each of the first fibers has a first fiber length of 45 to 120 microns and a first fiber diameter of 1 to 15 microns; wherein each of the second fibers has a second fiber length of 50 to 75 microns and a second fiber diameter of 8 to 14 microns.
4. The fireproof material for lithium battery module according to claim 3, It is characterized in that Based on 100 parts by weight of the total weight of the fireproof material, the first fiber material is used in an amount of 30 to 70 parts by weight, and the second fiber material is used in an amount of 30 to 70 parts by weight.
5. The fireproof material for lithium battery module according to any one of claims 1 to 4, It is characterized in that The multi-layered mesh structure of the fireproof material has a stacking number of layers between 8 and 16 layers and a stacking thickness between 0.5 and 4 mm; wherein the fireproof material has a thickness between 0.1 and 1.2 g / cm 3 and an overall density between 0.03 and 0.5 W / m·K.
6. A method for manufacturing a fireproof material for a lithium battery module, It is characterized in that The method for manufacturing the fireproof material comprises: A cotton opening step, comprising: opening a plurality of first fibers and a plurality of second fibers by a cotton opening machine; wherein each of the first fibers is an oxidized fiber, and each of the second fibers is a silicate fiber; a cotton blending step, comprising: mixing the plurality of first fibers and the plurality of second fibers that have been opened with a cotton blending machine; a combing step, comprising: combing the mixed plurality of first fibers and the plurality of second fibers by a combing machine, so that the length directions of the plurality of first fibers and the length directions of the plurality of second fibers tend to be consistent; a cotton weaving step, comprising: weaving the combed first fibers and the second fibers through a cotton weaving machine to form a mesh structure; a needling step, comprising: stacking the mesh structures into a stacked structure having multiple layers of mesh structures, and performing a needling operation on the stacked structure; and A hot pressing step, comprising: performing a hot pressing operation on the needle-pressed stacked structure by a hot press machine to form a fireproof material for a lithium battery module; The multi-layered mesh structure of the fireproof material has a stacking number of layers between 5 and 20 layers and a stacking thickness between 0.3 and 5 mm; The fireproof material has a thickness between 0.05 and 2 g / cm 3 and an overall density between 0.01 and 0.8 W / m·K.
7. The method for manufacturing a fireproof material for a lithium battery module according to claim 6, It is characterized in that In the combing step, the combing machine combs the plurality of first fibers and the plurality of second fibers through a needle cloth roller.
8. The method for manufacturing a fireproof material for a lithium battery module according to claim 7, It is characterized in that In the combing step, a combing needle spacing between any two adjacent combing needles among a plurality of combing needles disposed on the needle cloth roller is between 0.1 micrometers and 300 micrometers.
9. The method for manufacturing a fireproof material for a lithium battery module according to claim 6, It is characterized in that In the needling step, the needling operation has a needling density of 400 to 1,800 times per inch.
10. The method for manufacturing a fireproof material for a lithium battery module according to claim 6, It is characterized in that In the hot pressing step, a hot pressing temperature of the hot pressing operation is between 180 degrees Celsius and 240 degrees Celsius.
Citation Information
Patent Citations
Pipe covering fireproof material
CN110884233A
Multi-layer fireproof material for battery and manufacturing method of multi-layer fireproof material
CN112959759A
Thermal-insulation fireproof cloth for power battery and preparation method therefor
WO2023284272A1