Method for expanding aperture of full-porous spherical silica gel
By using salt solution and calcining treatment in silica gel, the pore size of the silica gel is expanded, and the problem of poor separation effect caused by small pore size in the prior art is solved, efficient separation of macromolecules and column efficiency improvement is achieved, and it is suitable for the field of chromatography.
Patent Information
- Application Number
- CN202411165969.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The pore size of existing industrially produced silica gel microspheres is small, which limits the separation effect on macromolecular compounds such as proteins and biological macromolecules, and cannot achieve optimal drug separation and column effectiveness.
By dispersing small pore mesoporous silica gel in a salt solution, drying and calcining, the salt melts and erodes the silica gel structure, forming large pores, and achieving pore size expansion. The specific steps include using single/compound salt solution, ultrasonication, stirring, Constant temperature drying and program heating and calcining, the pore size is controlled between 50 and 200 nm.
Large-pore silica gel with controllable pore size and narrow distribution is obtained, which is suitable for chromatography, and can achieve effective separation of macromolecules and high column efficiency. It is simple to operate and low cost. It is suitable for large-scale preparation and strong transplantability.
Smart Images

Figure CN119038561A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material preparation, relates to the pore expansion and application of spherical silica gel, and in particular to a method for expanding the pore size of fully porous spherical silica gel by selecting a salt solution, adjusting the salt concentration and controlling the temperature. Background Art
[0002] With the prosperity and development of social economy, people's desire for health and maintenance are increasing day by day. When people face health problems, the use of drugs is a direct, fast, extensive and effective means. Single-configuration chiral drugs often have higher activity and efficacy and lower toxic side effects than their racemic drugs. According to statistics, 56% of the drugs listed globally are of single configuration. In addition to artificial synthesis, another way to obtain single-configuration chiral drugs is to extract and separate them from nature. Chromatography, as the most effective method for splitting chiral drugs, has its irreplaceable advantages. Among them, the core role is played by the chiral stationary phase, also known as chiral filler, which is usually obtained by coating or bonding the derived chiral substance on the surface of spherical silica gel. The reason why silica gel can be used as the most commonly used chromatographic filler matrix is that it has the advantages of good chemical inertness, high mechanical strength, long service life, and no reaction with the reagents used. The separation of compounds of different molecular weights requires silica gel to provide different pore sizes. The larger the pore size of the silica gel microspheres, the larger the molecular weight of the substance that can be measured. The pore size of industrially produced raw silica balls is relatively small. If they are used as fillers or filler matrices to separate proteins, biomacromolecules and chiral substances with large molecular weights, the diffusion of molecules in and out of the pores will be restricted, and good separation effects and high column efficiency cannot be obtained. The pore size of the silica matrix needs to be expanded to meet the appropriate pore size requirements in order to achieve the best separation effect. Summary of the invention
[0003] The object of the present invention is to provide a method for expanding the pore size of fully porous spherical silica gel, which can be effectively used as a filler or filler matrix for separating macromolecular compounds, such as proteins, biomacromolecules, etc. The macroporous silica gel prepared by the present invention not only has a controllable pore size and a narrow pore size distribution, but also can obtain the required pore size after only one pore expansion, is simple to operate, low in cost, can be prepared in large quantities, and is particularly suitable for related applications in the field of chromatography.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] A method for expanding the pore size of a fully porous spherical silica gel, comprising the following specific steps:
[0006] Using small-pore mesoporous silica as raw material, spherical silica gel is dispersed in a single / double salt solution so that the salt solution can fully enter the internal pores of the silica gel. The silica gel is dried at a constant temperature for a period of time in an ordinary oven and a vacuum drying oven. The silica gel is calcined by heating to a specified high temperature through a program. The salt in the silica gel pores reaches a molten state and corrodes its structure, forming a new stacking method. After cooling, looser and larger pores are formed to obtain macroporous spherical silica gel.
[0007] The small-pore silica gel is used as the raw material, and the pore size of the raw silica gel is 2-10 nm.
[0008] The spherical silica gel is dispersed in a single / double salt solution:
[0009] If spherical silica gel is dispersed in a single salt solution and salt is soaked by ultrasound and stirring, the single salt includes an alkali metal halide salt, such as NaCl or LiCl, the concentration of the single salt solution is 2% to 10%, the ultrasound time of the salt soaking process is 5 to 30 minutes, and the stirring time is 1 to 10 hours.
[0010] If spherical silica gel is dispersed in a complex salt solution, the complex salt is a mixture of two single salts, and salt is soaked by ultrasound and stirring. The complex salt is a mixture of two single salts, such as two-component complex salt NaCl / LiCl, NaCl / NaNO3, the concentration of the complex salt solution is 4% to 15%, and the complex salt ratio is 10:5 to 1:3.
[0011] If spherical silica gel is dispersed in a complex salt solution and salt is soaked by ultrasound and stirring, the complex salt is a mixture of three single salts, such as three-component complex salts NaCl / LiCl / KNO3, NaCl / LiCl / NaNO3, the concentration of the complex salt solution is 20% to 40%, and the complex salt ratio is 10-20:5-10:5-10.
[0012] The temperatures for drying the silica gel in the common oven and the vacuum drying oven are 120-180° C. and 90-150° C. respectively, and the constant temperature time is 1-5 hours.
[0013] The silica gel is calcined by heating the temperature to a specified high temperature through a program, the program heating rate is 1 to 10°C / min, the heating time is 1.5 to 9 hours, and the pore size of the silica gel after pore expansion is 50 to 200 nm.
[0014] If a single-component salt is used for pore expansion, the silica gel is calcined at a temperature of 680 to 790° C., the calcination time at high temperature is 2 to 15 hours, and the pore size of the silica gel after pore expansion is 50 to 200 nm.
[0015] If two-component double salt is used for pore expansion, the temperature of silica gel calcined at high temperature is 500-650°C, the calcination time at high temperature is 2-10 hours, and the pore size of silica gel after pore expansion is 50-200nm.
[0016] If three-component double salt is used for pore expansion, the temperature of silica gel calcined at high temperature is 450-600°C, the calcination time at high temperature is 2-8 hours, and the pore size of silica gel after pore expansion is 50-200nm.
[0017] The macroporous silica gel obtained by any of the above-mentioned preparation methods can be applied in the field of chromatographic separation.
[0018] In order to obtain spherical silica gel with optimal pore size and suitable specific surface area, the present invention provides a method for expanding the pore size of fully porous spherical silica gel. Using small-pore mesoporous silica gel as raw material, spherical silica gel is dispersed in a single / complex salt solution, so that the salt solution can fully enter the internal pores of the silica gel, and the silica gel is dried at a constant temperature for a period of time in an ordinary oven and a vacuum drying oven, and the temperature is programmed to be increased to a specified high temperature. The salt in the silica gel pores reaches a molten state and corrodes its structure, forming a new stacking method. After cooling, a looser and larger pore is formed to obtain macroporous spherical silica gel. The macroporous silica gel prepared by the present invention not only has a controllable pore size and a narrow pore size distribution, but also can obtain the required pore size after only one pore expansion. It is simple to operate, low in cost, can be prepared in large quantities, and the method is highly transplantable. It can be applied to silica microspheres with a particle size of 3 to 10 μm, and is particularly suitable for related applications in the field of chromatography. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope image of small pore size mesoporous silica gel (5μm) raw material.
[0020] Figure 2 This is a scanning electron microscope image of the pore size of spherical silica gel after expansion by single salt (NaCl) (120nm).
[0021] Figure 3 This is a scanning electron microscope image of the pore size of spherical silica gel after expansion by single salt (NaCl) (50nm).
[0022] Figure 4 This is a scanning electron microscope image of the pore size of spherical silica gel after expansion by single salt (NaCl) (200nm).
[0023] Figure 5 This is a scanning electron microscope image of the pore size of spherical silica gel after expansion by a single salt (LiCl) (120nm).
[0024] Figure 6 This is a scanning electron microscope image of the pore size of spherical silica gel after expansion by a single salt (LiCl) (200nm).
[0025] Figure 7 This is a scanning electron microscope image of the pore size of spherical silica gel (5μm) after the two-component complex salt expanded.
[0026] Figure 8 This is a scanning electron microscope image of small pore size mesoporous silica gel (3μm) raw material.
[0027] Fig. 9 This is a scanning electron microscope image of the pore size of spherical silica gel (3μm) after the two-component complex salt expanded.
[0028] Fig.10 This is a scanning electron microscope image of small pore size mesoporous silica gel (10μm) raw material.
[0029] Fig.11 This is a scanning electron microscope image of the pore size of spherical silica gel (10μm) expanded by a two-component complex salt.
[0030] Fig.12 This is a scanning electron microscope image of the pore size of spherical silica gel after expansion by three-component complex salt (120nm).
[0031] Fig.13 The chromatogram of the separation of flavanones according to Application Example 1 is shown in FIG.
[0032] Fig.14 This is a chromatogram for batch comparison and separation of flavanones using Example 1.
[0033] Fig.15 The chromatogram is the separation chromatogram of flavanones according to Application Example 2.
[0034] Fig.16 This is a chromatogram for batch comparison and separation of flavanones using Example 2.
[0035] Fig.17 This is a chromatogram for batch comparison of flavanones using Example 3. DETAILED DESCRIPTION
[0036] The present invention is described in detail below in conjunction with the accompanying drawings and examples. However, the accompanying drawings and examples are not limitations of the technical solutions of the present invention. Any technical features and implementation schemes in the following examples are one or more of a variety of optional technical features and a variety of optional implementation schemes. For the sake of simplicity of description, the present invention cannot exhaustively list all the alternative technical features and implementation schemes contained in the present invention, so those skilled in the art should know that any technical features and implementation schemes in the present embodiment do not limit the protection scope of the present invention, and the protection scope includes any alternative technical features and implementation schemes taken by all those skilled in the art without creative work. Specifically, the implementation schemes obtained by replacing any technical features in the present invention or combining any two or more technical features provided by the present invention should be within the protection scope of the present invention. Those who do not indicate specific techniques and conditions in the examples are carried out according to the techniques and conditions described in the literature in this field or according to the product instructions, and those whose reagents or instruments are not indicated by the manufacturer are all conventional products that can be purchased commercially.
[0037] Example 1: Single salt expansion of spherical silica gel pore size
[0038] In order to obtain a chromatographic filler matrix suitable for separating macromolecular samples, the pore size of silica microspheres was expanded at a specified temperature using a single salt solution of a certain concentration. The specific steps were as follows: 50 g of small-pore mesoporous silica microspheres were taken as raw materials (particle size: 5 μm, pore size: 8 nm, scanning electron microscopy image as shown in FIG. Figure 1 As shown), disperse it into 500mL of 4% NaCl solution, ultrasonicate for 15min to allow the salt solution to evenly enter the internal pores of the silica gel, and stir at room temperature for 3h. After solid-liquid separation by filtration, the salt-soaked silica gel is first placed in a common oven preheated to 150°C and dried for 1h, and then vacuum dried at 110°C for 1h. Then transfer it to a muffle furnace, raise the temperature to 200°C for 40min and maintain it for 3h, then raise the temperature to 720°C through a 2h program and maintain it for 4h, and cool it naturally to room temperature. Wash it thoroughly with distilled water, then wash it with methanol, and dry it in an oven at 80°C for use. The scanning electron microscope image of the spherical silica gel after pore expansion is as follows Figure 2 As shown, the pore size is enlarged from 8nm to 120nm, the morphology of the silica microspheres is not destroyed, and the pore size distribution of the macropores is uniform.
[0039] Example 2
[0040] Similar to Example 1, except that NaCl is used as a single salt, and the solution concentration is 2%. The ultrasonic time during the salt immersion process is 5 minutes, and the stirring time is 1 hour. The temperature of the ordinary oven is 120°C, the temperature of the vacuum drying oven is 90°C, and the constant temperature time is 1 hour. The program heating rate is 3°C / min, the heating time is 4 hours, the final temperature is 680°C, and the maintenance time is 2 hours.
[0041] Pore diameter results: The pore diameter of the silica gel after pore expansion is 50nm. The SEM image after pore expansion is as follows: Figure 3 shown.
[0042] Example 3
[0043] Similar to Example 1, except that NaCl is used as a single salt and the solution concentration is 8%. The ultrasonic time during the salt immersion process is 20 minutes and the stirring time is 5 hours. The temperature of the ordinary oven is 160°C, the temperature of the vacuum drying oven is 130°C, and the constant temperature time is 3 hours. The program heating rate is 8°C / min, the heating time is 1.8 hours, the final temperature is 790°C, and the maintenance time is 9 hours.
[0044] Pore diameter results: The pore diameter of the silica gel after pore expansion is 200nm. The SEM image after pore expansion is as follows: Figure 4 shown.
[0045] Example 4
[0046] Similar to Example 1, except that LiCl is used as a single salt and the solution concentration is 6%. The ultrasonic time during the salt immersion process is 15 minutes and the stirring time is 3 hours. The temperature of the ordinary oven is 150°C, the temperature of the vacuum drying oven is 120°C, and the constant temperature time is 2 hours. The program heating rate is 5°C / min, the heating time is 2.5 hours, the final temperature is 680°C, and the maintenance time is 6 hours.
[0047] Pore diameter results: The pore diameter of the silica gel after pore expansion is 120nm. The SEM image after pore expansion is as follows: Figure 5 shown.
[0048] Example 5
[0049] Similar to Example 1, except that LiCl is used as a single salt, and the solution concentration is 10%. The ultrasonic time during the salt immersion process is 30 minutes, and the stirring time is 10 hours. The temperature of the ordinary oven is 180°C, the temperature of the vacuum drying oven is 150°C, and the constant temperature time is 5 hours. The program heating rate is 10°C / min, the heating time is 1.5 hours, the final temperature is 790°C, and the maintenance time is 15 hours.
[0050] Pore diameter results: The pore diameter of the silica gel after pore expansion is 200nm, as shown in the SEM image. Figure 6 shown.
[0051] Example 6: Expansion of the pore size of spherical silica gel by two-component double salt NaCl / LiCl
[0052] Take 50g of the same batch of silica microspheres as in Example 1 as raw material (pore size: 8nm, scanning electron microscope image as shown in Figure 1As shown). Weigh NaCl / LiCl = 15g / 10g and dissolve it in 500mL water to prepare a double salt solution. Disperse the silica gel in the double salt solution and ultrasonicate for 15 minutes so that the salt solution can evenly enter the internal pores of the silica gel. Stir at room temperature for 3 hours. After solid-liquid separation by filtration, first place the salt-soaked silica gel in a common oven preheated to 150°C and dry it for 1 hour, and then vacuum dry it at 110°C for 1 hour. Then transfer it to a muffle furnace, raise the temperature to 200°C for 40 minutes and maintain it for 3 hours, then raise the temperature to 600°C through a 1.2-hour program and maintain it for 8 hours, and cool it naturally to room temperature. Wash it thoroughly with distilled water, then wash it with methanol, and dry it in an oven at 80°C for use. The scanning electron microscope image of the spherical silica gel after pore expansion is as follows Figure 7 As shown, the pore size of the silica sphere is expanded from 8nm to 120nm, and the internal and external pores are controllably adjusted while maintaining the original shape of the spherical silica gel.
[0053] Example 7
[0054] Similar to Example 6, the difference is that the silica microspheres used have a particle size of 3 μm (pore size: 10 nm, see SEM image Figure 8 ). Weigh NaCl / LiCl = 15g / 3g and dissolve in 180mL water to prepare a double salt solution, ultrasonicate for 15min, and stir for 3h. The temperature of the ordinary oven is 150℃, the temperature of the vacuum drying oven is 120℃, and the constant temperature time is 2h. The program heating rate is 2℃ / min, the heating time is 5.5h, the final temperature is 650℃, and the maintenance time is 10h.
[0055] Pore diameter results: The pore diameter of the silica gel after pore expansion is 200nm, as shown in the SEM image. Fig. 9 shown.
[0056] Example 8
[0057] Similar to Example 6, except that the silica microspheres used had a particle size of 10 μm (pore size: 2 nm, see SEM image Fig.10 ). Weigh NaCl / LiCl = 5g / 15g and dissolve in 500mL water to prepare a double salt solution, ultrasonicate for 30min, and stir for 6h. The temperature of the ordinary oven is 150℃, the temperature of the vacuum drying oven is 120℃, and the constant temperature time is 3h. The program heating rate is 1℃ / min, the heating time is 9h, the final temperature is 550℃, and the maintenance time is 8h.
[0058] Pore diameter results: The pore diameter of the silica gel after pore expansion is 80nm, as shown in the SEM image Fig.11 shown.
[0059] Example 9: Three-component salt NaCl / LiCl / KNO3 to expand the pore size of spherical silica gel
[0060] Take 50g of the same batch of silica microspheres as in Example 1 as raw material (pore size: 8nm, scanning electron microscope image as shown in Figure 1 As shown). Weigh NaCl / LiCl / KNO3=15g / 10g / 7.5g and dissolve in 100mL water to prepare a three-component complex salt solution. Disperse silica gel in the complex salt solution and ultrasonicate for 20min to allow the salt solution to evenly enter the internal pores of the silica gel. Stir at room temperature for 5h. After filtration, first place the salt-soaked silica gel in a common oven preheated at 120℃ to dry for 1h, and then vacuum dry at 110℃ for 3h. Then transfer to a muffle furnace, raise the temperature to 180℃ at 5℃ / min and maintain for 3h, then raise the temperature to 530℃ after 1.1h and maintain for 12h, and cool naturally to room temperature.
[0061] Pore diameter results: SEM images of spherical silica gel after pore expansion Fig.12 As shown, the pore size of the silicon sphere expands from 8nm to 120nm, and the surface of the silicon sphere presents relatively dense channels.
[0062] Application Example 1
[0063] Weigh 15g of silica microspheres after pore expansion in Example 1, disperse them in 100mL of 10% hydrochloric acid solution, heat and reflux in an oil bath for 8h, wash with water until neutral, wash with methanol, and vacuum dry for 10h. In order to introduce amino groups to silica gel, the macroporous silica gel treated with hydrochloric acid is dispersed in 100mL of dry toluene solution, 7.5mL of 3-aminopropyltriethoxysilane is added, refluxed and stirred for 24h, and the product is washed with toluene, n-hexane, ethanol, and methanol in turn, and dried at 80°C for use.
[0064] 3 g of polysaccharide derivative (amylose-tris (3,5-dichlorophenylcarbamate)) was weighed and dissolved in 100 mL of tetrahydrofuran, and then 12 g of amino silica gel was added for reaction. After washing and drying, a chiral filler was obtained. The chiral filler was filled into a stainless steel column tube (250 mm × 4.6 mm id) by homogenization to obtain a chiral chromatographic column (column 1). In the normal phase mode with n-hexane / isopropanol as the mobile phase, flavanones were separated by Fig.13 It can be seen that the chiral column prepared using the macroporous silica gel obtained in Example 1 as the matrix has better separation ability and higher column efficiency.
[0065] According to the method of Example 1, another small-pore silica gel is used as a raw material for pore expansion, and the surface of the macroporous silica gel is modified in sequence according to the above steps, and a bonding reaction is carried out with a polysaccharide derivative (amylose-tris (3,5-dichlorophenylcarbamate)) to prepare a chiral filler, which is then filled into a chiral column (column 2) to separate flavanones. Fig.14As shown, the separation effect of flavanone on column 2 is almost the same as that on column 1, and the retention time, peak area and resolution presented in the two chromatograms are highly consistent. It can be seen that the macroporous silica gel expanded by the method of Example 1 as a chiral filler matrix has good batch-to-batch reproducibility.
[0066] Application Example 2
[0067] Similar to Application Example 1, the difference is that the macroporous silica gel is expanded by the two-component double salt of Example 6. The prepared chiral filler is filled into a chiral column (column 3) to perform separation test on flavanones. The separation chromatogram is shown in Fig.15 .like Fig.15 As shown, column 3 has good separation selectivity for flavanones and also has good column efficiency. Similarly, the method of Example 2 is used again to expand the pores of the silica gel raw material, and the obtained macroporous silica gel is gradually reacted until it is successfully prepared into a chiral filler, which is filled into a chiral column (column 4) for chromatographic separation experiments. Fig.16 As shown, the chromatograms of flavanones separated by columns 3 and 4 have a high degree of overlap, which proves that the macroporous silica gel expanded by the method of Example 6 as the chiral filler matrix has good batch-to-batch reproducibility.
[0068] Application Example 3
[0069] Similar to Application Example 1, the difference is that the macroporous silica gel is expanded by the three-component double salt of Example 9. The prepared chiral filler is filled into chiral columns (column 5 and column 6) to perform separation tests on flavanones. The separation chromatogram is shown in Fig.17 .like Fig.17 As shown, columns 5 and 6 not only have good separation selectivity for flavanones, but also have good reproducibility and stability by using the macroporous silica gel expanded by the method of Example 9 as the chiral filler chromatographic matrix.
[0070] The invention provides a method for expanding the pore size of fully porous spherical silica gel. The macroporous silica gel prepared by the method has not only controllable and adjustable pore size and narrow pore size distribution, but also can obtain the required pore size after only one pore expansion. The method is simple to operate, low in cost, can be prepared in large quantities, and has strong transplantability. The method can be applicable to silica microspheres with a particle size of 3 to 10 μm, is particularly suitable for related applications in the field of chromatography, is used as a chromatographic filler or a filler matrix, and has good separation performance and batch-to-batch reproducibility.
[0071] The description of the above disclosed embodiments is intended to enable those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art. The general principles defined by the present invention may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for expanding the pore size of fully porous spherical silica gel, characterized in that Specifically, the method includes taking small-pore mesoporous silica gel as raw material, dispersing spherical silica gel in a single salt solution or a double salt solution so that the salt solution can fully enter the internal pores of the silica gel, drying the silica gel at a constant temperature for a period of time in an ordinary oven and a vacuum drying oven, and calcining the silica gel by heating the temperature to a specified high temperature through a program. The salt in the silica gel pores reaches a molten state and corrodes its structure to form a new stacking method. After cooling, looser and larger pores are formed to obtain macroporous spherical silica gel.
2. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 1, characterized in that The small-pore mesoporous silica gel is used as the raw material, and the pore size of the raw silica gel is 2-10 nm.
3. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 1, characterized in that Spherical silica gel is dispersed in a single salt solution, and salt is soaked by ultrasound and stirring. The single salt includes an alkali metal halide salt, and the metal halide salt can be selected from NaCl or LiCl. The concentration of the single salt solution is 2% to 10%. The ultrasonic time of the salt soaking process is 5 to 30 minutes, and the stirring time is 1 to 10 hours.
4. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 1, characterized in that The spherical silica gel is dispersed in a complex salt solution and salt is soaked by ultrasound and stirring. The complex salt is a mixture of two single salts, and two-component complex salts such as NaCl / LiCl and NaCl / NaNO3 can be used. The concentration of the complex salt solution is 4% to 15%, and the complex salt ratio is 10:5 to 1:
3.
5. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 1, characterized in that Spherical silica gel is dispersed in a complex salt solution, and salt is soaked by ultrasound and stirring. The complex salt is a mixture of three single salts, and three-component complex salts NaCl / LiCl / KNO3 and NaCl / LiCl / NaNO3 can be used. The concentration of the complex salt solution is 20% to 40%, and the ratio of the complex salt is 10-20:5-10:5-10.
6. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 1, characterized in that The temperatures of drying the silica gel in a conventional oven and a vacuum drying oven at a constant temperature for a period of time are 120-180° C. and 90-150° C., respectively, and the constant temperature time is 1-5 hours; The silica gel is calcined by heating the temperature to a specified high temperature through a program, the rate of the program heating can be 1-10°C / min, the heating time can be 1.5-9h, and the pore size of the silica gel after the pore expansion can be 50-200nm.
7. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 3, characterized in that The temperature for calcining silica gel is 680-790° C., the calcination time at high temperature is 2-15 hours, and the pore size of the silica gel after pore expansion is 50-200 nm.
8. A method for expanding the pore size of a fully porous spherical silica gel as claimed in claim 4, characterized in that The calcining temperature of silica gel is 500-650° C., the calcining time at high temperature is 2-10 hours, and the pore size of the silica gel after pore expansion is 50-200 nm.
9. A method for expanding the pore size of fully porous spherical silica gel as claimed in claim 5, characterized in that The temperature for calcining silica gel is 450-600° C., the calcination time at high temperature is 2-8 hours, and the pore size of the silica gel after pore expansion is 50-200 nm.
10. The macroporous silica gel obtained by the method according to any one of claims 1 to 9 can be used in the field of chromatographic separation.
Citation Information
Patent Citations
Mesoporous silicon, preparation method of same, and method of photolyzing water to produce hydrogen
CN105905909A
Silica spheres and affinity carrier
US20140235435A1